Cold spraying pot and manufacturing method thereof

Through the cold spray process and multi-step processing, the problems of low deposition efficiency and poor non-stick performance of the magnetically conductive layer of traditional pots under high temperature conditions are solved, and efficient electromagnetic heating and thermal conductivity are improved.

CN118844787APending Publication Date: 2024-10-29NINGBO GRAMMY KITCHENWARE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410912960.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The magnetic conductive layer of traditional electromagnetic heating pots has problems such as high deposition temperature, low deposition efficiency, high porosity and poor non-stick performance under high temperature conditions. It is difficult to achieve both efficient deposition and high-performance coating production.

Method used

Using the cold spray process, amorphous metal alloy and liquid metal composite powder are sprayed with magnetic field assistance, combined with screen printing, pickling, alkali washing and fluorosilicone modification, and finally vacuum cold spraying non-stick coating, annealing treatment to improve Magnetic, thermal and non-stick properties.

Benefits of technology

A thick, high-density, high-strength and high-toughness magnetic and thermal conductive coating is achieved to meet the requirements for efficient electromagnetic heating and non-stick performance of electromagnetic heating pots under long-term high temperature conditions.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a manufacturing method of a cold spraying pot. The manufacturing method comprises the following steps: S1, providing a pretreated aluminum-based pot body; s2, composite powder comprising at least part of amorphous metal alloy is sprayed on the inner surface of the aluminum-based pot body in a magnetic field auxiliary cold spraying mode, and a magnetic conduction and heat conduction bottom layer is obtained; s3, a layer of ink pattern is printed on the surface of the substrate in a silk-screen mode, and then acid washing and alkali washing treatment are conducted in sequence; and S4, fluorosilicone resin modification treatment is conducted, then a non-stick coating material is sprayed in a vacuum cold spraying mode, and the cold spraying cookware is obtained after annealing treatment. According to the manufacturing method of the cold spraying cookware, the problems that efficient deposition cannot be taken into account in the manufacturing process of a magnetic conductive and heat conductive coating and a non-stick coating of an existing cookware, and the performance such as thickness, high binding force, high compactness, high strength and high toughness cannot be achieved are solved, so that the use requirements of efficient electromagnetic heating, heat conduction and non-stick performance of the cookware under the long-term high-temperature condition are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of cookware, and in particular to a cold spray cookware and a manufacturing method thereof. Background Art

[0002] Electromagnetic heating cookware is a kind of cookware that uses the principle of electromagnetic induction to generate a magnetic field at the bottom of the pan through an electromagnetic coil, converting electrical energy into thermal energy to achieve cooking; it has the advantages of fast heating, strong firepower, and more power saving. Usually, a magnetic conductive layer is coated on the bottom of the electromagnetic heating cookware, which responds to the high-frequency magnetic field of the induction cooker and transfers energy into the cookware, thereby achieving the purpose of heating the cookware.

[0003] The magnetic conductive layer of traditional electromagnetic heating cookware is obtained by thermal spraying, which has problems such as high deposition temperature, low deposition efficiency, and high porosity. The vigorous development of cold spraying technology and equipment has made cold spraying a rapid solid-state forming process, which has been applied in metal additive manufacturing and damage repair of key parts such as aerospace. Compared with traditional thermal spraying, cold spraying has low deposition temperature, high deposition efficiency, low porosity, and the powder is not prone to oxidation, decomposition, phase change, and grain growth of nanostructured materials during the deposition process, making it possible to produce high-quality coatings.

