Measurement method of interlocking relationship of fine particle products

CN118837172BActive Publication Date: 2024-11-29CHANGCHUN GOLD RES INST

Patent Information

Application Number
CN202411327581.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-29
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

The prior art is prone to sample aggregation when measuring the intercalation relationship of fine-grained products, resulting in inaccurate measurement data, especially in fine-grained samples, which is unable to accurately reflect the monomer dissociation degree of the target mineral.

Method used

Automatic mineralogical analysis samples were prepared by rolling, adding calcium carbonate and quartz, ultrasonic oscillation of anhydrous ethanol, mixing with epoxy resin, ultrasonic oscillation and dispersion of epoxy resin, and automatic mineralogical analysis was carried out to prepare and perform automatic mineralogical analysis. Measure the embedding relationship.

Benefits of technology

This method can accurately measure the embedding relationship of fine-grained products, reduce errors, provide reliable data support, and provide accurate data support for efficient utilization of ore resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118837172B_ABST
    Figure CN118837172B_ABST
Patent Text Reader

Abstract

The present invention provides a method for measuring the interlocking relationship of fine-particle products, and belongs to the technical field of process mineralogy. The method includes the steps of sample rolling, adding calcium carbonate and quartz, ultrasonic oscillation of anhydrous ethanol, ultrasonic oscillation dispersion after mixing with epoxy resin, preparing automatic mineralogical analysis samples, and performing automatic mineralogical analysis. The method is combined with automatic mineralogical analysis to save workload; the introduction of high-purity quartz and calcium carbonate for calibration makes the data more reasonable and accurate, and reduces errors. The existing measurement method directly measures, and there is a problem of low measured monomer data due to the mutual adhesion and agglomeration between fine particles. The present invention disperses the adhered particles by adding quartz and calcite (calcium carbonate), and calibrates the deviation data at the same time, so as to obtain true and accurate interlocking relationship data. The data is accurate and easy to operate, providing reliable data support for the efficient use of this ore resource.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of process mineralogy, and in particular to a method for measuring the interlocking relationship of micro-fine particle products. Background Art

[0002] Flotation technology is the main technology in the field of mineral processing, and with the continuous mining of some ore resources, their characteristics of being poor, fine and impure are becoming more and more obvious. Therefore, in order to achieve better flotation effect, improve the quality of concentrate and reduce impurities, it is necessary to make the target mineral better dissociated, that is, to make it as monomeric as possible after grinding (there are no other minerals around the target mineral). Therefore, the monomer dissociation degree (interlocking relationship) of the target mineral is an important parameter.

[0003] At present, the study of the interlocking relationship of target minerals has gradually abandoned the traditional method of manual microscopic identification, and more mineral automatic analysis systems are used to detect various products in the beneficiation process. Generally, for sample preparation for automatic mineralogical analysis, the research method of mixing the sample with epoxy resin and curing agent, removing bubbles and then curing and detecting is often used. However, this method has certain disadvantages for fine-grained samples: the phenomenon of sample agglomeration is prone to occur, that is, other minerals adhere to the periphery of the target mineral, and the data of its interlocking relationship has a large error after measurement, especially in fine-grained samples. This phenomenon is more common, making the measurement data of the monomer dissociation degree inaccurate, and the data of the target mineral in a monomer state is low, which cannot reflect the real situation.

[0004] In the prior art, the purpose of dispersing the sample is achieved by doping graphite during sample preparation; however, due to the special flake morphology of graphite, it has obviously different morphological characteristics from a large number of granular sample particles, and the dispersion effect on other particles is not good; and this part of graphite needs to be deleted as background during measurement, which is not applicable to samples containing graphite themselves; in addition, because graphite has a light specific gravity, it is difficult to mix evenly during sample preparation, and the dispersion effect is average.

[0005] In view of this, it is necessary to design an improved method for measuring the interlocking relationship of fine-particle products to solve the above problems. Summary of the invention

[0006] In view of the defects of the above-mentioned prior art, the present invention provides a method for measuring the interlocking relationship of fine-particle products. The method introduces high-purity quartz and calcium carbonate for calibration, has accurate measurement data, is applicable to a wide range of samples, and can accurately measure the interlocking relationship data of the target mineral in a sample, thereby providing reliable data support for the efficient utilization of this ore resource.

