Medical adhesive powder capable of gelling when encountering water as well as preparation method and application of medical adhesive powder

Medical adhesive powder is prepared through the cross-linking technology of poly(acrylic acid-succinimide) and polyethyleneimine, which solves the problems of weak adhesive force and complicated operation in the existing technology, and achieves high adhesiveness and biological Compatible medical adhesive for a variety of medical applications.

CN118846194APending Publication Date: 2024-10-29SHANDONG ACADEMY OF PHARMACEUTICAL SCIENCES
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410834107.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing medical adhesives have problems with weak adhesion, low water absorption capacity, complex operation, and high toxic and side effects in terms of hemostasis, wound closure, and dynamic wound adhesion.

Method used

Poly(acrylic acid-succinimide) and polyethyleneimine are cross-linked through hydrogen bonds and a small amount of covalent bonds to form a hydrogel. After freeze-drying and grinding, the medical adhesive powder is obtained. It has the characteristics of rapid water absorption and strong gel formation. Adhesion and ease of use.

Benefits of technology

It provides medical adhesive powder with high adhesion, safety and good biocompatibility, which is suitable for wet and dynamic wounds, extends the storage time, simplifies the operation process, and improves the sealing ability of biological tissues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention provides medical adhesive powder capable of gelling when encountering water as well as a preparation method and application of the medical adhesive powder, and belongs to a medical polymer biomaterial. The medical adhesive powder comprises a network system formed by cross-linking of poly (acrylic acid-succinimide) and polyethyleneimine, and the mass ratio of the poly (acrylic acid-succinimide) to the polyethyleneimine is (0.5-5): (0.5-5). The medical adhesive powder provided by the invention has extremely strong hydrophilicity, can quickly form gel after absorbing water, and shows good adhesion performance to different materials and biological tissues. The adhesive powder provided by the invention is simple in preparation method, low in cost and good in biocompatibility.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical polymer biomaterials, and in particular to a strong adhesive medical adhesive powder which can form gel when in contact with water, and a preparation method and application thereof. Background Art

[0002] Medical adhesives are medical materials that can be used in the medical field and have certain cell compatibility, mechanical strength and adhesion. Compared with ordinary adhesives, medical adhesives usually have corresponding biologically active functions in addition to adhesion, bonding and support functions. As a means of treatment and auxiliary treatment in clinical applications, medical adhesives have developed rapidly in recent years. Their application range has gradually expanded from tissue bonding and hemostasis to sealing, auxiliary medical device adhesion, accelerated wound healing and other functions.

[0003] At present, most medical adhesives used in clinical applications have certain limitations. For example, the widely used cyanoacrylate adhesives and fibrin glue play a certain role in hemostasis, wound closure and wound healing. Among them, fibrin glue has been proven to be superior to cotton fiber medical gauze in hemostasis since the beginning of the 20th century, and a large number of related studies and hemostasis products have emerged since then.

[0004] Chinese invention patent CN116693657A discloses a method for preparing a porcine fibrin hemostatic agent, which can reduce the damage to the active ingredients in fibrin while increasing the yield of functional protein, thereby enhancing its procoagulant hemostatic activity. Although fibrin exhibits high procoagulant activity, the tissue adhesion of fibrin adhesives is weak and cannot achieve effective closure of severe bleeding. Moreover, the fibrin glue currently used in clinical practice is mostly taken from animals, so it faces the problems of immunogenicity and pathogen contamination. The complicated operation steps and harsh storage conditions are also the disadvantages of fibrin adhesives.

[0005] Chinese invention patent CN112826976A discloses a low-whitening cyanoacrylate medical adhesive, which is mainly composed of cyanoacrylate. By adding a modifier, the whitening phenomenon of cyanoacrylate adhesives can be effectively reduced, and the adhesive properties of the adhesive can be significantly improved. The disadvantages of cyanoacrylate adhesives include poor biosafety, hardening in water, not easy to degrade, and easy to crack.

[0006] Chinese invention patent CN 113663117A discloses an anti-swelling bioadhesive, which is composed of a hydrogel substrate and a high molecular polymer brush bonded to the surface of the hydrogel substrate, and has certain anti-swelling properties as a hydrogel. However, although hydrogel has become a common dosage form of bioadhesive due to its good hydrophilicity, it is easy to age, has a short storage time, and has limited water absorption capacity and mechanical properties, and its adhesive ability to wet wounds or dynamic wounds needs to be improved. Summary of the invention

[0007] In view of the problems of weak adhesion, low water absorption capacity, complicated use method and easy peeling of dynamic wounds in traditional adhesives, this application proposes the following technical solutions:

[0008] On the one hand, the present application provides a medical adhesive powder, which includes a network system formed by cross-linking poly(acrylic acid-succinimide) and polyethyleneimine, and the mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine is (0.5~5):(0.5~5).

[0009] In one embodiment, the mass ratio of the poly(acrylic acid-succinimide) to polyethyleneimine is (3-1):(1-2), preferably (2-1):(1-2), for example, 2:1, 1:1, 1:2, and more preferably 1:1.

[0010] In one embodiment, the polyethyleneimine has the following structural formula:

[0011]

[0012] Preferably, the molecular weight of the polyethyleneimine is 10,000-150,000, for example, 10,000, 20,000, 30,000, 40,000, 50,000, 60,000, 70,000, 80,000, 90,000, 100,000, 110,000, 120,000, 130,000, 140,000, or 150,000.

[0013] Preferably, the molecular weight of the polyethyleneimine is 50,000-100,000, more preferably 60,000-80,000.

