Antiskid wear-resistant sole material and preparation method thereof

By using phenyltrimethoxysilane and other materials in the sole material to react to form an intermediate, and combining it with modified fillers and SBS masterbatch, through ultraviolet irradiation and hot extrusion processes, the problem of poor anti-slip and wear resistance of the sole material is solved. problem, achieving higher wear resistance and slip resistance.

CN118852831APending Publication Date: 2024-10-29GUANGDONG YUESHENG NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202410930817.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

At present, the anti-slip and wear-resistant effect of sole materials is poor, especially on the ground with chemical reagents such as water and oil, which poses a high risk of safety.

Method used

A method for preparing anti-slip and wear-resistant shoe sole materials is adopted. The intermediate is formed through the reaction of phenyltrimethoxysilane, isopropyl alcohol, sodium hydroxide and other materials, and is combined with modified fillers, SBS masterbatch, etc., and is irradiated by ultraviolet light. And the hot extrusion process is used to prepare the sole material, which increases the mechanical properties and anti-slip properties of the material.

Benefits of technology

It improves the wear resistance and anti-slip properties of the sole material, enhances the cross-linking degree of SBS molecules and the coordination degree of modified fillers, forms a rigid percolation network, and improves the anti-slip performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004939598000000111
    Figure BDA0004939598000000111
  • Figure BDA0004939598000000121
    Figure BDA0004939598000000121
Patent Text Reader

Abstract

The preparation method comprises the following steps: blending a functional filler, an additive, SBS master batch, benzoin dimethyl ether and tetrahydrofuran, grafting double bonds on a side chain of an SBS molecule and double bonds on the surface of the functional filler with sulfydryl on the additive under the irradiation of ultraviolet light, and carrying out melt extrusion to obtain the anti-skid wear-resistant sole material. The sole material contains a polyhedral oligomeric silsesquioxane structure, so that the mechanical property of the material can be improved, meanwhile, the crosslinking degree of SBS molecules is improved, the matching degree of the SBS molecules and the modified filler is enhanced, a rigid percolation network is formed, and then the wear-resistant effect of the material is improved; and the modified filler is loaded with nano silicon dioxide and nano titanium dioxide on the surface, so that the roughness of the modified filler is increased, and the skid resistance of the material is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of anti-skid and wear-resistant rubber preparation, and in particular to an anti-skid and wear-resistant sole material and a preparation method thereof. Background Art

[0002] Rubber material is a kind of material with sufficient elasticity, high strength, wide raw material source and low price. SBS is a kind of thermoplastic rubber, and the amount used in the production of soles accounts for more than 50% of the total output. In recent years, with the continuous development of the shoemaking industry, shoes are also developing in the direction of diversification, functionality and economy, and the requirements for the performance of the sole material are also constantly improving. Directly using rubber materials as sole materials often has poor wear resistance and serious wear after a period of use. In addition, its anti-slip performance is poor, especially on the ground with water, oil and other chemical reagents, which makes the safety hazard very high in special environments. Summary of the invention

[0003] The purpose of the present invention is to provide a non-slip and wear-resistant sole material and a preparation method thereof, which solves the problem that the current sole material has poor non-slip and wear-resistant effect.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a non-slip and wear-resistant sole material comprises the following steps:

[0006] Step A1: Phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water are mixed evenly, nitrogen protection is introduced, and the reaction is carried out for 3-5 hours at a speed of 120-150 r / min and a temperature of 85-90° C., and then the temperature is reduced to 20-25° C. and the reaction is carried out for 10-15 hours to obtain intermediate 1. Intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran are mixed evenly, and the reaction is carried out for 3-5 hours at a speed of 150-200 r / min and a temperature of 0° C., and then the temperature is increased to 20-25° C. and the reaction is carried out for 18-20 hours to obtain intermediate 2;

