Magnetic electrostatic spinning wound dressing as well as preparation method and application thereof
By introducing magnetic montmorillonite sheets into the polyvinylpyrrolidone skeleton to prepare magnetic electrospinning membranes, the problems of hemostasis and recurrence of wounds after hepatocellular carcinoma surgery were solved, and efficient hemostasis and magnetothermal efficacy were achieved.
Patent Information
- Application Number
- CN202410900414.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
AI Technical Summary
Postoperative recurrence and bleeding control of hepatocellular carcinoma are difficult problems. The existing magnetic medium solution is difficult to concentrate in the postoperative wound of liver cancer, and conventional wound dressings cannot firmly seal the wound in a wet environment, resulting in hemostasis failure.
Introduce magnetic montmorillonite sheets into the polyvinylpyrrolidone (PVP) skeleton, prepare magnetic electrospinning membranes through in-situ electrospinning technology, and combine with ethanol solution to form fiber membranes to improve stability and hemostatic performance in wet environments, and Prevent tumor recurrence by utilizing the magnetocaloric properties of magnetic montmorillonite.
Significantly improved the stability and hemostatic performance of the magnetic electrospun membrane in a wet environment, achieving rapid intraoperative hemostasis and postoperative recurrence prevention of liver cancer, reducing the disintegration rate from 100% to 15%, and preventing tumor killing through magnetic heat relapse.
Smart Images

Figure CN118846178A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and in particular to a magnetic electrostatic spinning wound dressing, a preparation method and application thereof. Background Art
[0002] Hepatocellular carcinoma (HCC) is a major challenge in the global public health field. Its five-year survival rate is only 18%. It is estimated that by 2030, more than one million patients worldwide will die from this disease. Although surgical resection is an important means of treating HCC, the recurrence rate of up to 70% within five years after surgery has become the main bottleneck of treatment failure. The residual tumor tissue at the resection margin of liver cancer and the intraoperative bleeding caused by the metastasis and implantation of tumor cells in the abdominal cavity are the main causes of postoperative recurrence of liver cancer. Although existing drugs such as sorafenib, Lenvatinib, and regorafenib are widely used in postoperative adjuvant treatment of HCC, their effect on improving postoperative survival rate is limited. Therefore, the prevention of postoperative recurrence and the effective control of intraoperative and postoperative bleeding during liver resection are still a major challenge in the current treatment of HCC.
[0003] Magnetic induction hyperthermia is a tumor treatment technology that relies on the heat generated by magnetic nanoparticles under an AC magnetic field to achieve local tumor temperature rise and thus kill the tumor. Compared with systemic chemoradiotherapy, magnetic induction hyperthermia has gradually attracted people's attention and research due to its advantages of almost no systemic toxicity, high tumor thermal killing efficiency, minimal invasion, and no tissue penetration depth. The implementation of local tumor magnetic hyperthermia has been proven to be an effective tumor treatment program. Conventional intravenous or intratumoral injection of magnetic medium solution is difficult to achieve the enrichment of magnetic medium in the wound after liver cancer surgery, and the magnetic medium solution has strong fluidity. Direct application on the wound after liver cancer surgery is easy to leak into the normal organs adjacent to the liver, causing damage to non-target tissues. Different from liquid preparations, solid wound dressings are excellent carriers for delivering magnetic media to the wound after tumor surgery. However, the wound after liver cancer surgery is slippery, and conventional wound dressings cannot firmly seal the liver wound due to the lack of wet environment adhesion and hemostasis, and there is a risk of falling off. Therefore, local magnetic hyperthermia for wounds after liver cancer surgery puts higher requirements on the wound dressing carrier.
[0004] In situ electrospinning technology has shown advantages in delicate surgeries such as minimally invasive liver resection due to its precise deposition, good wound matching and simple operability, and has great potential for clinical transformation. Polyvinylpyrrolidone (PVP), as a polymer with low toxicity, chemical stability and good biocompatibility, is widely used in the preparation of electrospinning membranes for wounds. However, due to the high water solubility of PVP, the pure PVP electrospinning frame is easy to disintegrate in a humid environment, and cannot quickly seal the bleeding wound, which easily leads to hemostasis failure.