[0007] To achieve the above object, the present invention provides a method for measuring the interlocking relationship of fine particle products, comprising the following steps:

[0008] S1, select two samples to be tested, 1.0-2.0g each, and crush them until there are no obvious agglomerated pseudo-particles, and record them as samples a1 and a2 respectively;

[0009] S2, adding b1 g of calcium carbonate to the sample a1 of step S1, and mixing them thoroughly to obtain sample c1; adding b2 g of quartz to the sample a2 of step S1, and mixing them thoroughly to obtain sample c2;

[0010] S3, placing samples c1 and c2 in anhydrous ethanol respectively, dispersing them by ultrasonic vibration for 10-20 minutes, heating and drying, volatilizing the anhydrous ethanol and then rolling and dispersing them to obtain dispersed samples d1 and d2;

[0011] S4, mixing the samples d1 and d2 of step S3 with epoxy resin respectively, stirring and ultrasonically vibrating for 10-20 minutes, adding a curing agent, stirring and ultrasonically vibrating for 10-20 minutes, and then cooling at a temperature of 25-50° C. until solidified, to obtain samples e1 and e2;

[0012] S5, side-cutting the samples e1 and e2 obtained in step S4, respectively, performing secondary mounting, rough grinding, polishing and carbon spraying, respectively, to prepare samples for automatic mineralogical analysis, which are recorded as samples f1 and f2;

[0013] S6, perform automatic mineralogical analysis on samples f1 and f2 respectively to obtain data g1n and g2n;

[0014] Wherein, n=1-8, representing the state of monomer, state of intergrowth with other metal sulfides, state of intergrowth with quartz, state of intergrowth with calcium carbonate, state of intergrowth with other gangue and metal oxides, state of being encapsulated by quartz, state of being encapsulated by calcium carbonate, state of being encapsulated by other gangue or metal oxides, respectively;

[0015] S7, calculate the intercalation relationship of the target mineral, recorded as hn; where n = 1-8, representing the state of monomer, state of intergrowth with other metal sulfides, state of intergrowth with quartz, state of intergrowth with calcium carbonate, state of intergrowth with other gangue and metal oxides, state of being enclosed by quartz, state of being enclosed by calcium carbonate, state of being enclosed by other gangue or metal oxides; then

[0016] h1= 1-∑hn, n=2-8;

[0017] h2=(g12* b1+ g22* b2) / (b1+ b2);

[0018] h3= g13;

[0019] h4= g24;

[0020] h5=(g15* b1+ g25* b2) / (b1+ b2);

[0021] h6= g16;

[0022] h7= g27;

[0023] h8=(g18* b1+ g28* b2) / (b1+ b2);

[0024] g12 is the data of the state of co-existence with other metal sulfides obtained by automatic mineralogical analysis of sample f1;

[0025] g22 is the data of the state of co-existence with other metal sulfides obtained by automatic mineralogical analysis of sample f2;

[0026] g13 is the data on the state of intergrowth with quartz obtained by automatic mineralogical analysis of sample f1;

[0027] g24 is the data on the state of coexistence with calcium carbonate obtained by automatic mineralogical analysis of sample f2;

[0028] g15 is the data of the state of intergrowth with other gangue and metal oxides obtained by automatic mineralogical analysis of sample f1;

[0029] g25 is the data of the state of intergrowth with other gangue and metal oxides obtained by automatic mineralogical analysis of sample f2;

[0030] g16 is the data of the quartz inclusion state obtained by automatic mineralogical analysis of sample f1;

[0031] g27 is the data of the calcium carbonate encapsulation state obtained by automatic mineralogical analysis of sample f2;

[0032] g18 is the data of the state of being encapsulated by other gangue or metal oxides obtained by automatic mineralogical analysis of sample f1;

[0033] g28 is the data of the state of being enclosed by other gangue or metal oxides obtained by automatic mineralogical analysis of sample f2.

[0034] In step S2, the value range of b1 is 1.0-5.0.

[0035] In step S2, the value range of b2 is 1.0-5.0.

[0036] In step S3, when samples c1 and c2 are placed in anhydrous ethanol respectively, the mass ratio of anhydrous ethanol to sample is (4-15):1.

[0037] In step S4, when samples d1 and d2 are mixed with epoxy resin, the mass ratio of epoxy resin to sample is (2-5):1.

[0038] In step S6, when automatic mineralogical analysis is performed on samples f1 and f2 respectively, the analysis conditions and parameters of the two samples are set to be the same.