[0007] Step A2: Intermediate 2, chloroplatinic acid, allyl alcohol glycidyl ether and toluene are uniformly mixed, nitrogen is introduced for protection, and the reaction is carried out for 10-15 hours at a speed of 120-150 r / min and a temperature of 80-85° C. to obtain intermediate 3; intermediate 3, diethanolamine and DMF are mixed, and the reaction is carried out for 4-6 hours at a speed of 120-150 r / min, a temperature of 60-70° C. and a pH value of 10-11, and the pH is adjusted to neutral, 3-mercaptoacetic acid and concentrated sulfuric acid are added, and the reaction is carried out for 6-8 hours at a temperature of 85-90° C. to obtain an additive;

[0008] Step A3: Disperse the modified filler in ethanol, stir and add KH570 and deionized water at a speed of 120-150 r / min and a temperature of 40-50° C., and react for 1-1.5 hours to obtain a functionalized filler, mix the functionalized filler, additives, SBS masterbatch, dimethyl benzoin and tetrahydrofuran evenly, irradiate under 360 nm ultraviolet light for 10-15 minutes, distill off the tetrahydrofuran, extrude the substrate at a temperature of 180-190° C. and cool to obtain a non-slip and wear-resistant sole material.

[0009] Furthermore, the amount ratio of phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water in step A1 is 120 mmol: 120 mL: 80 mmol: 3 mL, and the amount ratio of intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran is 12 g: 4.5 mL: 3.5 g: 20 mL.

[0010] Furthermore, the molar ratio of intermediate 2 and allyl alcohol glycidyl ether described in step A2 is 1:2, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol glycidyl ether, the molar ratio of intermediate 3, diethanolamine and 3-mercaptoacetic acid is 1:2:6, and the amount of concentrated sulfuric acid used is 1.5% of the mass of 3-mercaptoacetic acid.

[0011] Furthermore, the amount of KH570 in step A3 is 3% of the mass of the modified filler, and the mass ratio of the functional filler, the additive, the SBS masterbatch and the benzoin dimethyl ether is 10-15:20-25:100-120:0.15-0.3.

[0012] Further, the modified filler is prepared by the following steps:

[0013] Step B1: mixing carbon nanotubes, sulfuric acid solution and nitric acid solution, reacting for 3-5 hours at a speed of 120-150 r / min and a temperature of 90-100° C. to obtain carboxylated carbon nanotubes; uniformly mixing carboxylated carbon nanotubes, 3-dimethylamino-1-propanol, p-toluenesulfonic acid and toluene, reacting for 4-6 hours at a speed of 120-150 r / min and a temperature of 110-120° C. to obtain pretreated carbon nanotubes;

[0014] Step B2: Disperse the pretreated carbon tubes in ethyl acetate, add ethyl bromide, stir and react for 10-15 hours at a speed of 200-300 r / min and a temperature of 50-60° C. to obtain modified carbon tubes, and mix (N,N-dimethyl-3-aminopropyl)trimethoxysilane, ethyl bromide and toluene evenly, stir and react for 8-10 hours at a speed of 200-300 r / min and a temperature of 70-80° C. to obtain a modifier;

[0015] Step B3: The modified carbon tube, montmorillonite and tetrahydrofuran are mixed, stirred for 3-5 hours at a speed of 300-500r / min and a temperature of 70-75°C, and then a modifier is added, and stirring is continued for 4-6 hours. The temperature is lowered to 60-65°C, methyltriethoxysilane, dimethylethoxysilane and deionized water are added, and the reaction is continued for 2-3 hours. Tetrabutyl titanate is added and the reaction is continued for 3-5 hours to obtain a precursor, and the precursor is added to a muffle furnace, and calcined for 3-5 hours at a temperature of 600-700°C under nitrogen protection to obtain a modified filler.

[0016] Furthermore, the amount ratio of the carbon nanotubes, sulfuric acid solution and nitric acid solution described in step B1 is 0.3g:3mL:1mL, the mass fraction of the sulfuric acid solution is 95%, the mass fraction of the nitric acid solution is 65%, the molar ratio of the carboxyl groups on the carboxylated carbon nanotubes and 3-dimethylamino-1-propanol is 1:1, and the amount of p-toluenesulfonic acid is 1% by mass of 3-dimethylamino-1-propanol.