[0014] In one embodiment, the poly(acrylic acid-succinimide) has a structure as shown in formula (I):

[0015] ...... (I),

[0016] In formula (I), n is 100-4000, and m is 1-800.

[0017] Among them, the poly(acrylic acid-succinimide) with the above-mentioned degree of polymerization has a certain proportion of succinimide groups and a certain molecular weight. At a certain proportion of succinimide groups, the bonding ability of the adhesive system can be significantly improved, while too much proportion will lead to a decrease in the overall bonding strength of the system; at a certain molecular weight, poly(acrylic acid-succinimide) can have physical and chemical properties that are more suitable for composite with polyethyleneimine to make adhesive applications.

[0018] In one embodiment, the adhesive powder described in the present application has a porous structure on the surface and below the surface at the microscopic level. The skeleton structure of the porous structure has a uniform texture and a wide distribution of pore sizes, ranging from tens to hundreds of microns, and most of these pores are not connected, forming a cross-linked network system.

[0019] In one embodiment, the particle size of the medical adhesive powder is 10-1000 μm.

[0020] Preferably, the average particle size of the medical adhesive powder is 10-500 μm, more preferably 50-200 μm.

[0021] On the other hand, the present application provides a method for preparing the above-mentioned medical adhesive powder, comprising:

[0022] Step 1, respectively preparing a poly(acrylic acid-succinimide) solution and a polyethyleneimine solution, mixing them according to a mass ratio and fully stirring them, so that the poly(acrylic acid-succinimide) and the polyethyleneimine are cross-linked through hydrogen bonds and a small amount of covalent bonds to form a hydrogel;

[0023] Step 2: freeze-drying the hydrogel to make it into powder, thereby obtaining the medical adhesive powder.

[0024] In one embodiment, in the step 1, the concentration of the poly(acrylic acid-succinimide) solution is 5% to 50%, and the concentration of the polyethyleneimine solution is 5% to 50%.

[0025] In one embodiment, the solvent for preparing the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution is water, preferably ultrapure water.

[0026] Optionally, the concentrations of the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, etc., and they can be mixed in equal volumes or in proportion. The mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine in the final solution can be the required mass ratio.

[0027] In one embodiment, the mixing and stirring time in step 1 is 30 to 120 s, for example, 50 s, 75 s, 100 s, etc., and then standing at room temperature for 0 to 3 min.

[0028] In one embodiment, the freeze-drying conditions in step 2 are: freeze-drying at -40°C for 2-5 days, for example, 2 days, 3 days, 4 days, or 5 days.

[0029] In one embodiment, in the step 2, the hydrogel is freeze-dried to prepare a powder with a size of 10 to 1000 μm.

[0030] In one embodiment, the hydrogel is freeze-dried and then ground into powder.

[0031] In one embodiment, the grinding time is 5 to 15 min, for example, 5 min, 10 min, or 15 min.

[0032] In one embodiment, the grinding process of the hydrogel freeze-dried product is carried out in a dry environment, for example, the grinding can be carried out under an infrared sample preparation lamp.

[0033] In one embodiment, the powdered hydrogel freeze-dried product is sealed and stored at -40°C.

[0034] In one embodiment, the poly(acrylic acid-succinimide) is prepared by polymerization of acrylic acid and N-acryloyloxysuccinimide, and the reaction molar ratio is (100-4000):(1-800).

[0035] Specifically, the polymerization reaction is reversible addition-fragmentation chain transfer polymerization (RAFT).

[0036] In one embodiment, the feed ratio of N-acryloxysuccinimide in poly(acrylic acid-succinimide) is 0.01% to 25% of the total molar number of acrylic acid and N-acryloxysuccinimide, for example, it can be 0.01%, 1%, 5%, 10%, 15%, 20% and 25%, etc., preferably 1% to 20%.

[0037] In one embodiment, the solvent for the polymerization reaction is N,N-dimethylacetamide.

[0038] In one embodiment, the N,N-dimethylacetamide solvent is an ultra-dry solvent.

[0039] In one embodiment, an initiator and a chain transfer agent are further added into the reaction.

[0040] In one embodiment, the molar ratio of the acrylic acid, N-acryloxysuccinimide initiator and chain transfer agent is (100-4000):(1-800):1:(0.2-0.4).

[0041] In one embodiment, the initiator is 4-cyano-4-[[(dodecylthio)thionemethyl]thio]pentanoic acid.

[0042] In one embodiment, the chain transfer agent is azobisisobutyronitrile.

[0043] In one embodiment, the volume ratio of the mass of acrylic acid, N-acryloyloxysuccinimide, 4-cyano-4-[[(dodecylthio)thioketonemethyl]thio]pentanoic acid and azobisisobutyronitrile to the N,N-dimethylacetamide solvent is 1:(3-5).

[0044] In one embodiment, the reaction conditions are: in a closed environment without oxygen, at 65° C. to 75° C. for 15 to 30 h.

[0045] In one embodiment, deoxygenation is performed by passing a non-reactive gas, such as nitrogen or an inert gas.

[0046] In one embodiment, the reaction is followed by dialysis and freeze-drying.

[0047] In one embodiment, the dialysis time is 2 to 5 days, the water change frequency during the dialysis process is 2 to 6 times / d, and the molecular weight cutoff of the dialysis bag is 500 to 5000 Da.

[0048] In one embodiment, the freeze-drying method comprises: freeze-drying at -40°C for 2 to 5 days.