[0004] However, although the cold spray process has received more and more attention and concern, its application in the field of cookware manufacturing is still in the initial exploration stage and has not yet been widely promoted and applied. There is still a lot of room for improvement in its process technology in order to produce high-performance electromagnetic heating cookware. Summary of the invention

[0005] In view of the above shortcomings of the prior art, the present invention provides, on the one hand, a method for manufacturing cold sprayed cookware to solve the problem that the existing production process of the magnetic and thermal conductive coating and the non-stick coating of the cookware cannot take into account efficient deposition and obtain performance problems such as thickness, high bonding strength, high density, high strength and high toughness, so as to meet the use requirements of the cookware under long-term high temperature conditions such as efficient electromagnetic heating, thermal conductivity and non-stick performance.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0007] A method for manufacturing a cold spray cookware, the method comprising the following steps:

[0008] S1: providing an aluminum-based pot body after pre-treatment; the pre-treatment includes but is not limited to degreasing, sandblasting, cleaning and other treatment methods;

[0009] S2: Spraying a composite powder including at least a part of an amorphous metal alloy onto the inner surface of the aluminum-based pot body obtained in step S1 by means of magnetic field-assisted cold spraying to obtain a magnetically conductive and thermally conductive bottom layer; the thickness of the magnetically conductive and thermally conductive bottom layer is 1 to 1.5 mm;

[0010] S3: firstly screen-printing a layer of ink pattern on the magnetic and thermal conductive bottom layer obtained in step S2, and then sequentially performing acid washing and alkali washing treatments;

[0011] S4: performing fluorosilicone resin modification treatment on the magnetic and thermal conductive bottom layer treated in step S3, and then spraying a non-stick coating material by vacuum cold spraying, and obtaining the cold sprayed cookware after annealing treatment.

[0012] As a preferred technical solution, the preparation method of the metal alloy is as follows: first weigh raw materials composed of iron powder, cobalt powder, silicon powder and boron powder, wherein the iron powder, cobalt powder, silicon powder and boron powder are 50:30:15:5, then smelt the alloy by arc melting under the protection of argon gas, and then rapidly cool at a cooling rate of 110±10°C per minute, and finally obtain the metal alloy by atomization. In the present application, the disordered state of each atom in the liquid state at high temperature is rapidly "frozen" to form an amorphous solid, thereby obtaining an amorphous metal alloy composed of metal iron and cobalt and non-metal silicon and boron. The addition of the metal alloy not only makes the coating have the characteristics of high strength and excellent toughness, but also because its resistivity is higher than that of general metal crystals, it can greatly reduce eddy current loss, has magnetic properties of low loss and high magnetic permeability, effectively improves the deposition efficiency of the composite powder on the surface of the aluminum-based pot body, and obtains a thick, high-density and high-performance magnetic and thermal conductive coating.

[0013] As a preferred technical solution, the composite powder also includes liquid metal, copper, chromium, iron or iron-based alloy. Furthermore, the present application not only improves the deposition speed and deposition efficiency of the metal raw materials in the composite powder during the room temperature cold spraying process by compounding liquid metal, copper and chromium, but also obtains a stable and dense iron-based magnetic and thermal conductive coating, thereby improving the magnetic and thermal conductive properties of the cookware of the present application.

[0014] As a preferred technical solution, the magnetic induction intensity of the magnetic field-assisted cold spraying is 1.0-1.5T, and the coercive force of the permanent magnet is 500-1000kA / m; the working pressure of the cold spraying is 1.5-2.5MPa, the spraying temperature is room temperature, the powder feeding rate is 300-500g / min, and the spraying distance is 10-30mm. The present application uses a magnetic field-assisted cold spraying method, which can accelerate the movement of magnetic atoms in the composite powder to the surface of the aluminum-based pot body, thereby improving the deposition efficiency; and effectively control the dispersion of magnetic atoms, so that the composite powder is focused and deposited on the surface of the aluminum-based pot body, thereby obtaining a thick, highly dense and high-performance magnetic and thermal conductive coating.

[0015] As a preferred technical solution, the ink is composed of 42 to 47 parts of water-soluble acrylic resin, 0.5 to 1 part of monoethanolamine, 0.5 to 1 part of polyethylene wax, 1 to 2 parts of glycerol, 50 to 90 parts of pigment and 40 to 60 parts of deionized water.