[0017] Furthermore, the amount ratio of the pretreated carbon tubes and ethyl bromide in step B2 is 1 g:8 mL, and the molar ratio of (N,N-dimethyl-3-aminopropyl)trimethoxysilane and ethyl bromide is 1:1.

[0018] Furthermore, the amount ratio of the modified carbon tube, montmorillonite, modifier, methyltriethoxysilane, dimethylethoxysilane, deionized water and tetrabutyl titanate described in step B3 is 1g:3g:2g:8mL:5mL:30mL:1mL.

[0019] The beneficial effects of the present invention are as follows: the anti-skid and wear-resistant sole prepared by the present invention is prepared by hydrolyzing and condensing phenyltrimethoxysilane as a raw material to form sodium octaphenylcyclotetrasiloxane tetrasilanolate to prepare intermediate 1, reacting intermediate 1 with methyldichlorosilane so that the chlorine atom site on methyldichlorosilane reacts with sodium silanolate on intermediate 1 to prepare intermediate 2, and reacting intermediate 2 with allyl alcohol glycidyl ether under the action of chloroplatinic acid so that the S on intermediate 2 reacts with sodium silanolate. iH reacts with double bonds on allyl alcohol glycidyl ether to obtain intermediate 3, intermediate 3 reacts with diethanolamine so that the epoxy group on intermediate 3 reacts with the secondary amine on diethanolamine, 3-thioglycolic acid is added to modify the 3-thioglycolic acid under the action of concentrated sulfuric acid so that the carboxyl and hydroxyl groups on the 3-thioglycolic acid are esterified to obtain an additive, the modified filler is treated with KH570 so that double bonds are grafted on the surface to obtain a functional filler, the functional filler, the additive, SBS masterbatch, benzoin dimethyl ether and tetrahydrofuran are blended, and under ultraviolet light irradiation, the double bonds on the side chains of the SBS molecules and the double bonds on the surface of the functional filler can be grafted with the thiol groups on the additive, and then melt-extruded to obtain a non-slip and wear-resistant sole material.

[0020] The modified filler is treated with a sulfuric acid solution and a nitric acid solution to graft carboxyl groups on the surface of carbon nanotubes, and obtain carboxylated carbon nanotubes. The carboxylated carbon nanotubes are subjected to an esterification reaction with 3-dimethylamino-1-propanol, so that the carboxyl groups on the carboxylated carbon nanotubes react with the hydroxyl groups on the 3-dimethylamino-1-propanol to obtain pretreated carbon nanotubes. The pretreated carbon nanotubes are treated with ethyl bromide, so that the dimethylamino groups on the pretreated carbon nanotubes react with the bromine atom sites of ethyl bromide to obtain modified carbon nanotubes. (N, The modified carbon tube, montmorillonite and the modifier are mixed, and the modified carbon tube and the montmorillonite are composited by ion exchange, and siloxane groups are grafted on the surface. Methyltriethoxysilane, dimethylethoxysilane and tetrabutyl titanate are then added for hydrolysis and condensation to form titanium-containing organic silicon on the surface, and finally calcined to form nano silicon dioxide and nano titanium dioxide loading on the surface to obtain a modified filler.

[0021] The sole material contains a cage-type silsesquioxane structure that can increase the mechanical properties of the material, while improving the cross-linking degree of the SBS molecules, enhancing the compatibility of the SBS molecules with the modified fillers to form a rigid percolation network, thereby improving the wear resistance of the material. The modified fillers increase their own roughness by loading nano-silicon dioxide and nano-titanium dioxide on the surface, thereby increasing the anti-slip properties of the material. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A method for preparing a non-slip and wear-resistant sole material comprises the following steps:

[0025] Step A1: Phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out at a speed of 120 r / min and a temperature of 85° C. for 3 hours, then the temperature is lowered to 20° C. and the reaction is carried out for 10 hours to obtain intermediate 1; intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran are mixed evenly, and the reaction is carried out at a speed of 150 r / min and a temperature of 0° C. for 3 hours, then the temperature is raised to 20° C. and the reaction is carried out for 18 hours to obtain intermediate 2;