[0049] On the other hand, the present application provides the use of the medical adhesive, or the medical adhesive prepared by the preparation method, in the preparation of trauma auxiliary treatment products.

[0050] In one embodiment, the trauma auxiliary treatment product includes, but is not limited to, protective products for hemostasis and wounds, tissue sealing products, drug delivery products, injury protection products, injury repair products and / or biological scaffolds, etc.

[0051] In one embodiment, according to the actual application scenario, conventional additive components in the art may be added to the adhesive network system provided in the present application, or other active functional ingredients may be added to make it have other active functions.

[0052] In one embodiment, the medical adhesive powder has a gelling time of less than 5 s when exposed to water.

[0053] In one embodiment, the water absorption capacity of the medical adhesive powder is 0.5 to 2.5 times its own mass.

[0054] In one embodiment, the shear strength of the medical adhesive powder on the polyethylene sheet is 20-30 kPa.

[0055] In one embodiment, the medical adhesive powder is suitable for use on moist wounds and / or dynamic wounds.

[0056] In one embodiment, the wound is a hemorrhagic wound, including organ bleeding caused by accidental trauma or occurring during surgery.

[0057] Alternatively, the organ may be the liver, spleen, kidney, gastrointestinal tract, heart or skin.

[0058] In one embodiment, the method for using the medical adhesive powder is as follows:

[0059] For moist wound tissue, take an appropriate amount of the medical adhesive powder and cover it on the wound surface. The adhesive powder immediately absorbs the blood or tissue fluid on the wound surface to form a gel-like seal on the wound. For dry tissue or medical devices, take an appropriate amount of the medical adhesive powder, add 1 to 1.5 times the weight of water to the powder, and let it stand for a few seconds to obtain a gel-like adhesive, which is then applied to the surface of the tissue or medical device.

[0060] This application has at least the following technical advantages or effects:

[0061] 1. In view of the problems of weak adhesion, complex operation and large toxic and side effects of existing medical adhesives, the present application provides a medical adhesive powder that can form gel when exposed to water, has high adhesion and is easy to use, and a preparation method thereof. The present application polymerizes acrylic acid and N-acryloyl succinimide into poly(acrylic acid-succinimide) through a RAFT reaction, cross-links poly(acrylic acid-succinimide) with polyethyleneimine through hydrogen bonds and a small amount of covalent bonds to form a hydrogel, and finally freeze-dries and grinds to obtain a medical adhesive powder. The preparation method of the medical adhesive powder is simple, the raw materials are cheap and easy to obtain, and the adhesive powder has the characteristics of rapid water absorption and gelation, strong adhesion, suitability for dynamic environments and simple use, and can be widely used in the field of medical bonding.

[0062] 2. In the preparation and use method of the medical adhesive powder provided in the present application, the raw material synthesis and the mixing and powdering process are simple, the storage and transportation conditions of the obtained adhesive powder are simple, the use method is simple, and the application range is wide; and the adhesive powder contains only two components, the composition is simple, and the preparation process of the adhesive powder only requires mixing, freeze drying and grinding, and the process is simple. In addition, the prepared adhesive powder is simple to use, and does not require complex equipment and complicated operation steps.

[0063] 3. The medical adhesive provided in the present application is normally stored in a powder dosage form. On the one hand, compared with other dosage forms, it is not easy to age and deteriorate and has a long storage time; on the other hand, the solid powder dosage form itself has good water absorption capacity, and the adhesive prepared in the present application adopts a network system formed by cross-linking poly(acrylic acid-succinimide) and polyethyleneimine. Its porous network structure further improves its water absorption advantage, and is particularly suitable for the adhesion of wet wounds. It can assist in absorbing bleeding and exudate from wet wounds, which is beneficial to the treatment and healing of wet wounds.

[0064] 4. The component poly (acrylic acid-succinimide) in the medical adhesive powder provided by the present application contains succinimide groups, which can form covalent bonds with another component polyethyleneimine and amino groups on the surface of biological tissues, that is, the strength of the gel itself is enhanced, and the bonding strength to the target surface is enhanced, and a strong sealing ability can be achieved for biological tissue wounds, so that its application range can be expanded to the fields of tissue sealing, drug delivery, active substance carriers and biological scaffolds. Moreover, at a specific succinimide group content ratio and molecular weight, the prepared adhesive can have more suitable physical and chemical properties for application, as well as significantly improved bonding ability.

[0065] 5. The freeze-dried powder prepared by compounding poly(acrylic acid-succinimide) and polyethyleneimine in the present application can have a porous structure of a more stable cross-linked network system, and its network structure and mechanical properties are not affected after freeze-drying and repeated water absorption freeze-drying treatment. In addition, the adhesive powder prepared by poly(acrylic acid-succinimide) and polyethyleneimine at a specific mass ratio will not be too thin or too hardened after water absorption, and will not lose the adhesive ability, and can show better adhesive performance.

[0066] 6. The medical adhesive powder provided in this application also has good cell compatibility and blood compatibility, is safer to use, and has good biocompatibility.

[0067] 7. The medical adhesive powder provided in the present application has a fast gelling speed when in contact with water, has a good water absorption capacity, does not harden after absorbing water to form a gel, and has strong mechanical properties for bonding, and can be applied to various irregular surfaces, especially dynamic surfaces, and is not prone to peeling. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0069] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:

[0070] Figure 1 The present invention is a typical example of a preparation route of the medical adhesive powder.

[0071] Figure 2 1 is a hydrogen nuclear magnetic resonance spectrum of poly(acrylic acid-succinimide) used in the medical adhesive powder described in a typical embodiment of the present invention before and after polymerization.