[0005] Based on the above challenges, after in-depth research and repeated practice, the present invention proposes to introduce magnetic montmorillonite sheets into the PVP polymer skeleton, and successfully prepares a multifunctional magnetic electrospinning membrane (abbreviated as PMI) with excellent biosafety, wound hemostasis function and magnetothermal performance through in-situ electrospinning technology, which significantly improves the stability of the magnetic electrospinning membrane in a wet environment (the disintegration rate is reduced from 100% to 15%). With minimally invasive technology, the precise in-situ deposition of the spinning membrane on the liver wound surface under laparoscopic guidance is achieved, achieving the goal of intraoperative hemostasis and postoperative recurrence prevention of liver cancer. Summary of the invention
[0006] The purpose of the present invention is to solve the problem that polyvinyl pyrrolidone (PVP) cannot be deposited in situ on the surface of a bleeding wound to form an electrospinning film, and to provide a magnetic electrospinning wound dressing, a preparation method and an application thereof.
[0007] In order to achieve the above purpose, the present invention discloses a method for preparing a magnetic electrospinning wound dressing, and the specific process is as follows: polyvinyl pyrrolidone and magnetic montmorillonite particles are mixed in ethanol, and the fibers are deposited on a collecting plate to form a fiber film through an electrospinning device.
[0008] The preparation method of the magnetic montmorillonite particles comprises the following steps:
[0009] S1, adding montmorillonite and ferric acetylacetonate into tetraethylene glycol, and obtaining a uniformly dispersed solution by ultrasonic crushing;
[0010] S2, vacuum treating the mixed solution, and then performing a thermal decomposition reaction to in-situ grow ferroferric oxide nanoparticles on the montmorillonite;
[0011] S3, the high temperature reaction is finished, cooled to room temperature, centrifuged and washed to obtain magnetic montmorillonite particles.
[0012] In the step S1, the mass ratio of iron acetylacetonate to montmorillonite is 1:1.
[0013] The vacuum reaction time in step S2 is 120 minutes, the reaction temperature is increased from 30°C to 300°C, the heating time is 90 minutes, and the temperature is maintained for 30 minutes after the heating is completed.
[0014] In step S3, centrifugal washing is performed using ethanol washing, and the centrifugal speed is 3000 r / min.
[0015] The mass ratio of the magnetic montmorillonite particles to polyvinyl pyrrolidone is 1:1 to 1:3.
[0016] The volume of the ethanol was 5 mL.
[0017] The present invention discloses a magnetic electrostatic spinning wound dressing prepared by the above-mentioned preparation method and the application of the magnetic electrostatic spinning wound dressing in the preparation of hemostasis during liver cancer resection and postoperative anti-recurrence treatment drugs.
[0018] Compared with the prior art, the beneficial effects of the present invention are:
[0019] 1. The magnetic electrospinning wound dressing prepared by the present invention uses ethanol and polyvinyl pyrrolidone to prepare the spinning solution. Under the condition of ensuring biological safety, the magnetic montmorillonite is embedded in the polymer skeleton as a filler, so that the polyvinyl pyrrolidone electrospinning film has the ability to resist spontaneous disintegration in a humid environment;
[0020] 2. The magnetic electrospinning wound dressing prepared by the present invention has good hemostatic performance. The negative charge distribution on the surface of the montmorillonite sheet can activate the coagulation function of platelets / red blood cells. When blood interacts with the montmorillonite sheet in the magnetic electrospinning wound dressing, the negative charge on the montmorillonite and the high-efficiency liquid adsorption performance enhance the interfacial stimulation of red blood cells and improve the coagulation ability, thereby achieving the purpose of rapid hemostasis during liver cancer resection;
[0021] 3. The magnetic montmorillonite sheet has stable magnetothermal heating performance, which gives the magnetic electrospinning membrane the ability to kill tumors magnetothermally, and can effectively prevent the recurrence of liver cancer after resection. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Schematic diagram of synthesizing magnetic electrospinning membrane in the present invention (a), and photos of PVP, PMI1, PMI2, and PMI3;