[0026] Step A2: Intermediate 2, chloroplatinic acid, allyl alcohol glycidyl ether and toluene are mixed uniformly, nitrogen is introduced for protection, and the mixture is reacted for 10 hours at a speed of 120 r / min and a temperature of 80° C. to obtain intermediate 3; intermediate 3, diethanolamine and DMF are mixed, and the mixture is reacted for 4 hours at a speed of 120 r / min, a temperature of 60° C. and a pH value of 10, and the pH is adjusted to be neutral, 3-mercaptoacetic acid and concentrated sulfuric acid are added, and the mixture is reacted for 6 hours at a temperature of 85° C. to obtain an additive;

[0027] Step A3: Disperse the modified filler in ethanol, stir and add KH570 and deionized water at a speed of 120 r / min and a temperature of 40°C, and react for 1 hour to obtain a functionalized filler. Evenly mix the functionalized filler, additives, SBS masterbatch, dimethyl benzoin and tetrahydrofuran, irradiate under 360nm ultraviolet light for 10 minutes, distill off the tetrahydrofuran, extrude the substrate at a temperature of 180°C and cool it to obtain a non-slip and wear-resistant sole material.

[0028] The amount ratio of phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water described in step A1 is 120mmo l:120mL:80mmo l:3mL, and the amount ratio of intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran is 12g:4.5mL:3.5g:20mL.

[0029] The molar ratio of intermediate 2 and allyl alcohol glycidyl ether described in step A2 is 1:2, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol glycidyl ether, the molar ratio of intermediate 3, diethanolamine and 3-mercaptoacetic acid is 1:2:6, and the amount of concentrated sulfuric acid used is 1.5% of the mass of 3-mercaptoacetic acid.

[0030] The amount of KH570 described in step A3 is 3% of the mass of the modified filler, the mass ratio of the functional filler, the additive, the SBS masterbatch and dimethyl benzoate is 10:20:100:0.15, and the model of the SBS masterbatch is F875.

[0031] The modified filler is prepared by the following steps:

[0032] Step B1: mixing carbon nanotubes, sulfuric acid solution and nitric acid solution, reacting for 3 hours at a speed of 120 r / min and a temperature of 90° C. to obtain carboxylated carbon nanotubes; uniformly mixing carboxylated carbon nanotubes, 3-dimethylamino-1-propanol, p-toluenesulfonic acid and toluene, reacting for 4 hours at a speed of 120 r / min and a temperature of 110° C. to obtain pretreated carbon nanotubes;

[0033] Step B2: Disperse the pretreated carbon tubes in ethyl acetate, add ethyl bromide, stir and react for 10 hours at a speed of 200 r / min and a temperature of 50°C to obtain modified carbon tubes, mix (N,N-dimethyl-3-aminopropyl)trimethoxysilane, ethyl bromide and toluene evenly, stir and react for 8 hours at a speed of 200 r / min and a temperature of 70°C to obtain a modifier;

[0034] Step B3: The modified carbon tube, montmorillonite and tetrahydrofuran are mixed, stirred at a speed of 300 r / min and a temperature of 70°C for 3 hours, and then a modifier is added, and stirring is continued for 4 hours. The temperature is lowered to 60°C, and methyltriethoxysilane, dimethylethoxysilane and deionized water are added, and the reaction is continued for 2 hours. Tetrabutyl titanate is added, and the reaction is continued for 3 hours to obtain a precursor. The precursor is added into a muffle furnace, and calcined for 3 hours at a temperature of 600°C under nitrogen protection to obtain a modified filler.

[0035] The amount ratio of the carbon nanotubes, sulfuric acid solution and nitric acid solution described in step B1 is 0.3g:3mL:1mL, the mass fraction of the sulfuric acid solution is 95%, the mass fraction of the nitric acid solution is 65%, the molar ratio of the carboxyl groups on the carboxylated carbon nanotubes and 3-dimethylamino-1-propanol is 1:1, and the amount of p-toluenesulfonic acid is 1% by mass of 3-dimethylamino-1-propanol.

[0036] The amount ratio of the pretreated carbon tubes and ethyl bromide in step B2 is 1 g:8 mL, and the molar ratio of (N,N-dimethyl-3-aminopropyl)trimethoxysilane and ethyl bromide is 1:1.