[0072] Figure 3 1. The hydrogen nuclear magnetic resonance spectra of poly(acrylic acid-succinimide) and polyacrylic acid used in the medical adhesive powder described in a typical embodiment of the present invention after 1, 2 and 3 d of dialysis.

[0073] Figure 4 This is a graph showing the lap-shear strength results of poly(acrylic acid-succinimide) with different N-acryloyloxysuccinimide feed ratios of the medical adhesive powder described in a typical embodiment of the present invention, where the ordinate is shear strength in kPa.

[0074] Figure 5 This is a graph showing the properties of the adhesive after polyethyleneimine is replaced with different components in a typical embodiment of the present invention.

[0075] Figure 6 This is a graph showing the gel strength effects of different mixing mass ratios of the medical adhesive powder components poly(acrylic acid-succinimide) and polyethyleneimine described in a typical embodiment of the present invention.

[0076] Figure 7 This is a diagram showing the water absorption performance and gelling effect of the medical adhesive powder described in a typical embodiment of the present invention.

[0077] Figure 8 This is a scanning electron microscope result of the medical adhesive powder in a typical embodiment of the present invention. DETAILED DESCRIPTION

[0078] In order to more clearly explain the overall concept of the application, the following is described in detail by way of embodiment. In the following description, a large amount of specific details are provided so as to provide a more thorough understanding of the application. However, it is obvious to those skilled in the art that the application can be implemented without one or more of these details. In other examples, in order to avoid confusion with the application, some technical features well known in the art are not described.

[0079] The technical scheme of the present invention is further described in detail below in conjunction with several preferred embodiments and accompanying drawings. Obviously, the described embodiments are only a part of embodiments of the present invention, rather than all embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work belong to the scope of protection of the present invention. It should be noted that the experimental methods adopted in the following preparation examples and embodiments, if not otherwise specified, are conventional methods, and the reagents used in the preparation examples and embodiments, if not otherwise specified, are reagents supplied by conventional reagent manufacturers.

[0080] The experimental reagents and experimental instrument information involved in the following examples are shown in Table 1:

[0081] Table 1 Reagent and instrument information Reagents and instruments Purity / Model factory Acrylic acid (M=72.06 g / mol) Chromatographic pure Shanghai Anaiji Chemical N-Acryloyloxysuccinimide (M=169.13 g / mol) Chromatographic pure Shanghai Yuanye Biotechnology Co., Ltd. 4-Cyano-4-[[(dodecylthio)thionemethyl]thio]pentanoic acid Chromatographic pure Tianjin Zancheng Technology Co., Ltd. Azobisisobutyronitrile Chromatographic pure Shanghai MacLean Biochemical Technology Co., Ltd. N,N-Dimethylacetamide Chromatographic pure Shanghai MacLean Biochemical Technology Co., Ltd. Polyethyleneimine (molecular weight 10000~150000) Chromatographic pure Shanghai Yuanye Biotechnology Co., Ltd. Universal material testing machine Instron 3365 Instron (Shanghai) Testing Equipment Trading Co., Ltd. Scanning electron microscopy Quattro ESEM Thermo Fisher Scientific

[0082] Example 1

[0083] This embodiment provides a medical adhesive powder, and the preparation method thereof comprises the following steps:

[0084] 1. Preparation of poly(acrylic acid-succinimide), comprising the following steps:

[0085] (1) Add 4.28 g acrylic acid (0.059 mol), 0.1 g N-acryloyloxysuccinimide (0.0006 mol), 0.024 g 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and 0.0019 g azobisisobutyronitrile to 1.4 mL ultra-dry N,N-dimethylacetamide;

[0086] (2) Add magnetrons to the solution of step (1) and deoxygenate with Ar gas for 30 min;

[0087] (3) The reaction solution in step (2) was sealed and placed in an oil bath at 65°C for 15 h;

[0088] (4) After the reaction is completed, the reaction solution is poured into a dialysis bag (molecular weight cutoff 500 Da) and dialyzed for 2 days, and freeze-dried for 2 days to obtain poly(acrylic acid-succinimide) with a molar ratio of N-acryloylsuccinimide to feed of 1%.

[0089] 2. The poly(acrylic acid-succinimide) prepared in this example is mixed with another component, polyethyleneimine, and freeze-dried to obtain a medical adhesive powder. The specific steps are as follows:

[0090] (1) Preparation of gel: Dissolve 0.2 g of poly(acrylic acid-succinimide) (N-acryloyl succinimide feed ratio 1%) in ultrapure water to prepare a 10% poly(acrylic acid-succinimide) solution; dissolve 0.2 g of polyethyleneimine (molecular weight 75,000) in ultrapure water to prepare a 10% polyethyleneimine solution. Mix equal volumes of the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution, and stir thoroughly for 30 s to allow the poly(acrylic acid-succinimide) and polyethyleneimine to cross-link through hydrogen bonds and a small amount of covalent bonds to form a hydrogel;

[0091] (2) Powder preparation: After stirring the poly(acrylic acid-succinimide) and polyethyleneimine hydrogel in step (1), the mixture is immediately transferred to a -40°C refrigerator for freezing and then freeze-dried for 2 days. The freeze-dried poly(acrylic acid-succinimide) and polyethyleneimine hydrogel is ground for 5 minutes under infrared sample preparation to obtain a water-gelling medical adhesive powder.