[0023] Figure 2 is a scanning electron microscope image of montmorillonite in the present invention;
[0024] Figure 3 is a scanning electron microscope image of the magnetic montmorillonite of the present invention;
[0025] Figure 4 is a transmission electron microscope image of the magnetic montmorillonite in the present invention;
[0026] Figure 5 Scanning electron microscope photos (a) and transmission electron microscope photos (b) of different ratios of PVP and magnetic montmorillonite (1:0, 1:1, 1:2, 1:3);
[0027] Figure 6 The infrared spectra of PVP, MMT, MI and PMI3;
[0028] Figure 7 XRD patterns of PVP, MI and PMI3;
[0029] Figure 8Thermogravimetric analysis diagrams of PVP, MI, and PMI3;
[0030] Fig. 9 The disintegration photos of different ratios of PVP and magnetic montmorillonite (PVP, PMI1, PMI2, PMI3) in the blood (a), and the disintegration rate after 20 minutes (b);
[0031] Fig.10 Schematic diagram of the shrinkage resistance of different ratios of PVP and magnetic montmorillonite (PVP, PMI1, PMI2, PMI3) under constant temperature and humidity (a), and the shrinkage resistance after 48 hours (b);
[0032] Fig.11 The film formation of two ratios (PVP, PMI3) of electrospinning in a wet environment for 5 minutes;
[0033] Fig.12 The magnetic thermal heating curves (a) and infrared thermal imaging images (b) of PVP and PMI3;
[0034] Fig.13 This is a demonstration diagram of the magnetic properties of PVP and PMI3;
[0035] Fig.14 The adhesion performance of the magnetic electrospun wound dressing in the embodiment of the present invention is shown in Figure 1. Schematic diagram of in-situ electrospinning on the skin (a), and a photo of the adhesion demonstration of in-situ electrospinning of PMI3 on pig skin, pig liver, and pig kidney after unfolding, twisting, and folding (b);
[0036] Fig.15 The mechanical properties of the magnetic electrospun wound dressing in the embodiment of the present invention are shown in Figure 1. The tensile schematic diagram of PMI3 (a) and the stress-strain curve (b);
[0037] Fig.16 Actual photos of hemolysis of different components (a) and a bar graph of hemolysis rate (b);
[0038] Fig.17 The in vitro hemostatic performance of the magnetic electrospun wound dressing in the embodiment of the present invention. In vitro plate coagulation images of different components (a), and coagulation time bar graph (b);
[0039] Fig.18 The in vitro hemostatic performance of the magnetic electrospun wound dressing in the embodiment of the present invention. In vitro coagulation photos of different materials (a), and the OD values of the corresponding supernatants of different groups (b);
[0040] Fig.19 Schematic diagram of coagulation mechanism (a), scanning electron micrograph of red blood cells in the untreated group (b), scanning electron micrograph of red blood cells after PMI3 treatment (c);
[0041] Fig. 20 The in vivo hemostatic performance of the magnetic electrospun wound dressing in the embodiment of the present invention. The hemostatic time of rat liver (a) and the comparison of blood loss (b);
[0042] Fig.21 The in vivo hemostatic performance of the magnetic electrospun wound dressing in the embodiment of the present invention. Actual photo of liver hemostasis in the abdominal cavity of a rabbit (a), and comparison of blood loss (b);
[0043] Fig. 22 This is the in vivo efficacy evaluation of the magnetic electrospinning wound dressing in the embodiment of the present invention. Photos of tumor growth in mice after treatment;
[0044] Fig.23 This is an in vivo treatment evaluation of the magnetic electrospinning wound dressing in the embodiment of the present invention. Infrared thermal image of mice after exposure to an alternating magnetic field (a), and the corresponding temperature change curve (b);
[0045] Fig.24 This is an in vivo treatment evaluation of the magnetic electrospinning wound dressing in the embodiment of the present invention. Tumor growth volume curve of mice after treatment in each group (a), tumor weight bar graph on the 8th day (b), and comparison of postoperative recurrence of mice (c);
[0046] Fig.25 This is the in vivo treatment evaluation of the magnetic electrospinning wound dressing in the present invention. H&E staining and TNFα section data of mice after 8 days of treatment in each group (B) Quantification of cell nuclei in tumor tissue sections. DETAILED DESCRIPTION
[0047] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.