[0037] The amount ratio of the modified carbon tube, montmorillonite, modifier, methyltriethoxysilane, dimethylethoxysilane, deionized water and tetrabutyl titanate described in step B3 is 1g:3g:2g:8mL:5mL:30mL:1mL.

[0038] Example 2

[0039] A method for preparing a non-slip and wear-resistant sole material comprises the following steps:

[0040] Step A1: Phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water were mixed evenly, nitrogen was introduced for protection, and the reaction was carried out at a speed of 120 r / min and a temperature of 88° C. for 4 hours, then the temperature was lowered to 23° C. and the reaction was carried out for 13 hours to obtain intermediate 1; intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran were mixed evenly, and the reaction was carried out at a speed of 150 r / min and a temperature of 0° C. for 4 hours, then the temperature was raised to 23° C. and the reaction was carried out for 19 hours to obtain intermediate 2;

[0041] Step A2: Intermediate 2, chloroplatinic acid, allyl alcohol glycidyl ether and toluene are mixed uniformly, nitrogen is introduced for protection, and the mixture is reacted for 13 hours at a speed of 120 r / min and a temperature of 83° C. to obtain intermediate 3; intermediate 3, diethanolamine and DMF are mixed, and the mixture is reacted for 5 hours at a speed of 150 r / min, a temperature of 65° C. and a pH value of 10, and the pH is adjusted to be neutral, 3-mercaptoacetic acid and concentrated sulfuric acid are added, and the mixture is reacted for 7 hours at a temperature of 85° C. to obtain an additive;

[0042] Step A3: Disperse the modified filler in ethanol, stir and add KH570 and deionized water at a speed of 120 r / min and a temperature of 45°C, and react for 1.3 hours to obtain a functionalized filler. Evenly mix the functionalized filler, additives, SBS masterbatch, dimethyl benzoin and tetrahydrofuran, irradiate under 360nm ultraviolet light for 13 minutes, distill off the tetrahydrofuran, extrude the substrate at a temperature of 185°C and cool it to obtain a non-slip and wear-resistant sole material.

[0043] The amount ratio of phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water described in step A1 is 120mmo l:120mL:80mmo l:3mL, and the amount ratio of intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran is 12g:4.5mL:3.5g:20mL.

[0044] The molar ratio of intermediate 2 and allyl alcohol glycidyl ether described in step A2 is 1:2, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol glycidyl ether, the molar ratio of intermediate 3, diethanolamine and 3-mercaptoacetic acid is 1:2:6, and the amount of concentrated sulfuric acid used is 1.5% of the mass of 3-mercaptoacetic acid.

[0045] The amount of KH570 described in step A3 is 3% of the mass of the modified filler, the mass ratio of the functional filler, the additive, the SBS masterbatch and dimethyl benzoate is 13:23:110:0.2, and the SBS masterbatch model is F875.

[0046] The modified filler is prepared by the following steps:

[0047] Step B1: mixing carbon nanotubes, sulfuric acid solution and nitric acid solution, reacting for 4 hours at a speed of 120 r / min and a temperature of 95° C. to obtain carboxylated carbon nanotubes; uniformly mixing carboxylated carbon nanotubes, 3-dimethylamino-1-propanol, p-toluenesulfonic acid and toluene, reacting for 5 hours at a speed of 120 r / min and a temperature of 115° C. to obtain pretreated carbon nanotubes;

[0048] Step B2: Disperse the pretreated carbon tubes in ethyl acetate, add ethyl bromide, stir and react for 13 hours at a speed of 200 r / min and a temperature of 55°C to obtain modified carbon tubes, mix (N,N-dimethyl-3-aminopropyl)trimethoxysilane, ethyl bromide and toluene evenly, stir and react for 9 hours at a speed of 300 r / min and a temperature of 75°C to obtain a modifier;

[0049] Step B3: The modified carbon tubes, montmorillonite and tetrahydrofuran were mixed, stirred at a speed of 300 r / min and a temperature of 73°C for 4 hours, then a modifier was added, and stirring was continued for 5 hours. The temperature was lowered to 63°C, methyltriethoxysilane, dimethylethoxysilane and deionized water were added, and the reaction was continued for 2.5 hours. Then, tetrabutyl titanate was added and the reaction was continued for 4 hours to obtain a precursor. The precursor was added into a muffle furnace, and calcined at a temperature of 650°C under nitrogen protection for 4 hours to obtain a modified filler.