[0039] In step S2, the quartz content in the quartz is 99.90% or more, and the particle size of the quartz is less than 20 μm.

[0040] In step S2, the calcium carbonate content in the calcium carbonate is 99.90% or more; and the particle size of the calcium carbonate is less than 20 μm.

[0041] In step S1, the homogeneity of the two samples to be tested is the same.

[0042] The beneficial effects of the present invention are:

[0043] The method for measuring the interlocking relationship of fine-particle products provided by the present invention comprises the steps of sample rolling, adding calcium carbonate and quartz, ultrasonic oscillation of anhydrous ethanol, ultrasonic oscillation dispersion after mixing with epoxy resin, preparing automatic mineralogical analysis samples, and performing automatic mineralogical analysis. The sample preparation process of this method is simple, does not require special processes and steps, and does not require special parameter adjustment during the measurement process; then the sample is automatically analyzed for mineralogical analysis, which saves workload; high-purity quartz and calcium carbonate are introduced for calibration, and the data is more reasonable and accurate, reducing errors. In addition, the added quartz and calcium carbonate are conventional substances, which are easy to obtain, easy to identify during the measurement process, and have low errors.

[0044] The existing measurement method directly measures, and due to the adhesion and agglomeration between fine particles, there is a problem that the measured monomer data is low. The present invention disperses the adhered particles by adding quartz and calcite (calcium carbonate). At the same time, the test data of the two samples are mutually verified and the deviation data is calibrated to obtain true and accurate embedding relationship data. The data is accurate and easy to operate, providing reliable data support for the efficient use of this ore resource. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 A schematic diagram of the process flow of the method for measuring the interlocking relationship of fine particle products provided by the present invention. DETAILED DESCRIPTION

[0046] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0047] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0048] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0049] See also Figure 1 As shown, the present invention provides a method for measuring the interlocking relationship of fine particle products, comprising the following steps:

[0050] S1, select two samples to be tested, each weighing 1.0-2.0 g, and crush them until there are no obvious agglomerated pseudo-particles, and record them as samples a1 and a2 respectively; wherein, the homogeneity of the two samples to be tested is the same.

[0051] S2, adding calcium carbonate b1 g to the sample a1 of step S1, and mixing thoroughly to obtain sample c1;

[0052] Add quartz b2 g to the sample a2 in step S1 and mix thoroughly to obtain sample c2;

[0053] The calcium carbonate is preferably high-purity calcium carbonate; the calcium carbonate content in the calcium carbonate is 99.90% or more; the particle size of the calcium carbonate is less than 20 μm. The value range of b1 is 1.0-5.0.

[0054] The quartz is preferably high-purity quartz, the quartz content in the quartz is 99.90% or more, and the quartz particle size is less than 20 μm. The value range of b2 is 1.0-5.0.

[0055] S3, placing samples c1 and c2 in anhydrous ethanol respectively, dispersing them by ultrasonic vibration for 10-20 minutes, heating and drying, volatilizing the anhydrous ethanol and then rolling and dispersing them to obtain dispersed samples d1 and d2;

[0056] Among them, when samples c1 and c2 are placed in anhydrous ethanol respectively, the mass ratio of anhydrous ethanol to sample is (4-15):1.

[0057] S4, respectively mix the samples d1 and d2 of step S3 with epoxy resin, stir and disperse by ultrasonic vibration for 10-20 minutes, then add curing agent, stir and ultrasonic vibration for 10-20 minutes, and then place under cooling temperature of 25-50°C until solidified to obtain samples e1 and e2.

[0058] The curing agent is used to mix with the epoxy resin in proportion to gradually solidify the epoxy resin.

[0059] Among them, when samples d1 and d2 are mixed with epoxy resin, the mass ratio of epoxy resin to sample is (2-5):1.

[0060] S5, side-cutting the samples e1 and e2 obtained in step S4, respectively, performing secondary mounting, rough grinding, polishing and carbon spraying, respectively, to prepare samples for automatic mineralogical analysis, which are recorded as samples f1 and f2;

[0061] S6, perform automatic mineralogical analysis on samples f1 and f2 respectively to obtain data g1n and g2n;

[0062] Wherein, n=1-8, representing the state of monomer, state of intergrowth with other metal sulfides, state of intergrowth with quartz, state of intergrowth with calcium carbonate, state of intergrowth with other gangue and metal oxides, state of being encapsulated by quartz, state of being encapsulated by calcium carbonate, state of being encapsulated by other gangue or metal oxides, respectively;

[0063] When the automatic mineralogical analysis is performed on samples f1 and f2, the analysis conditions and parameter settings of the two are the same, such as the same magnification, measurement height, saturation voltage, brightness and contrast.