[0092] Example 2

[0093] This embodiment provides a medical adhesive powder, and the preparation method thereof comprises the following steps:

[0094] 1. Preparation of poly(acrylic acid-succinimide), comprising the following steps:

[0095] (1) Add 8.208 g acrylic acid (0.114 mol), 1.014 g N-acryloyloxysuccinimide (0.006 mol), 0.024 g 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and 0.0029 g azobisisobutyronitrile to 37.00 mL ultra-dry N,N-dimethylacetamide;

[0096] (2) adding magnetrons to the solution of step (1) and deoxygenating with Ar gas for 45 min;

[0097] (3) The reaction solution in step (2) was sealed and placed in an oil bath at 70°C for 24 h;

[0098] (4) After the reaction is completed, the reaction solution is poured into a dialysis bag (molecular weight cutoff 1000 Da) and dialyzed for 3 days, and freeze-dried for 3 days to obtain poly(acrylic acid-succinimide) with a molar ratio of N-acryloylsuccinimide to feed of 5%.

[0099] 2. The poly(acrylic acid-succinimide) prepared in this example is mixed with another component, polyethyleneimine, and freeze-dried to obtain a medical adhesive powder. The specific steps are as follows:

[0100] (1) Preparation of gel: Dissolve 0.2 g of poly(acrylic acid-succinimide) (N-acryloyl succinimide feed ratio 5%) in ultrapure water to prepare a 10% poly(acrylic acid-succinimide) solution; dissolve 0.2 g of polyethyleneimine (molecular weight 75,000) in ultrapure water to prepare a 10% polyethyleneimine solution; mix equal volumes of the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution, and stir thoroughly for 60 s to allow the poly(acrylic acid-succinimide) and polyethyleneimine to cross-link through hydrogen bonds and a small amount of covalent bonds to form a hydrogel;

[0101] (2) Powder preparation: After stirring the poly(acrylic acid-succinimide) and polyethyleneimine hydrogel in step (1), the mixture is immediately transferred to a -40°C refrigerator for freezing and then freeze-dried for 3 days. The freeze-dried poly(acrylic acid-succinimide) and polyethyleneimine hydrogel is ground for 10 minutes under infrared sample preparation to obtain a water-gelling medical adhesive powder.

[0102] Example 3

[0103] This embodiment provides a medical adhesive powder, and the preparation method thereof comprises the following steps:

[0104] 1. Preparation of poly(acrylic acid-succinimide), comprising the following steps:

[0105] (1) Add 7.776 g acrylic acid (0.108 mol), 1.014 g N-acryloyloxysuccinimide (0.006 mol), 0.024 g 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and 0.0029 g azobisisobutyronitrile to 35.27 mL ultra-dry N,N-dimethylacetamide;

[0106] (2) adding magnetrons to the solution of step (1) and deoxygenating with Ar gas for 45 min;

[0107] (3) The reaction solution in step (2) was sealed and placed in an oil bath at 70°C for 24 h;

[0108] (4) After the reaction is completed, the reaction solution is poured into a dialysis bag (molecular weight cutoff 1000 Da) and dialyzed for 3 days, and freeze-dried for 3 days to obtain poly(acrylic acid-succinimide) with a molar ratio of N-acryloylsuccinimide to feed of 10%.

[0109] 2. The poly(acrylic acid-succinimide) prepared in this example is mixed with another component, polyethyleneimine, and freeze-dried to obtain a medical adhesive powder. The specific steps are as follows:

[0110] (1) Preparation of gel: Dissolve 0.2 g of poly(acrylic acid-succinimide) (N-acryloyl succinimide feed ratio 10%) in ultrapure water to prepare a 10% poly(acrylic acid-succinimide) solution; dissolve 0.2 g of polyethyleneimine (molecular weight 75,000) in ultrapure water to prepare a 10% polyethyleneimine solution; mix equal volumes of the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution, and stir thoroughly for 60 s to allow the poly(acrylic acid-succinimide) and polyethyleneimine to cross-link through hydrogen bonds and a small amount of covalent bonds to form a hydrogel;

[0111] (2) Powder preparation: After stirring the poly(acrylic acid-succinimide) and polyethyleneimine hydrogel in step (1), the mixture is immediately transferred to a -40°C refrigerator for freezing and then freeze-dried for 3 days. The freeze-dried poly(acrylic acid-succinimide) and polyethyleneimine hydrogel is ground for 10 minutes under infrared sample preparation to obtain a water-gelling medical adhesive powder.

[0112] Example 4

[0113] This embodiment provides a medical adhesive powder, and the preparation method thereof comprises the following steps:

[0114] 1. Preparation of poly(acrylic acid-succinimide), comprising the following steps:

[0115] (1) Add 7.344 g acrylic acid (0.102 mol), 2.030 g N-acryloyloxysuccinimide (0.012 mol), 0.024 g 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and 0.0029 g azobisisobutyronitrile to 37.60 mL ultra-dry N,N-dimethylacetamide;

[0116] (2) adding magnetrons to the solution of step (1) and deoxygenating with Ar gas for 45 min;

[0117] (3) The reaction solution in step (2) was sealed and placed in an oil bath at 70°C for 24 h;

[0118] (4) After the reaction is completed, the reaction solution is poured into a dialysis bag (molecular weight cutoff 1000 Da) and dialyzed for 3 days, and freeze-dried for 3 days to obtain poly(acrylic acid-succinimide) with a molar ratio of N-acryloylsuccinimide to feed of 15%.