[0050] The amount ratio of the carbon nanotubes, sulfuric acid solution and nitric acid solution described in step B1 is 0.3g:3mL:1mL, the mass fraction of the sulfuric acid solution is 95%, the mass fraction of the nitric acid solution is 65%, the molar ratio of the carboxyl groups on the carboxylated carbon nanotubes and 3-dimethylamino-1-propanol is 1:1, and the amount of p-toluenesulfonic acid is 1% by mass of 3-dimethylamino-1-propanol.

[0051] The amount ratio of the pretreated carbon tubes and ethyl bromide in step B2 is 1 g:8 mL, and the molar ratio of (N,N-dimethyl-3-aminopropyl)trimethoxysilane and ethyl bromide is 1:1.

[0052] The amount ratio of the modified carbon tube, montmorillonite, modifier, methyltriethoxysilane, dimethylethoxysilane, deionized water and tetrabutyl titanate described in step B3 is 1g:3g:2g:8mL:5mL:30mL:1mL.

[0053] Example 3

[0054] A method for preparing a non-slip and wear-resistant sole material specifically comprises the following steps:

[0055] Step A1: Phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out at a speed of 150 r / min and a temperature of 90° C. for 5 hours, then the temperature is lowered to 25° C. and the reaction is carried out for 15 hours to obtain intermediate 1; intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran are mixed evenly, and the reaction is carried out at a speed of 200 r / min and a temperature of 0° C. for 5 hours, then the temperature is raised to 25° C. and the reaction is carried out for 20 hours to obtain intermediate 2;

[0056] Step A2: Intermediate 2, chloroplatinic acid, allyl alcohol glycidyl ether and toluene are uniformly mixed, nitrogen is introduced for protection, and the mixture is reacted for 15 hours at a speed of 150 r / min and a temperature of 85° C. to obtain intermediate 3; intermediate 3, diethanolamine and DMF are mixed, and the mixture is reacted for 6 hours at a speed of 150 r / min, a temperature of 70° C. and a pH value of 11, and the pH is adjusted to be neutral, 3-mercaptoacetic acid and concentrated sulfuric acid are added, and the mixture is reacted for 8 hours at a temperature of 90° C. to obtain an additive;

[0057] Step A3: Disperse the modified filler in ethanol, stir and add KH570 and deionized water at a speed of 150 r / min and a temperature of 50°C, and react for 1.5 hours to obtain a functionalized filler. Evenly mix the functionalized filler, additives, SBS masterbatch, dimethyl benzoin and tetrahydrofuran, irradiate under 360nm ultraviolet light for 15 minutes, distill off the tetrahydrofuran, extrude the substrate at a temperature of 190°C and cool it to obtain a non-slip and wear-resistant sole material.

[0058] The amount ratio of phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water described in step A1 is 120mmo l:120mL:80mmo l:3mL, and the amount ratio of intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran is 12g:4.5mL:3.5g:20mL.

[0059] The molar ratio of intermediate 2 and allyl alcohol glycidyl ether described in step A2 is 1:2, the amount of chloroplatinic acid used is 1‰ of the mass of allyl alcohol glycidyl ether, the molar ratio of intermediate 3, diethanolamine and 3-mercaptoacetic acid is 1:2:6, and the amount of concentrated sulfuric acid used is 1.5% of the mass of 3-mercaptoacetic acid.

[0060] The amount of KH570 described in step A3 is 3% of the mass of the modified filler, the mass ratio of the functional filler, the additive, the SBS masterbatch and dimethyl benzoate is 15:25:120:0.3, and the SBS masterbatch model is F875.