[0048] Example 1
[0049] 1. Preparation of magnetic montmorillonite
[0050] Weigh 300 mg of sodium montmorillonite and 300 mg of ferric acetylacetonate in 50 mL of tetraethylene glycol, and place the resulting solution under an ultrasonic crusher for 5 minutes to make the solution evenly dispersed;
[0051] Transfer the solution after ultrasonic disruption to a three-necked flask, connect a condenser, add a magnet, stir on a magnetic stirrer, seal the gas outlet with a rubber stopper, start vacuuming, and maintain for 2 hours;
[0052] After the vacuum is over, nitrogen is introduced and the reaction is placed on a heating device. The temperature is raised from 30°C to 300°C in 90 minutes and kept at 300°C for 30 minutes. Nitrogen reflux is required for the entire reaction.
[0053] After cooling to room temperature, centrifuge at 3000r / min for 10min, wash three times with ethanol, collect and dry.
[0054] Figure 1 (a) is a schematic diagram of the synthesis of magnetic electrospinning membrane PMI3. Figure 2 This is a scanning electron microscope image of montmorillonite. Figure 3 This is a scanning electron microscope image of magnetic montmorillonite. Figure 4 This is a transmission electron microscope picture of magnetic montmorillonite. By comparison, it can be seen that magnetic iron oxide nanoparticles can be successfully grown in situ on montmorillonite sheets.
[0055] 2. Preparation of magnetic electrospinning membrane
[0056] Weigh polyvinyl pyrrolidone (PVP) and magnetic montmorillonite iron in a ratio of 1:3, dissolve in 5 mL of ethanol, stir with a magnetic stirrer, load into a 5 mL syringe and place in a portable electrospinning device to obtain an electrospinning membrane in a collector.
[0057] Example 2
[0058] In this embodiment, the doping ratio of PVP and magnetic montmorillonite is 1:0, and other preparation conditions are the same as those in Example 1.
[0059] Example 3
[0060] In this embodiment, the doping ratio of PVP and magnetic montmorillonite is 1:1, and other preparation conditions are the same as those in Example 1.
[0061] Example 4
[0062] In this embodiment, the doping ratio of PVP and magnetic montmorillonite is 1:2, and other preparation conditions are the same as those in Example 1.
[0063] like Figure 1 (b) is a schematic diagram of electrospun membranes with different proportions. Figure 5 The scanning electron microscope and transmission electron microscope images of electrospun membranes with different proportions show that the fibers of pure PVP are randomly distributed and have a smooth surface. As the doping amount increases, the fiber surface begins to become rough, and magnetic montmorillonite protrusions begin to appear in the middle of the fiber. The higher the content, the more protrusions there are. These montmorillonite layers are stacked, filling the entire framework and playing a role in fixing the structure. Figure 6 The infrared spectra of PVP, MMT, MI, and PMI3 show the characteristic peaks of montmorillonite minerals, ~3576-3230cm -1 Al-OH bending vibration, ~1037cm -1 Vibration of Si-O skeleton, ~1290cm -1CN stretching vibration, this series is the characteristic peak of montmorillonite, ~1651cm -1 The peak is the characteristic peak of C=O stretching vibration, ~1462cm -1 This is the CH bending vibration, and this series of peaks are characteristic peaks of PVP. This shows that montmorillonite has been successfully compounded on the PVP fiber skeleton. In the XRD spectrum, the characteristic crystal plane of ferroferric oxide in PMI can be seen, confirming that magnetic montmorillonite is on the spinning fiber. Figure 8 It can be seen that the thermogravimetric analysis spectrum shows that the ratio of the final product PVP and magnetic montmorillonite is 1:3, which is consistent with the conditions.
[0064] Fig. 9 The disintegration of the electrospun membrane in the blood at different ratios in the embodiments of the present invention is shown in detail, including the actual disintegration picture (a) and the disintegration rate statistics after 20 minutes (b). In view of the high risk of bleeding and liver wound infiltration that often accompanies hepatocellular carcinoma resection, this experiment simulated acute bleeding conditions to evaluate the structural stability of the electrospun PMI film. Fig. 9 It can be clearly observed from the data analysis of (b) that with the increase of MI content, the anti-disintegration performance of electrospun PMIs membrane in blood gradually improves. Among them, the PMI3 film showed excellent stability, and its disintegration rate was only 15.31±7.90%, which was significantly lower than PVP (100%), PMI1 (80.92±5.58%) and PMI2 (50.14±6.72%). This discovery not only provides key data support for understanding the behavior of PMI films in the blood environment, but also lays a solid foundation for the development of medical materials with excellent anti-blood disintegration performance.