[0016] After the magnetic and thermally conductive coating of the present invention is screen-printed with a pattern, an ink covering layer and an ink-free covering layer will be formed on the inner surface of the pot body. Part of the surface metal in the magnetic and thermally conductive coating without ink coverage is corroded by the pickling solution, thereby forming a magnetic and thermally conductive coating with a concave-convex network pattern structure; and then an alkaline washing solution is used to wash away the ink on the magnetic and thermally conductive coating, so that the entire inner surface of the aluminum-based pot body is not covered with ink, which facilitates the fluorosilicone resin modification treatment in step S4.

[0017] As a preferred technical solution, the acid washing treatment adopts hydrofluoric acid, hydrogen peroxide, citric acid, tannic acid and deionized water; the alkali washing treatment adopts a compound of cerium ammonium nitrate and sodium hydroxide solution.

[0018] As a preferred technical solution, the spraying temperature of the vacuum cold spraying is 320-350°C, the powder feeding rate is 300-500g / min, and the spraying distance is 20-50mm. The present invention performs vacuum cold spraying on non-stick coating materials of a certain particle size within a specific spraying temperature range, achieving efficient deposition and high density of ultrafine titanium dioxide powder and aluminum oxide powder, and because the particles undergo severe plastic deformation and dynamic crushing, the strong bonding force between the broken particles is increased, thereby ensuring the stable non-stick performance of the aluminum-based pot body of the present application under long-term high temperature conditions.

[0019] As a preferred technical solution, the non-stick coating material is composed of PTFE resin powder with a particle size of 20 to 50 μm, titanium dioxide powder with a particle size of 0.5 to 1 μm, and aluminum oxide powder with a particle size of 0.1 to 0.5 μm.

[0020] As a preferred technical solution, the annealing treatment temperature is 200-250° C. The present application further reduces the microstrain of the coating on the surface of the cookware through annealing treatment, thereby further improving the magnetic and thermal conductivity and high temperature resistance of the cold sprayed cookware of the present application.

[0021] Another aspect of the present invention is to provide a cold spray cookware, which is manufactured using the above-mentioned method for manufacturing the cold spray cookware.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The manufacturing method of the cold spray cookware of the present application is to compound an amorphous metal alloy with liquid metal, copper, chromium, iron or iron-based alloy, and spray it by magnetic field-assisted cold spraying to obtain a thick and dense magnetic and thermal conductive base layer; then, an ink pattern is screen-printed, and after acid and alkali washing, a fluorosilicone resin modification treatment is performed, and finally a non-stick coating is sprayed by vacuum cold spraying. After annealing, a thick, high-bonding, high-density, high-strength and high-toughness cold spray cookware is obtained, which can meet the use requirements of electromagnetic heating cookware under long-term high temperature conditions such as efficient electromagnetic heating, thermal conductivity and non-stick performance. DETAILED DESCRIPTION

[0024] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0025] Example 1

[0026] The method for manufacturing the cold spray cookware of this embodiment comprises the following steps:

[0027] S1: Provide an aluminum-based pot body after pre-treatments such as degreasing, sandblasting, and cleaning. The degreasing, sandblasting, and cleaning treatments of this embodiment are conventional technical means in the art and will not be described in detail here.

[0028] S2: Spray a composite powder including liquid metal (the liquid metal is a eutectic alloy of 75% gallium and 25% indium), copper, chromium, iron and a completely amorphous metal alloy on the inner surface of the aluminum-based pot body obtained in step S1 by magnetic field-assisted cold spraying to obtain a magnetic and thermally conductive bottom layer; the mass ratio of the liquid metal, copper, chromium, iron and the metal alloy is 10:30:5:40:15; the thickness of the magnetic and thermally conductive bottom layer is 1.1 mm; the magnetic induction intensity of the magnetic field-assisted cold spraying is 1.0 T, and the coercive force of the permanent magnet used is 1000 kA / m; the working gas pressure of the cold spraying is 1.5 MPa, the spraying temperature is room temperature, the powder feeding rate is 300 g / min, and the spraying distance is 20 mm.