[0061] The modified filler is prepared by the following steps:

[0062] Step B1: mixing carbon nanotubes, sulfuric acid solution and nitric acid solution, reacting for 5 hours at a speed of 150 r / min and a temperature of 100° C. to obtain carboxylated carbon nanotubes; uniformly mixing carboxylated carbon nanotubes, 3-dimethylamino-1-propanol, p-toluenesulfonic acid and toluene, reacting for 6 hours at a speed of 150 r / min and a temperature of 120° C. to obtain pretreated carbon nanotubes;

[0063] Step B2: Disperse the pretreated carbon tubes in ethyl acetate, add ethyl bromide, stir and react for 15 hours at a speed of 300 r / min and a temperature of 60°C to obtain modified carbon tubes, mix (N,N-dimethyl-3-aminopropyl)trimethoxysilane, ethyl bromide and toluene evenly, stir and react for 10 hours at a speed of 300 r / min and a temperature of 80°C to obtain a modifier;

[0064] Step B3: The modified carbon tube, montmorillonite and tetrahydrofuran are mixed, stirred at a speed of 500 r / min and a temperature of 75°C for 5 hours, and then a modifier is added, and stirring is continued for 6 hours. The temperature is lowered to 65°C, and methyltriethoxysilane, dimethylethoxysilane and deionized water are added. After reacting for 3 hours, tetrabutyl titanate is added and the reaction is continued for 5 hours to obtain a precursor. The precursor is added into a muffle furnace and calcined for 5 hours at a temperature of 700°C under nitrogen protection to obtain a modified filler.

[0065] The amount ratio of the carbon nanotubes, sulfuric acid solution and nitric acid solution described in step B1 is 0.3g:3mL:1mL, the mass fraction of the sulfuric acid solution is 95%, the mass fraction of the nitric acid solution is 65%, the molar ratio of the carboxyl groups on the carboxylated carbon nanotubes and 3-dimethylamino-1-propanol is 1:1, and the amount of p-toluenesulfonic acid is 1% by mass of 3-dimethylamino-1-propanol.

[0066] The amount ratio of the pretreated carbon tubes and ethyl bromide in step B2 is 1 g:8 mL, and the molar ratio of (N,N-dimethyl-3-aminopropyl)trimethoxysilane and ethyl bromide is 1:1.

[0067] The amount ratio of the modified carbon tube, montmorillonite, modifier, methyltriethoxysilane, dimethylethoxysilane, deionized water and tetrabutyl titanate described in step B3 is 1g:3g:2g:8mL:5mL:30mL:1mL.

[0068] Comparative Example 1

[0069] Compared with Example 1, no additives were added in this comparative example, and the remaining steps were the same.

[0070] Comparative Example 2

[0071] Compared with Example 1, this comparative example uses pentaerythritol tetraacrylate instead of the additive, and the other steps are the same.

[0072] Comparative Example 3

[0073] Compared with Example 1, in this comparative example, the modified carbon tube, montmorillonite and tetrahydrofuran are mixed, stirred for 3 hours at a speed of 300 r / min and a temperature of 70° C., and the obtained product replaces the modified filler, and the other steps are the same.

[0074] Comparative Example 4

[0075] Compared with Example 1, this comparative example uses carbon nanotubes instead of the modified filler, and the remaining steps are the same.

[0076] The loss and friction coefficient of Examples 1-3 and Comparative Examples 1-4 were tested according to the standard of GB / T9867-2008, and the SRA friction coefficient and SRB friction coefficient were tested according to the standard of ISO13287-2012. The test results are shown in the following table.

[0077]

[0078]

[0079] It can be seen from the above table that the present invention has a very good wear-resistant and anti-slip effect.

[0080] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a non-slip and wear-resistant sole material, characterized in that: The specific steps include: Step A1: Phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out to obtain intermediate 1; intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran are mixed for reaction to obtain intermediate 2; Step A2: intermediate 2, chloroplatinic acid, allyl alcohol glycidyl ether and toluene are mixed to react to obtain intermediate 3, intermediate 3, diethanolamine and DMF are mixed to react, the pH is adjusted to neutral, 3-mercaptoacetic acid and concentrated sulfuric acid are added to react to obtain an additive; Step A3: Disperse the modified filler in ethanol, stir and add KH570 and deionized water to react to obtain a functionalized filler, mix the functionalized filler, additives, SBS masterbatch, benzoin dimethyl ether and tetrahydrofuran evenly, irradiate with ultraviolet light, distill off the tetrahydrofuran, extrude the substrate and cool it to obtain a non-slip and wear-resistant sole material.