[0065] Fig.10 The shrinkage performance of the electrospun membranes of different proportions in the embodiments of the present invention under standard environmental conditions (temperature 25°C, humidity 60%) is shown. By observing the actual image (a), it can be clearly seen that with the gradual increase of the MI sheet content in the PVP skeleton, the anti-shrinkage performance of the electrospun PMIs film is significantly improved. Fig.10The data in (b) further confirm this trend. Compared with the significant shrinkage rate of the electrospun PVP film (80.11±3.48%), the electrospun PMI3 film still maintains a low shrinkage rate (12.75±5.03%) after 48 hours of shrinkage test, showing excellent anti-shrinkage performance. In addition, the shrinkage rate of the electrospun PMI3 film is also significantly lower than that of the electrospun PMI1 film (78.65±3.50%) and the electrospun PMI2 film (46.60±4.90%), which further proves the effectiveness of the addition of MI sheets in improving the stability of electrospun PMIs films. The reason why the electrospun PMIs film of the present invention has good anti-shrinkage ability is mainly due to the synergistic effect between PVP fibers and MMT sheets. The MMT sheet effectively stabilizes the fiber skeleton and regulates the spontaneous shrinkage behavior of the PVP fiber through the intermolecular interaction between the MMT sheet and the PVP fiber. At the same time, the PVP fiber provides a solid support skeleton for the MMT sheet. Under the optimized combination of PVP and magnetic montmorillonite content ratio of 1:3, the anti-shrinkage rate of the electrospun PMIs film of the present invention is as high as more than 80%, which is significantly better than other ratio combinations. Therefore, the ratio of PVP and magnetic montmorillonite content selected in the embodiment of the present invention is 1:3, which is regarded as the optimal ratio. This discovery is of great significance for improving the stability and performance of electrospun PMIs films in practical applications.
[0066] Fig.11 The film formation of two electrospinning methods in a wet environment for 5 minutes with a ratio of PVP to magnetic montmorillonite of 1:0 and 1:3 in the embodiment of the present invention (a), and the film peeling demonstration diagram of the ratio of 1:3 after film formation (b). Because PVP nanofibers are hydrophilic, the nanofibers dissolve rapidly once they come into contact with the wet tissue surface and are difficult to deposit on the wet surface. However, montmorillonite, as a blocking structure, blocks the fiber dissolution, causing the fiber to gradually deposit on the wet surface.
[0067] Fig.12 The comparison of the magnetocaloric properties of PVP and PMI3 under the action of an alternating magnetic field (AMF) in the embodiments of the present invention is presented in detail. Fig.12 As shown in (a), when PMI3 is exposed to an alternating magnetic field, especially at a field strength of 25 kA / m, its magnetocaloric temperature increases significantly over time, from an initial 25°C to 50°C. This significant temperature rise characteristic enables it to have the potential to kill tumor cells in medical applications. Furthermore, Fig.12 (b) shows the infrared thermal image under the action of an alternating magnetic field, which intuitively reflects the magnetothermal response of the PMI3 material. By adding magnetic montmorillonite, PMI3 produces efficient heat conversion under the action of a magnetic field, a property that is of great significance for tumor hyperthermia treatment.
[0068] exist Fig.13In the embodiment of the present invention shown, we show a comparative demonstration of the magnetic properties of PVP and PMI3. In the experiment, when the PVP fiber membrane is close to the magnet, no adsorption phenomenon occurs, and it has been verified that the influence of electrostatic interference has been eliminated. In contrast, when the PMI3 material is close to the magnet, due to the presence of magnetic montmorillonite particles embedded inside, it shows significant magnetic adsorption characteristics. This result clearly verifies that the wound dressing prepared by electrospinning technology is indeed magnetic.
[0069] Fig.14 The schematic diagram of PMI3 adhesion to pig skin tissue (a) and the actual adhesion diagram on different tissues (b) in the embodiment of the present invention show that a hole with a diameter of 10 mm is punched in the pig skin, liver and kidney. After in situ electrospinning on the tissue surface, the fiber membrane is tightly attached to the tissue surface after twisting and folding, indicating that in situ electrospinning has excellent adhesion properties. Fig.15 Schematic diagram of PMI3 stretching (a) and tensile strain-stress curve (b). It can be seen that the stress reaches 81Kpa, which can meet the adhesion requirements for the bleeding liver edge.