[0064] S7, calculate the intercalation relationship of the target mineral, recorded as hn; where n = 1-8, representing the state of monomer, state of intergrowth with other metal sulfides, state of intergrowth with quartz, state of intergrowth with calcium carbonate, state of intergrowth with other gangue and metal oxides, state of being enclosed by quartz, state of being enclosed by calcium carbonate, state of being enclosed by other gangue or metal oxides; then

[0065] h1= 1-∑hn(n=2-8);

[0066] h2=(g12* b1+ g22* b2) / (b1+ b2);

[0067] h3= g13;

[0068] h4= g24;

[0069] h5=(g15* b1+ g25* b2) / (b1+ b2);

[0070] h6= g16;

[0071] h7= g27;

[0072] h8=(g18* b1+ g28* b2) / (b1+ b2);

[0073] g12 is the data of the state of co-existence with other metal sulfides obtained by automatic mineralogical analysis of sample f1;

[0074] g22 is the data of the state of co-existence with other metal sulfides obtained by automatic mineralogical analysis of sample f2;

[0075] g13 is the data on the state of intergrowth with quartz obtained by automatic mineralogical analysis of sample f1;

[0076] g24 is the data on the state of coexistence with calcium carbonate obtained by automatic mineralogical analysis of sample f2;

[0077] g15 is the data of the state of intergrowth with other gangue and metal oxides obtained by automatic mineralogical analysis of sample f1;

[0078] g25 is the data of the state of coexistence with other gangue and metal oxides obtained by automatic mineralogical analysis of sample f2;

[0079] g16 is the data of the quartz inclusion state obtained by automatic mineralogical analysis of sample f1;

[0080] g27 is the data of the calcium carbonate encapsulation state obtained by automatic mineralogical analysis of sample f2;

[0081] g18 is the data of the state of being encapsulated by other gangue or metal oxides obtained by automatic mineralogical analysis of sample f1;

[0082] g28 is the data of the state of being enclosed by other gangue or metal oxides obtained by automatic mineralogical analysis of sample f2.

[0083] This measurement method introduces high-purity quartz and calcium carbonate for calibration, and has accurate measurement data, is applicable to a wide range of samples, and can accurately measure the embedded relationship data of the target minerals in a sample, providing reliable data support for the efficient use of this ore resource.

[0084] The method for measuring the interlocking relationship of fine particle products provided by the present invention is described below in conjunction with specific embodiments.

[0085] Example 1

[0086] This embodiment provides a method for measuring the interlocking relationship of a fine-grained product, which measures the interlocking relationship of pyrite in a sample, and specifically includes the following steps:

[0087] S1, select two samples to be tested, each weighing 2.0 g, and record them as samples a1 and a2 after rolling;

[0088] S2, adding 2.0 g of calcium carbonate to sample a1, and mixing thoroughly to obtain sample c1; wherein the content of calcium carbonate in the calcium carbonate is 99.95%; and the particle size of the calcium carbonate is 5 μm;

[0089] 2.0 g of quartz was added to sample a2 and mixed thoroughly to obtain sample c2; wherein the content of quartz in the quartz was 99.95%; and the particle size of the quartz was 5 μm;

[0090] S3, take 4.0g of samples c1 and 4.0g of samples c2 respectively, put them in 20ml of anhydrous ethanol, disperse them by ultrasonic vibration for 20 minutes, heat and dry them, and roll and disperse them after volatilization to obtain samples d1 and d2; at this time, the mass ratio of anhydrous ethanol to sample is 4.45:1.

[0091] S4, mix samples d1 and d2 with 10 ml of epoxy resin, stir and ultrasonically oscillate for 20 minutes, then add 5 ml of curing agent, stir and ultrasonically oscillate for 20 minutes, and then place under cooling temperature of 25-50°C until solidified to obtain samples e1 and e2; the mass ratio of epoxy resin to sample is 2.5:1.