[0119] 2. The poly(acrylic acid-succinimide) prepared in this example is mixed with another component, polyethyleneimine, and freeze-dried to obtain a medical adhesive powder. The specific steps are as follows:

[0120] (1) Preparation of gel: Dissolve 0.2 g of poly(acrylic acid-succinimide) (N-acryloyl succinimide feed ratio 15%) in ultrapure water to prepare a 10% poly(acrylic acid-succinimide) solution; dissolve 0.2 g of polyethyleneimine (molecular weight 75,000) in ultrapure water to prepare a 10% polyethyleneimine solution. Mix equal volumes of the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution, and stir thoroughly for 60 s to allow the poly(acrylic acid-succinimide) and polyethyleneimine to cross-link through hydrogen bonds and a small amount of covalent bonds to form a hydrogel;

[0121] (2) Powder preparation: After stirring the poly(acrylic acid-succinimide) and polyethyleneimine hydrogel in step (1), the mixture is immediately transferred to a -40°C refrigerator for freezing and then freeze-dried for 3 days. The freeze-dried poly(acrylic acid-succinimide) and polyethyleneimine hydrogel is ground for 10 minutes under infrared sample preparation to obtain a water-gelling medical adhesive powder.

[0122] Example 5

[0123] This embodiment provides a medical adhesive powder, and the preparation method thereof comprises the following steps:

[0124] 1. Preparation of poly(acrylic acid-succinimide), comprising the following steps:

[0125] (1) Add 6.912 g acrylic acid (0.096 mol), 3.044 g N-acryloyloxysuccinimide (0.018 mol), 0.024 g 4-cyano-4-[[(dodecylthio)thiomethyl]thio]pentanoic acid and 0.0029 g azobisisobutyronitrile to 39.93 mL ultra-dry N,N-dimethylacetamide;

[0126] (2) adding magnetrons to the solution of step (1) and deoxygenating with Ar gas for 45 min;

[0127] (3) The reaction solution in step (2) was sealed and placed in an oil bath at 70°C for 24 h;

[0128] (4) After the reaction is completed, the reaction solution is poured into a dialysis bag (molecular weight cutoff 1000 Da) and dialyzed for 3 days, and freeze-dried for 3 days to obtain poly(acrylic acid-succinimide) with a molar ratio of N-acryloylsuccinimide to feed of 20%.

[0129] 2. The poly(acrylic acid-succinimide) prepared in this example is mixed with another component, polyethyleneimine, and freeze-dried to obtain a medical adhesive powder. The specific steps are as follows:

[0130] (1) Preparation of gel: Dissolve 0.2 g of poly(acrylic acid-succinimide) (N-acryloyl succinimide feed ratio 20%) in ultrapure water to prepare a 10% poly(acrylic acid-succinimide) solution; dissolve 0.2 g of polyethyleneimine (molecular weight 75,000) in ultrapure water to prepare a 10% polyethyleneimine solution; mix equal volumes of the poly(acrylic acid-succinimide) solution and the polyethyleneimine solution, and stir thoroughly for 60 s to allow the poly(acrylic acid-succinimide) and polyethyleneimine to cross-link through hydrogen bonds and a small amount of covalent bonds to form a hydrogel;

[0131] (2) Powder preparation: After stirring the poly(acrylic acid-succinimide) and polyethyleneimine hydrogel in step (1), the mixture is immediately transferred to a -40°C refrigerator for freezing and then freeze-dried for 3 days. The freeze-dried poly(acrylic acid-succinimide) and polyethyleneimine hydrogel is ground for 10 minutes under infrared sample preparation to obtain a water-gelling medical adhesive powder.

[0132] Embodiment 6-9

[0133] The preparation methods of Examples 6-9 are substantially the same as those of Example 2, with the only difference being that, in the glue preparation step of Step 2, the mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine in Example 2 is 1:1, while the mass ratios of poly(acrylic acid-succinimide) to polyethyleneimine in Examples 6-9 are 3:1, 2:1, 1:2 and 1:3, respectively, and the remaining steps are the same as those of Example 2.

[0134] Example 10

[0135] The preparation methods of this embodiment are substantially the same as those of embodiment 2, except that in the preparation of poly(acrylic acid-succinimide) in step 1, N-acryloyloxysuccinimide is not added, and poly(acrylic acid-succinimide) having a molar ratio of N-acryloylsuccinimide feed of 0% is obtained, i.e., polyacrylic acid is obtained.

[0136] And the polyacrylic acid and polyethyleneimine are composite cross-linked to prepare an adhesive, that is, the remaining steps are the same as those in Example 2.

[0137] The reaction process and reaction formula involved in the above embodiments are as follows Figure 1 shown.

[0138] Test Example 1

[0139] Taking the poly(acrylic acid-succinimide) prepared in Example 2 with a 5% N-acryloylsuccinimide feed molar ratio as an example, the monomer conversion rate of the poly(acrylic acid-succinimide) in the synthesis step was evaluated.

[0140] Evaluation method: During the polymerization reaction, take 50 μL of the reaction solution before and after the reaction, add 500 μL of heavy water, mix well, and transfer to an NMR tube for NMR analysis. The results are shown in Figure 2 .

[0141] Performance characterization: Figure 2 As shown, according to the change in the number of double bond hydrogens in the reaction solution before and after polymerization, the monomer conversion rate of the polymerization reaction was calculated to be 97.4%, indicating that the polymer conversion rate obtained by the preparation method was high and almost all the monomers participated in the reaction.