[0070] exist Fig.16 The hemolytic performance of a specific material in an embodiment of the present invention is shown in Figure (a) and Figure (b). As shown in Figure (a) and Figure (b), the material did not undergo hemolysis and fully met the predetermined hemolysis evaluation criteria. Fig.17 In this study, we conducted an in-depth study on the in vitro hemostatic properties of PMI3 fiber membrane. The hemostatic ability of PMI3 was comprehensively investigated through in vitro coagulation experiments and blood absorption capacity evaluation. As shown in the in vitro well plate coagulation image in Figure (a) and the coagulation time bar graph in Figure (b), PMI3 can form a complete and stable blood clot in a very short time (1.5±0.2min), and its coagulation time is much lower than that of the control group (7.3±0.2min), gelatin sponge group (3.4±0.3min), PVP group (5.3±0.3min) and MI group (2.9±0.2min). This significant advantage shows that PMI3 material exhibits excellent coagulation ability in in vitro experiments, indicating its great potential in clinically effectively stopping severe bleeding situations such as liver bleeding. In addition, through continuous experimental observation and evaluation of the absorbance of the clot supernatant, we further confirmed the coagulation effect of PMI3 material. The clots treated with PMI3 reached a stable state in a very short time, and the relative absorbance value of the supernatant at 545 nm was significantly lower than that of other samples, which fully demonstrated that PMI3 can significantly promote the in vitro coagulation process.
[0071] Fig.17The in vitro hemostatic performance of the magnetic electrospinning wound dressing in the embodiment of the present invention. The hemostatic ability of the PMI3 fiber membrane was examined by in vitro coagulation experiments and blood absorption capacity evaluation. Through the in vitro well plate coagulation images (a) of different components, and the coagulation time bar graph (b) analysis, compared with the control group, PMI3 had a complete and stable blood clot after 1.5±0.2min. The coagulation time was much lower than that of other groups. (Control group: 7.3±0.2min, gelatin sponge group: 3.4±0.3min, PVP: 5.3±0.3min, MI: 2.9±0.2min) This shows that the PMI3 material has good coagulation ability and can effectively stop liver bleeding clinically. Fig.18 Through continuous experimental observation and evaluation of the absorbance of the clot supernatant, the coagulation ability and state of the clot were understood. The clot treated with PMI3 reached a stable state after 5 minutes, and the relative absorbance value (OD at 545nm) of the supernatant was significantly lower than that of other samples, indicating that PMI3 can effectively promote in vitro coagulation. Fig.19 (a), (b), and (c) show the coagulation mechanism observed using a scanning electron microscope. Protein fibers on the surface of red blood cells can be clearly observed in the scanning electron microscope images of whole blood directly dropped onto MI and PMI3. In contrast, this phenomenon is not seen in red blood cells without any sample added.
[0072] Fig. 20 In order to further study the in vivo hemostatic performance of the in situ magnetic electrospun membrane in the rat liver hemostasis model in the present invention, the electrospun PMI3 film was precisely deposited at the bleeding site of the liver using an in situ deposition method. Blood loss is a key indicator for evaluating hemostatic ability. Fig. 20 As shown in (b), the blood loss of the electrospun PMI3 film group was 0.16±0.05g, which was significantly lower than that of the control group (1.45±0.13g) and the gelatin sponge treatment group (0.52±0.12g). In order to further verify the hemostatic effect of PMI3, the present invention selected the in situ electrospinning hemostasis in the liver of New Zealand rabbits. Fig.21 As shown in (a) and (b), the electrospun PMI3 film showed precise in situ deposition on the liver wound and achieved effective hemostasis. Compared with the gauze compression hemostasis group (blood loss: 15.49±3.81g), the blood loss in the electrospun PMI3 film treatment group was significantly reduced (3.39±0.76g). These results indicate that laparoscopically guided in situ deposition of electrospun PMI3 film provides an effective approach for hemostasis during HCC resection.