[0092] S5, cutting the side of samples e1 and e2, re-mounting, rough grinding, polishing and carbon spraying, respectively, to prepare samples for automatic mineralogical analysis, and obtaining samples f1 and f2;

[0093] Secondary mounting means cutting the sample vertically, placing the cut sample sideways downward, and fixing the sample in the sample preparation mold with glue again.

[0094] S6, perform automatic mineralogical analysis on samples f1 and f2, and obtain data g1n and g2n, see Table 1 for details.

[0095] During the automatic mineralogy analysis, the measurement parameters of the test samples f1 and f2 were set to be the same, with the magnification being 800 times, the measurement height being 1.4 mm, the saturation voltage being 25.0 kV, and the brightness and contrast being 78.0 and 28.0 respectively.

[0096] S7, calculate the embedding relationship of the target mineral, denoted as hn, then

[0097] h1=1-(5.34%+6.15%+1.86%+1.46%+3.56%+2.17%+2.34%)=1-21.71%=78.29%

[0098] h2=(g12* b1+ g22* b2) / (b1+ b2)=(5.23%+5.44%)*2 / 4=5.34%;

[0099] h3= g13=6.15%;

[0100] h4= g24=1.86%;

[0101] h5=(g15* b1+ g25* b2) / (b1+ b2)=(1.59%+1.33%)*2 / 4=1.46%;

[0102] h6= g16=3.56%;

[0103] h7= g27=2.17%;

[0104] h8=(g18* b1+ g28* b2) / (b1+ b2)=(1.14%+1.20%)*2 / 4=1.17%;

[0105] Table 1 Pyrite intercalation relationship measurement results

[0106] In the table, h2-h8 refers to the sum of h2, h3, h4, h5, h6, h7, and h8.

[0107] Direct measurement means: quartz and calcium carbonate are not added during sample preparation, 4.0 g of unknown sample is directly sampled, the sample preparation process and test conditions are the same as those in Example 1, and then automatic mineralogical analysis is performed using MLA automatic mineralogical analysis equipment, and the data obtained is used as the final test result.

[0108] The direct measurement process in the subsequent embodiments is the same as that in this embodiment, except that the sample size is adjusted accordingly, and the details will not be repeated here.

[0109] It can be seen from the experiment that the direct measurement data has a large deviation and cannot match the mineral processing experimental phenomenon well. According to the subsequent mineral processing effect, it can be seen that the data obtained by the measurement method of the present invention is closer to the mineral processing result, that is, the measurement result of the present invention is more accurate. For example, in the normal flotation process, the pyrite that can be recovered is the monomer + pyrite in the state of co-existence with sulfides. The result of direct measurement is that the recoverable pyrite (monomer state + co-existence with sulfides) is 57.63%, and the recoverable pyrite measured by this method is 83.63%. This data is more in line with the actual pyrite recovery situation.

[0110] Example 2

[0111] This embodiment provides a method for measuring the interlocking relationship of a fine particle product, and measuring the interlocking relationship of arsenopyrite in a sample, specifically comprising the following steps:

[0112] S1, select two samples to be tested, each weighing 1.50 g, and crush them into samples a1 and a2;

[0113] S2, adding 0.50 g of calcium carbonate to sample a1, and mixing thoroughly to obtain sample c1; wherein the content of calcium carbonate in the calcium carbonate is 99.95%; and the particle size of the calcium carbonate is 5 μm;

[0114] 0.50 g of quartz was added to sample a2 and mixed thoroughly to obtain sample c2; wherein the content of quartz in the quartz was 99.95%; and the particle size of the quartz was 5 μm;

[0115] S3, take 2.0g of samples c1 and 2.0g of samples c2 respectively, put them in 20ml of anhydrous ethanol, disperse them by ultrasonic vibration for 20 minutes, heat and dry them, and roll and disperse them after volatilization to obtain samples d1 and d2; wherein the mass ratio of anhydrous ethanol to sample is 8.9:1.

[0116] S4, mix samples d1 and d2 with 10 ml of epoxy resin, stir and ultrasonically oscillate for 20 minutes, then add 5 ml of curing agent, stir and ultrasonically oscillate for 20 minutes, and then place under cooling temperature of 25-50°C until solidified to obtain samples e1 and e2; the mass ratio of epoxy resin to sample is 5:1.