[0142] Test Example 2

[0143] Taking the poly(acrylic acid-succinimide) prepared in Example 2 with a feed molar ratio of 5% of N-acryloylsuccinimide as an example, the nuclear magnetic resonance hydrogen spectrum characteristics of the prepared poly(acrylic acid-succinimide) were evaluated.

[0144] Evaluation method: Weigh 15 mg of poly(acrylic acid-succinimide) solid, dissolve it in 500 μL of heavy water, mix well, and transfer it to an NMR tube for NMR analysis. The results are shown in Figure 3 .

[0145] Performance characterization: Figure 3 As shown, the characteristic peak of N-acryloyl succinimide appears in the H NMR spectrum, indicating that the synthesis of poly(acrylic acid-succinimide) is successful. In addition, according to the peak area analysis, it can be obtained that the succinimide ester group accounts for 0.5% of the total molar number of the poly(acrylic acid-succinimide) unit. Therefore, its structural formula can be judged as:

[0146] ...... (I),

[0147] In the above structural formula (I) obtained in Example 2, n is 3800 and m is 200.

[0148] Based on this, it can be known that in the structural formula (I) of the aforementioned embodiments 1 to 5, the value of n is 100 to 4000, and the value of m is 1 to 800.

[0149] Test Example 3

[0150] This test example evaluates the effect of the molar ratio of N-acryloylsuccinimide in the prepared poly(acrylic acid-succinimide) on the adhesion of the final medical adhesive.

[0151] Evaluation method: According to the preparation method described in the above examples, poly (acrylic acid-succinimide) with a feed molar ratio of 1%, 5%, 10%, 15% and 20% of N-acryloyl succinimide was synthesized, and the poly (acrylic acid-succinimide) without N-acryloyl succinimide (i.e., the feed molar ratio was 0%) in Comparative Example 1 was used as a comparison, and the poly (acrylic acid-succinimide) was compounded with polyethylene imine to prepare adhesive powders, i.e., the adhesive powders prepared in Examples 1-5. Before the test, 1 to 1.5 times the mass of water was added to the powder, and after standing for a few seconds, the bonding performance of the prepared adhesive powder was evaluated by a lap shear test. The operation is as follows:

[0152] Two polyethylene sheets with a length of 5.5 cm, a width of 2 cm, and a thickness of 0.15 cm are overlapped with a contact area of ​​2 cm in length and 1 cm in width. The contact surfaces of the two polyethylene sheets are bonded and connected with an adhesive, and the amount of adhesive used is based on the complete coverage of the contact area. The unoverlapped part of the polyethylene sheet is fixed on the material machine fixture. A 50 N sensor is used to test at a constant tensile speed of 10 mm / min. The shear strength is determined by dividing the maximum load force by the adhesion area.

[0153] The lap shear strength is calculated using the following formula:

[0154] Shear strength = FL / (w × l)

[0155] Among them, FL is the maximum load force during the stretching process, w and l are the width and length of the overlapping surface of the polyethylene sheet, respectively.

[0156] The experimental results are shown in Table 2 and Figure 4 .

[0157] Table 2 N-Acryloylsuccinimide Feed Molar Ratio Shear strength / kPa 1% 7.06 5% 25.10 10% 11.87 15% 7.42 20% 7.24 Polyacrylic acid (0%) 6.76

[0158] Performance characterization: As shown in the data in Table 2, after the introduction of N-acryloyl succinimide into the polyacrylic acid molecule, its bonding ability is enhanced. When the molar ratio of N-acryloyl succinimide is 5%, PNP shows a maximum shear strength of 25.10 kPa, which shows a significantly improved shear strength compared to polyacrylic acid. When the N-acryloyl succinimide feed ratio is higher than 5%, the bonding strength is significantly reduced. In addition, the poly-N-acryloyl succinimide formed by the polymerization of N-acryloyl succinimide monomer itself is powder or powdery precipitate when it is not added with water or when it is added with water, and does not have bonding properties. This shows that the introduction of an appropriate amount of N-acryloyl succinimide can significantly improve the bonding ability of the adhesive system.

[0159] Test Example 4

[0160] This test example evaluates the effect of the type of amino-containing polymer in the prepared adhesive on the construction of the hydrogel.

[0161] Evaluation method: The hydrogel was prepared according to the preparation method described in Example 2, except that polyethyleneimine was replaced with ε-polylysine and carboxymethyl chitosan, and the prepared PAA-NHS and ε-polylysine were mixed in equal volumes to observe the gel formation. The results are shown in Figure 5 .

[0162] Performance characterization: Figure 5 As shown in the figure, the prepared PAA-NHS and ε-polylysine do not form a hydrogel and no precipitate is formed after mixing. After the prepared PAA-NHS is mixed with carboxymethyl chitosan, a precipitate is precipitated in the solution, but the precipitate is a loose flocculent precipitate and cannot form a hydrogel. It can be seen that compared with other conventional preparations that can be used to prepare hydrogels, polyethyleneimine is more suitable for compounding with the prepared poly (acrylic acid-succinimide) to form a hydrogel adhesive with a network system.

[0163] Test Example 5

[0164] This test example evaluates the effect of the mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine in the prepared adhesive on the gel strength of the hydrogel.

[0165] Evaluation method: The adhesives prepared in Examples 6-9 and Example 2, i.e., adhesives with a mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine of 3:1, 2:1, 1:1, 1:2 and 1:3, respectively, were subjected to a finger press-stretch process to visually test the mechanical properties of the same mass of adhesive hydrogels when they were in a hydrogel state. The experimental results are shown in Figure 6 .