[0029] S3: Screen print a layer of ink pattern on the magnetic and thermal conductive bottom layer obtained in step S2, and then perform acid washing and alkali washing treatment in sequence; the ink is composed of 42 parts of water-soluble acrylic resin, 0.5 parts of monoethanolamine, 0.5 parts of polyethylene wax, 1 part of glycerol, 50 parts of pigment and 40 parts of deionized water. The acid washing treatment is composed of 10 parts by weight of hydrofluoric acid, 15 parts by weight of hydrogen peroxide, 8 parts by weight of citric acid, 7 parts by weight of tannic acid and 60 parts by weight of deionized water; the alkali washing treatment is composed of a compound of ammonium cerium nitrate and sodium hydroxide solution with a mass volume ratio of 1:20.

[0030] S4: spray a layer of 5 μm fluorosilicone resin on the magnetic and thermal conductive bottom layer treated in step S3 for fluorosilicone resin modification, then spray the non-stick coating material by vacuum cold spraying, and obtain the cold sprayed cookware after annealing. The total thickness of the coating on the surface of the cookware is 1.5 mm. The spraying temperature of the vacuum cold spraying is 320°C, the powder feeding rate is 300 g / min, and the spraying distance is 20 mm. The non-stick coating material is composed of PTFE resin powder with an average particle size of 20 μm, titanium dioxide powder with an average particle size of 0.5 μm, and aluminum oxide powder with an average particle size of 0.1 μm. Specifically, PTFE resin powder, titanium dioxide powder and aluminum oxide powder with a mass ratio of 1:1:1 are added to ethanol, and ultrasonic-assisted stirring is performed; after preparation, the mass concentrations of the titanium dioxide powder and aluminum oxide powder are both 5%. The treatment temperature of the annealing treatment is 220°C.

[0031] The preparation method of the metal alloy comprises the following steps: firstly weighing raw materials consisting of iron powder, cobalt powder, silicon powder and boron powder, wherein the ratio of the iron powder, cobalt powder, silicon powder and boron powder is 50:30:15:5; then smelting the alloy by arc melting under the protection of argon gas; then rapidly cooling at a cooling rate of 100° C. per minute; and finally obtaining the metal alloy by atomization.

[0032] The cold sprayed cookware samples produced in this embodiment have no cracking after appearance inspection; the maximum electromagnetic heating power can reach 1800W, and the magnetic permeability is 90%; the average porosity of the cookware surface coating is 0.02%; the microhardness is 72.4HV 0.1 ; After 7 cycles of hot and cold shock test (heating at 280℃ for 60 minutes, then taking it out and cooling it in 25℃ tap water), the coating showed no defects such as shedding and cracking. At the same time, the non-stick performance test of fried eggs was carried out according to GB / T32095.2, and the test results showed that the evaluation level reached Level I.

[0033] Example 2

[0034] The method for manufacturing the cold spray cookware of this embodiment comprises the following steps:

[0035] S1: Provide an aluminum-based pot body after pre-treatments such as degreasing, sandblasting, and cleaning. The degreasing, sandblasting, and cleaning treatments of this embodiment are conventional technical means in the art and will not be described in detail here.

[0036] S2: Spray the composite powder including liquid metal (the liquid metal is a eutectic alloy of 75% gallium and 25% indium), copper, chromium, iron and completely amorphous metal alloy on the inner surface of the aluminum-based pot body obtained in step S1 by magnetic field-assisted cold spraying to obtain a magnetic conductive and thermal conductive bottom layer; the mass ratio of the liquid metal, copper, chromium, iron and metal alloy is 15:30:5:40:10; the thickness of the magnetic conductive and thermal conductive bottom layer is 1.3mm; the magnetic induction intensity of the magnetic field-assisted cold spraying is 1.0T, and the coercive force of the permanent magnet is 1000kA / m; the working gas pressure of the cold spraying is 2MPa, the spraying temperature is room temperature, the powder feeding rate is 400g / min, and the spraying distance is 20mm. The preparation method of the metal alloy is the same as that of Example 1.