[0117] S5, cutting the side of samples e1 and e2, re-mounting, rough grinding, polishing and carbon spraying, respectively, to prepare samples for automatic mineralogical analysis, and obtaining samples f1 and f2;

[0118] S6, automatic mineralogical analysis was performed on samples f1 and f2, and the same measurement parameters were set, with a magnification of 750 times, a measurement height of 1.4 mm, a saturation voltage of 25.0 kV, and brightness and contrast of 78.0 and 28.0 respectively, to obtain data g1n and g2n;

[0119] S7, calculate the intercalation relationship of the target mineral, denoted as hn, see Table 2 for details.

[0120] Table 2 Measurement results of arsenopyrite embedding relationship%

[0121]

[0122] In the table, h2-h8 refers to the sum of h2, h3, h4, h5, h6, h7, and h8.

[0123] Example 3

[0124] This embodiment provides a method for measuring the interlocking relationship of a fine-grained product, which measures the interlocking relationship of sphalerite in a sample; the method specifically comprises the following steps:

[0125] S1, select two samples to be tested, 2.0g each, and crush them into samples a1 and a2;

[0126] S2, adding 2.0 g of calcium carbonate to sample a1, and mixing thoroughly to obtain sample c1; wherein the content of calcium carbonate in the calcium carbonate is 99.90%; and the particle size of the calcium carbonate is 10 μm;

[0127] 2.0 g of quartz was added to sample a2 and mixed thoroughly to obtain sample c2; wherein the content of quartz in the quartz was 99.90%; and the particle size of the quartz was 10 μm;

[0128] S3, place samples c1 and c2 in 16 ml of anhydrous ethanol respectively, disperse them by ultrasonic vibration for 20 minutes, heat and dry them, and roll and disperse them after volatilization to obtain samples d1 and d2; wherein the mass ratio of anhydrous ethanol to sample is 6.32:1.

[0129] S4, mix samples d1 and d2 with 10.0 ml of epoxy resin, stir and disperse by ultrasonic vibration for 20 minutes, then add 5.0 ml of curing agent, stir and ultrasonic vibration for 20 minutes, and then cool to 25-50°C until solidified to obtain samples e1 and e2; wherein the mass ratio of epoxy resin to sample is 2.50:1.

[0130] S5, cutting the side of samples e1 and e2, re-mounting, rough grinding, polishing and carbon spraying, respectively, to prepare samples for automatic mineralogical analysis, and obtaining samples f1 and f2;

[0131] S6, perform automatic mineralogical analysis on samples f1 and f2 to obtain data g1n and g2n;

[0132] S7, calculate the intercalation relationship of the target mineral, recorded as hn, and the specific data are shown in Table 3.

[0133] Table 3 Sphalerite intercalation relationship measurement results %

[0134]

[0135] In the table, h2-h8 refers to the sum of h2, h3, h4, h5, h6, h7, and h8.

[0136] Compared with direct measurement, the measuring method of the present invention adds calcium carbonate and quartz, ultrasonic vibration of anhydrous ethanol, and ultrasonic vibration dispersion of epoxy resin to prepare automatic mineralogical analysis samples. The sample preparation process is simple, and then the sample is automatically analyzed for mineralogical analysis, which saves workload. The present invention disperses the adhering particles by introducing high-purity quartz and calcium carbonate, and calibrates the deviation data at the same time, and the data is accurate. The present invention is practical, the data is accurate, and the embedded relationship of the target mineral in a sample can be accurately measured. The data is accurate and easy to operate, providing reliable data support for the efficient use of this ore resource.