2. The method for preparing a non-slip and wear-resistant sole material according to claim 1, characterized in that: The amount ratio of phenyltrimethoxysilane, isopropanol, sodium hydroxide and deionized water described in step A1 is 120mmol:120mL:80mmol:3mL, and the amount ratio of intermediate 1, triethylamine, methyldichlorosilane and tetrahydrofuran is 12g:4.5mL:3.5g:20mL.

3. The method for preparing a non-slip and wear-resistant sole material according to claim 1, characterized in that: The molar ratio of intermediate 2 and allyl alcohol glycidyl ether described in step A2 is 1:2, and the molar ratio of intermediate 3, diethanolamine and 3-mercaptoacetic acid is 1:2:

6.

4. The method for preparing a non-slip and wear-resistant sole material according to claim 1, characterized in that: The amount of KH570 used in step A3 is 3% of the mass of the modified filler, and the mass ratio of the functional filler, additive, SBS masterbatch and benzoin dimethyl ether is 10-15:20-25:100-120:0.15-0.

3.

5. The method for preparing a non-slip and wear-resistant sole material according to claim 1, characterized in that: The modified filler is prepared by the following steps: Step B1: mixing carbon nanotubes, sulfuric acid solution and nitric acid solution to react to obtain carboxylated carbon nanotubes, and mixing carboxylated carbon nanotubes, 3-dimethylamino-1-propanol, p-toluenesulfonic acid and toluene to react to obtain pretreated carbon nanotubes; Step B2: dispersing the pretreated carbon tubes in ethyl acetate, adding ethyl bromide, stirring and reacting to obtain a modified carbon tube, and mixing (N,N-dimethyl-3-aminopropyl)trimethoxysilane, ethyl bromide and toluene, stirring and reacting to obtain a modifier; Step B3: After the modified carbon tube, montmorillonite and tetrahydrofuran are mixed and stirred, a modifier is added, stirring is continued, methyltriethoxysilane, dimethylethoxysilane and deionized water are added, and after reaction, tetrabutyl titanate is added and the reaction is continued to obtain a precursor, and the precursor is calcined to obtain a modified filler.

6. The method for preparing a non-slip and wear-resistant sole material according to claim 5, characterized in that: The amount ratio of the carbon nanotubes, sulfuric acid solution and nitric acid solution in step B1 is 0.3 g:3 mL:1 mL, and the molar ratio of the carboxyl groups on the carboxylated carbon nanotubes to 3-dimethylamino-1-propanol is 1:

1.

7. The method for preparing a non-slip and wear-resistant sole material according to claim 5, characterized in that: The amount ratio of the pretreated carbon tubes and ethyl bromide in step B2 is 1 g:8 mL, and the molar ratio of (N,N-dimethyl-3-aminopropyl)trimethoxysilane and ethyl bromide is 1:

1.

8. The method for preparing a non-slip and wear-resistant sole material according to claim 5, characterized in that: The amount ratio of the modified carbon tube, montmorillonite, modifier, methyltriethoxysilane, dimethylethoxysilane, deionized water and tetrabutyl titanate described in step B3 is 1g:3g:2g:8mL:5mL:30mL:1mL.

9. A non-slip and wear-resistant sole material, characterized by: Prepared according to any one of the preparation methods described in claims 1-8.

Citation Information

Patent Citations

  • Carbon nanotube modified thermoplastic elastomer composite material with solvent resistance and preparing method thereof

    CN105602181A

  • Antibacterial material

    WO2023029272A1

Cited By

  • Ceramic material and application thereof in fuse

    CN118993702A

  • Wear-resistant thermoplastic colloidal particle for shoe sole and preparation method of wear-resistant thermoplastic colloidal particle