[0037] S3: Screen print a layer of ink pattern on the magnetic and thermal conductive bottom layer obtained in step S2, and then carry out acid washing and alkali washing treatment in sequence; the ink is composed of 43 parts of water-soluble acrylic resin, 0.7 parts of monoethanolamine, 0.7 parts of polyethylene wax, 1.5 parts of glycerol, 70 parts of pigment and 50 parts of deionized water. The acid washing treatment is composed of 10 parts by weight of hydrofluoric acid, 15 parts by weight of hydrogen peroxide, 8 parts by weight of citric acid, 7 parts by weight of tannic acid and 60 parts by weight of deionized water; the alkali washing treatment is composed of a compound of ammonium cerium nitrate and sodium hydroxide solution with a mass volume ratio of 1:20.

[0038] S4: spray a layer of 5 μm fluorosilicone resin on the magnetic and thermal conductive bottom layer treated in step S3 for fluorosilicone resin modification, then spray the non-stick coating material by vacuum cold spraying, and obtain the cold sprayed cookware after annealing. The total thickness of the coating on the surface of the cookware is 2.0 mm. The spraying temperature of the vacuum cold spraying is 340°C, the powder feeding rate is 400 g / min, and the spraying distance is 30 mm. The non-stick coating material is composed of PTFE resin powder with an average particle size of 30 μm, titanium dioxide powder with an average particle size of 0.7 μm, and aluminum oxide powder with an average particle size of 0.3 μm. Specifically, PTFE resin powder, titanium dioxide powder and aluminum oxide powder with a mass ratio of 3:2:2 are added to ethanol, and ultrasonic-assisted stirring is performed; after preparation, the mass concentrations of the titanium dioxide powder and aluminum oxide powder are both 6%. The treatment temperature of the annealing treatment is 210°C.

[0039] The cold sprayed cookware samples produced in this embodiment have no cracking after appearance inspection; the maximum electromagnetic heating power can reach 1800W, and the magnetic permeability is 90%; the average porosity of the cookware surface coating is 0.012%; the microhardness is 72.4HV 0.1; After 7 cycles of hot and cold shock test (heating at 280℃ for 60 minutes, then taking it out and cooling it in 25℃ tap water), the coating showed no defects such as shedding and cracking. At the same time, the non-stick performance test of fried eggs was carried out according to GB / T32095.2, and the test results showed that the evaluation level reached Level I.

[0040] Example 3

[0041] The method for manufacturing the cold spray cookware of this embodiment comprises the following steps:

[0042] S1: Provide an aluminum-based pot body after pre-treatments such as degreasing, sandblasting, and cleaning. The degreasing, sandblasting, and cleaning treatments of this embodiment are conventional technical means in the art and will not be described in detail here.

[0043] S2: Spray the composite powder including liquid metal (the liquid metal is a eutectic alloy of 75% gallium and 25% indium), copper, chromium, iron-chromium alloy and completely amorphous metal alloy on the inner surface of the aluminum-based pot body obtained in step S1 by magnetic field-assisted cold spraying to obtain a magnetic conductive and thermal conductive bottom layer; the mass ratio of the liquid metal, copper, chromium, iron-chromium alloy and metal alloy is 10:25:5:50:10; the thickness of the magnetic conductive and thermal conductive bottom layer is 1.5mm; the magnetic induction intensity of the magnetic field-assisted cold spraying is 1.0T, and the coercive force of the permanent magnet is 1000kA / m; the working gas pressure of the cold spraying is 2.5MPa, the spraying temperature is room temperature, the powder feeding rate is 500g / min, and the spraying distance is 30mm. The preparation method of the metal alloy is the same as that of Example 1.