[0166] Performance characterization: Figure 6 As shown in the figure, when the mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine is 3:1, the adhesive hydrogel strength is the highest, and the hydrogel exhibits properties similar to hard solids, with almost no adhesive properties. As the mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine decreases, the adhesive gel strength gradually weakens, gradually changing from a hard solid to a gel, until the mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine is 1:3, the adhesive behaves like a liquid and cannot gel at all. This shows that the appropriate mass ratio of poly(acrylic acid-succinimide) to polyethyleneimine can obtain an adhesive gel strength suitable for medical use.

[0167] Test Example 6

[0168] The water absorption properties of the prepared adhesive powders were evaluated.

[0169] Evaluation method: PNP powder was prepared according to the preparation method described in Example 2. A 1% mass fraction of Rhodamine B aqueous solution was added dropwise to the surface of the PNP powder to observe the absorption of the solution by the PNP powder. After the PNP powder absorbed the solution, the PNP / solution mixture was stirred to observe the gel formation. The experimental results are shown in Figure 7 .

[0170] Performance characterization: Figure 7 As shown, the prepared adhesive powder can quickly absorb the added Rhodamine B solution. After the adhesive powder absorbs the liquid, the mixture is immediately stirred, and the results show that the adhesive immediately forms a hydrogel after absorbing the solution. This result shows that the prepared adhesive powder has excellent water absorption and rapid gelation properties.

[0171] Test Example 7

[0172] The surface morphology of the prepared adhesive gel and powder was observed.

[0173] Evaluation method: According to the preparation method described in Example 2, freeze-dried samples of adhesive gel, PNP powder and freeze-dried samples of adhesive powder after absorbing water into gel were prepared. The prepared samples were pasted on the conductive glue of the scanning electron microscope sample stage, sprayed with gold, and transferred to the scanning electron microscope studio to observe the surface morphology of the samples. The results are shown in Figure 8 .

[0174] Performance characterization: Figure 8 As shown in the figure, the prepared adhesive powder shows a dense and non-voided surface layer under the microscopic view, and a porous structure below the surface layer. The pores are widely distributed and mostly unconnected, and the particle size is about 100 μm. There is no significant difference in the surface morphology between the freeze-dried sample of the adhesive gel and the second freeze-dried sample of the adhesive powder after absorbing water, and both show a porous morphology. This shows that the water absorption and gelation process has no obvious effect on the structure of the adhesive gel.

[0175] The above is only an embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.

Claims

1. A medical adhesive powder, characterized in that: The adhesive powder comprises a network system formed by cross-linking poly(acrylic acid-succinimide) and polyethyleneimine, and the mass ratio of the poly(acrylic acid-succinimide) to the polyethyleneimine is (0.5-5):(0.5-5).

2. The medical adhesive powder according to claim 1, characterized in that The mass ratio of the poly(acrylic acid-succinimide) to polyethyleneimine is (3-1):(1-2), preferably (2-1):(1-2).

3. The medical adhesive powder according to claim 1, characterized in that The poly(acrylic acid-succinimide) has a structure as shown in formula (I): ......(I), In formula (I), n is 100-4000, and m is 1-800.

4. The medical adhesive powder according to claim 1, characterized in that: The molecular weight of the polyethyleneimine is 10,000-150,000.

5. The medical adhesive powder according to claim 1, characterized in that The particle size of the medical adhesive powder is 10-1000 μm.

6. The method for preparing the medical adhesive powder according to any one of claims 1 to 5, characterized in that: include: Step 1, respectively preparing a poly(acrylic acid-succinimide) solution and a polyethyleneimine solution, mixing them according to a mass ratio and stirring them, so that the poly(acrylic acid-succinimide) and the polyethyleneimine are cross-linked through hydrogen bonds and covalent bonds to form a hydrogel; Step 2: freeze-drying the hydrogel to make it into powder, thereby obtaining the medical adhesive powder.

7. The method according to claim 6, characterized in that In the step 1, the concentration of the poly(acrylic acid-succinimide) solution is 5% to 50%, and the concentration of the polyethyleneimine solution is 5% to 50%; And / or, the mixing and stirring in step 1 is stirring at room temperature for 30 to 120 seconds, and then standing at room temperature for 0 to 3 minutes; And / or, the freeze-drying conditions in step 2 are: freeze-drying at -40°C for 2-5 days.

8. The method according to claim 6, characterized in that The poly(acrylic acid-succinimide) is prepared by polymerization of acrylic acid and N-acryloyloxysuccinimide, and the reaction molar ratio is (100-4000): (1-800).

9. The method according to claim 8, characterized in that The polymerization reaction conditions are: reacting at 65°C to 75°C for 15 to 30 hours in a closed environment without oxygen; And / or, an initiator and a chain transfer agent are further added to the polymerization reaction; And / or, after the polymerization reaction is completed, dialysis and freeze-drying are performed.

10. Use of the medical adhesive powder according to any one of claims 1 to 5, or the medical adhesive powder prepared by any one of claims 6 to 9 in preparing a wound auxiliary treatment product; Preferably, the trauma auxiliary treatment products include protective products for hemostasis and wounds, tissue sealing products, drug delivery products and / or biological scaffolds; Preferably, the medical adhesive powder is suitable for moist wounds and / or dynamic wounds.

Citation Information

Cited By

  • Polyethyleneimine / polyacrylic acid-based hydrogel for wound repair and preparation method of polyethyleneimine / polyacrylic acid-based hydrogel

    CN119733081A

  • Large-size MXene-based water-resistant stable adhesive and preparation method thereof

    CN122563540A