[0137] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for measuring the interlocking relationship of fine-grained products. It is characterized in that The steps include: S1, select two samples to be tested, 1.0-2.0g each, and crush them until there are no obvious agglomerated pseudo particles, and record them as samples a1 and a2 respectively; S2, adding b1 g of calcium carbonate to the sample a1 of step S1, and mixing them thoroughly to obtain a sample c1; adding b2 g of quartz to the sample a2 of step S1, and mixing them thoroughly to obtain a sample c2; S3, placing samples c1 and c2 in anhydrous ethanol respectively, dispersing them by ultrasonic vibration for 10-20 minutes, heating and drying, volatilizing the anhydrous ethanol and then rolling and dispersing them to obtain dispersed samples d1 and d2; S4, mixing the samples d1 and d2 of step S3 with epoxy resin respectively, stirring and ultrasonically vibrating for 10-20 minutes, adding a curing agent, stirring and ultrasonically vibrating for 10-20 minutes, and then cooling at a temperature of 25-50° C. until solidified, to obtain samples e1 and e2; S5, cutting the samples e1 and e2 obtained in step S4, respectively, re-mounting, rough grinding, polishing and carbon spraying, respectively, to prepare samples for automatic mineralogical analysis, which are recorded as samples f1 and f2; S6, perform automatic mineralogical analysis on samples f1 and f2 respectively to obtain data g1n and g2n; Wherein, n=1-8, representing the state of monomer, state of intergrowth with other metal sulfides, state of intergrowth with quartz, state of intergrowth with calcium carbonate, state of intergrowth with other gangue and metal oxides, state of being encapsulated by quartz, state of being encapsulated by calcium carbonate, state of being encapsulated by other gangue or metal oxides, respectively; S7, calculate the intercalation relationship of the target mineral, recorded as hn; where n = 1-8, representing the state of monomer, state of intergrowth with other metal sulfides, state of intergrowth with quartz, state of intergrowth with calcium carbonate, state of intergrowth with other gangue and metal oxides, state of being enclosed by quartz, state of being enclosed by calcium carbonate, state of being enclosed by other gangue or metal oxides; then h1= 1-∑hn, n=2-8; h2=(g12* b1+ g22* b2) / (b1+ b2); h3= g13; h4= g24; h5=(g15* b1+ g25* b2) / (b1+ b2); h6= g16; h7= g27; h8=(g18* b1+ g28* b2) / (b1+ b2); g12 is the data of the state of co-existence with other metal sulfides obtained by automatic mineralogical analysis of sample f1; g22 is the data of the state of co-existence with other metal sulfides obtained by automatic mineralogical analysis of sample f2; g13 is the data on the state of intergrowth with quartz obtained by automatic mineralogical analysis of sample f1; g24 is the data on the state of coexistence with calcium carbonate obtained by automatic mineralogical analysis of sample f2; g15 is the data of the state of intergrowth with other gangue and metal oxides obtained by automatic mineralogical analysis of sample f1; g25 is the data of the state of coexistence with other gangue and metal oxides obtained by automatic mineralogical analysis of sample f2; g16 is the data of the quartz inclusion state obtained by automatic mineralogical analysis of sample f1; g27 is the data of the calcium carbonate encapsulation state obtained by automatic mineralogical analysis of sample f2; g18 is the data of the state of being encapsulated by other gangue or metal oxides obtained by automatic mineralogical analysis of sample f1; g28 is the data of the state of being enclosed by other gangue or metal oxides obtained by automatic mineralogical analysis of sample f2.

2. The method for measuring the interlocking relationship of fine particle products according to claim 1, Features: In step S2, the value range of b1 is 1.0-5.

0.

3. The method for measuring the interlocking relationship of fine particle products according to claim 1, Features: In step S2, the value range of b2 is 1.0-5.

0.

4. The method for measuring the interlocking relationship of micro-particle products according to claim 1, Features: In step S3, when samples c1 and c2 are placed in anhydrous ethanol respectively, the mass ratio of anhydrous ethanol to sample is (4-15):

1.

5. The method for measuring the interlocking relationship of micro-particle products according to claim 1, Features: In step S4, when samples d1 and d2 are mixed with epoxy resin, the mass ratio of epoxy resin to sample is (2-5):

1.

6. The method for measuring the interlocking relationship of fine particle products according to claim 1, Features: In step S6, when automatic mineralogical analysis is performed on samples f1 and f2 respectively, the analysis conditions and parameters of the two samples are set to be the same.

7. The method for measuring the interlocking relationship of micro-particle products according to claim 1, Features: In step S2, the quartz content in the quartz is 99.90% or more, and the particle size of the quartz is less than 20 μm.

8. The method for measuring the interlocking relationship of micro-particle products according to claim 1, Features: In step S2, the calcium carbonate content in the calcium carbonate is 99.90% or more; and the particle size of the calcium carbonate is less than 20 μm.

9. The method for measuring the interlocking relationship of micro-particle products according to claim 1, Features: In step S1, the homogeneity of the two samples to be tested is the same.

Citation Information

Patent Citations

  • Method forpreparing iron concentrate for making iron from phosphorus-containing oolitic hematite

    CN101054625A

  • Floatation process of complex lead zinc ores

    CN101602030A

Cited By

  • Method for determining embedding state of target element

    CN122385862A

  • Method for determining the state of inclusion of target elements

    CN122385862B