[0044] S3: Screen print a layer of ink pattern on the magnetic and thermal conductive bottom layer obtained in step S2, and then carry out acid washing and alkali washing treatment in sequence; the ink is composed of 47 parts of water-soluble acrylic resin, 1 part of monoethanolamine, 1 part of polyethylene wax, 2 parts of glycerol, 90 parts of pigment and 60 parts of deionized water. The acid washing treatment is composed of 10 parts by weight of hydrofluoric acid, 15 parts by weight of hydrogen peroxide, 8 parts by weight of citric acid, 7 parts by weight of tannic acid and 60 parts by weight of deionized water; the alkali washing treatment is composed of a compound of ammonium cerium nitrate and sodium hydroxide solution with a mass volume ratio of 1:20.

[0045] S4: spray a layer of 5 μm fluorosilicone resin on the magnetic and thermal conductive bottom layer treated in step S3 for fluorosilicone resin modification, then spray the non-stick coating material by vacuum cold spraying, and obtain the cold sprayed cookware after annealing. The total thickness of the coating on the surface of the cookware is 2.5 mm. The spraying temperature of the vacuum cold spraying is 350°C, the powder feeding rate is 500 g / min, and the spraying distance is 50 mm. The non-stick coating material is composed of PTFE resin powder with an average particle size of 50 μm, titanium dioxide powder with an average particle size of 1 μm, and aluminum oxide powder with an average particle size of 0.5 μm. Specifically, PTFE resin powder, titanium dioxide powder and aluminum oxide powder with a mass ratio of 1:1:1 are added to ethanol, and ultrasonic-assisted stirring is performed; after preparation, the mass concentrations of the titanium dioxide powder and aluminum oxide powder are both 7%. The treatment temperature of the annealing treatment is 250°C.

[0046] The cold sprayed cookware samples produced in this embodiment have no cracking after appearance inspection; the maximum electromagnetic heating power can reach 1800W, and the magnetic permeability is 90%; the porosity of the cookware surface coating is 0.03%; the microhardness is 72.4HV 0.1 ; After 7 cycles of hot and cold shock test (heating at 280℃ for 60 minutes, then taking it out and cooling it in 25℃ tap water), the coating showed no defects such as shedding and cracking. At the same time, the non-stick performance test of fried eggs was carried out according to GB / T32095.2, and the test results showed that the evaluation level reached Level I.

[0047] Comparative Example 1

[0048] The manufacturing method of the cold spray cookware in this comparative example has the same operating steps as those in Example 1, except that, in the manufacturing method of this comparative example, the composite powder in step S2 does not include an amorphous metal alloy.

[0049] The cold sprayed cookware samples obtained in this comparative example showed no cracking after appearance inspection; the maximum electromagnetic heating power can reach 1600W, the magnetic permeability is 80%; the microhardness is 71.1HV 0.1 In the hot and cold shock test (heating at 280°C for 60 minutes, then taking it out and cooling it in 25°C tap water), it was observed that the coating had slight cracks and other defects in the 5th cycle.

[0050] Comparative Example 2

[0051] The manufacturing method of the cold spray cookware in this comparative example has the same operating steps as those in Example 1, except that in the manufacturing method of this comparative example, the composite powder in step S2 does not include liquid metal.

[0052] The cold sprayed cookware samples obtained in this comparative example showed no cracking after appearance inspection; the maximum electromagnetic heating power can reach 1600W, the magnetic permeability is 83%; the microhardness is 71.5HV 0.1 In the hot and cold shock test (heating at 280°C for 60 minutes, then taking it out and cooling it in 25°C tap water), it was observed that the coating had slight cracks and other defects in the 5th cycle.

[0053] Comparative Example 3

[0054] The manufacturing method of the cold spray cookware in this comparative example has the same operating steps as those in Example 1, except that the manufacturing method in this comparative example does not include step S3.

[0055] The cold sprayed cookware samples prepared in this comparative example showed no cracking after appearance inspection; after 5 cycles of hot and cold shock test (heating at 280°C for 60 minutes and then taking out and cooling in 25°C tap water), the coating was observed to have defects such as slight cracking.

[0056] Comparative Example 4

[0057] The manufacturing method of the cold spray cookware in this comparative example has the same operating steps as those in Example 1, except that, in the manufacturing method of this comparative example, no annealing treatment is performed in step S4.