[0073] Currently, surgical resection is still one of the main strategies for treating liver cancer, but postoperative recurrence is a major problem facing this method. Therefore, the efficacy of electrospun PMI3 film combined with AMF in preventing tumor recurrence was evaluated using a mouse subcutaneous tumor resection model (e.g. Fig. 22 ).like Fig.23 As shown in the figure, the thermal infrared images and temperature changes of the blank group and the PMI3 film + AMF combined treatment group in the coil were compared. The data showed that under the magnetic field, the temperature of the tumor site in the PMI3 film + AMF combined treatment group reached 45°C within 10 minutes, which was enough to ablate tumor cell tissue. Fig.24 (a) and (b) are the changes of tumors within 8 days after excision treatment. After 8 days of treatment, the tumor volume and weight of mice in the PMI3 film + AMF combined treatment group decreased to 0, while the tumor volume of mice in the PBS + AMF treatment group was 210.79 ± 29.20 cm 3 The tumor weight was 0.36±0.09 g, and the tumor volume of mice in the PMI3-treated group was 144.26±50.06 cm 3 , the tumor weight was 0.29±0.09g. Fig.24 As shown in (c), there was no tumor recurrence in the postoperative mice treated with PMI3 film + AMF combination within 8 days, while the PBS + AMF treatment group and the electrospun PMI3 film treatment group showed obvious signs of tumor recurrence within 8 days, and the tumor recurrence rate of the PBS + AMF treatment group and the electrospun PMI3 film treatment group reached 100%, which was much higher than that of the electrospun PMI3 film + AMF treatment group (0%).
[0074] like Fig.25 As shown in the figure, hematoxylin and eosin (H&E) staining was performed on mouse skin tissue, and the images showed that a small number of apoptotic cells were observed in the PBS+AMF and electrospun PMI3 film treatment groups, while more extensive necrosis occurred in the electrospun PMI3 film+AMF treatment group. Fig.25 As shown in the figure, the quantitative statistics of cell nuclei further confirmed that magnetic hyperthermia induced cell apoptosis, which was significantly higher than that of PBS+AMF (5548±582nuclei / mm 2 ) and PMI3 film alone (5479±547 nuclei / mm 2 ) treatment group, the number of nuclei in the tumor sections of the PMI3+AMF group (297±75nuclei / mm 2 The above experimental data show that the combination of electrospun PMI3 film and AMF can effectively inhibit tumor recurrence.
[0075] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.
Claims
1. A method for preparing a magnetic electrospinning wound dressing, characterized in that: The specific process is as follows: polyvinyl pyrrolidone and magnetic montmorillonite particles are mixed in an ethanol solution, and the fibers are deposited on a collecting plate through an electrospinning device to form a fiber membrane.
2. The method for preparing a magnetic electrospinning wound dressing according to claim 1, characterized in that: The preparation method of the magnetic montmorillonite particles comprises the following steps: S1, adding montmorillonite and ferric acetylacetonate into tetraethylene glycol, and obtaining a uniformly dispersed solution by ultrasonic crushing; S2, vacuum treating the mixed solution, and then performing a thermal decomposition reaction to in-situ grow ferroferric oxide nanoparticles on the montmorillonite; S3, the high temperature reaction is finished, cooled to room temperature, centrifuged and washed to obtain magnetic montmorillonite particles.
3. The method for preparing a magnetic electrospinning wound dressing according to claim 2, characterized in that: In the step S1, the mass ratio of iron acetylacetonate to montmorillonite is 1:
1.
4. The method for preparing a magnetic electrospinning wound dressing according to claim 2, characterized in that: The vacuum reaction time in step S2 is 120 minutes, the reaction temperature is increased from 30°C to 300°C, the heating time is 90 minutes, and the temperature is maintained for 30 minutes after the heating is completed.
5. The method for preparing a magnetic electrospinning wound dressing according to claim 2, characterized in that: In step S3, centrifugal washing is performed using ethanol washing, and the centrifugal speed is 3000 r / min.
6. The method for preparing a magnetic electrospinning wound dressing according to claim 1, characterized in that: The mass ratio of the magnetic montmorillonite particles to polyvinyl pyrrolidone is 1:1 to 1:
3.
7. The method for preparing a magnetic electrospinning wound dressing according to claim 1, characterized in that: The volume of the ethanol was 5 mL.
8. A magnetic electrospinning wound dressing prepared by the preparation method according to any one of claims 1 to 7.