[0058] The cold sprayed cookware samples made in this comparative example showed no cracking after appearance inspection; the maximum electromagnetic heating power can reach 1720W, the magnetic permeability is 83%; the microhardness is 64.8HV 0.1 ; After 6 cycles of hot and cold shock test (heating at 280°C for 60 minutes, then taking it out and cooling it in 25°C tap water), the coating was observed to have slight cracks and other defects.

[0059] It can be seen that the patent of the present invention has considerable advantages over the currently used technology. The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may have various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention to be protected.

Claims

1. A method for manufacturing a cold spray cookware, characterized in that: The production method comprises the following steps: S1: Provide aluminum-based pot body after pre-treatment; S2: Spraying a composite powder including at least a part of an amorphous metal alloy onto the inner surface of the aluminum-based pot body obtained in step S1 by means of magnetic field-assisted cold spraying to obtain a magnetically conductive and thermally conductive bottom layer; S3: firstly screen-printing a layer of ink pattern on the magnetic and thermal conductive bottom layer obtained in step S2, and then sequentially performing acid washing and alkali washing treatments; S4: performing fluorosilicone resin modification treatment on the magnetic and thermal conductive bottom layer treated in step S3, and then spraying a non-stick coating material by vacuum cold spraying, and obtaining the cold sprayed cookware after annealing treatment.

2. The method for making a cold spray cookware according to claim 1, characterized in that: The preparation method of the metal alloy comprises the following steps: firstly weighing raw materials consisting of iron powder, cobalt powder, silicon powder and boron powder, then smelting the alloy by arc melting under the protection of argon gas, then rapidly cooling at a cooling rate of 110±10° C. per minute, and finally obtaining the metal alloy by atomization.

3. The method for making a cold spray cookware according to claim 1, characterized in that: The composite powder also includes liquid metal, copper, chromium, iron or an iron-based alloy.

4. The method for making a cold spray cookware according to claim 1, characterized in that: The magnetic field assisted cold spraying has a magnetic induction intensity of 1.0-1.5T, and the coercive force of the permanent magnet is 500-1000kA / m; the working gas pressure of the cold spraying is 1.5-2.5MPa, the spraying temperature is room temperature, the powder feeding rate is 300-500g / min, and the spraying distance is 10-30mm.

5. The method for manufacturing a cold spray cookware according to claim 1, characterized in that: The ink consists of 42-47 parts of water-soluble acrylic resin, 0.5-1 parts of monoethanolamine, 0.5-1 parts of polyethylene wax, 1-2 parts of glycerol, 50-90 parts of pigment and 40-60 parts of deionized water.

6. The method for manufacturing a cold spray cookware according to claim 1, characterized in that: The acid washing treatment adopts hydrofluoric acid, hydrogen peroxide, citric acid, tannic acid and deionized water; the alkali washing treatment adopts cerium ammonium nitrate and sodium hydroxide solution.

7. The method for manufacturing a cold spray cookware according to claim 1, characterized in that: The spraying temperature of the vacuum cold spraying is 320-350° C., the powder feeding rate is 300-500 g / min, and the spraying distance is 20-50 mm.

8. The method for making a cold spray cookware according to claim 1, characterized in that: The non-stick coating material consists of PTFE resin powder with a particle size of 20 to 50 μm, titanium dioxide powder with a particle size of 0.5 to 1 μm and aluminum oxide powder with a particle size of 0.1 to 0.5 μm.

9. The method for manufacturing a cold spray cookware according to claim 1, characterized in that: The annealing treatment is performed at a temperature of 200-250°C.

10. A cold spray cookware, characterized in that: The cookware is manufactured by the manufacturing method of the cold spray cookware according to any one of claims 1 to 9.

Citation Information

Cited By

  • Aluminum base material IH applicable electric appliance inner pot and preparation method and application thereof

    CN120287007A

  • Aluminum base IH applicable electric cooker inner pot and preparation method and application thereof