Flame-retardant gel electrolyte, preparation method thereof and semi-solid lithium metal battery

Through the use of fully flame-retardant gel electrolyte, the safety hazards and short life problems of lithium metal batteries during the cycle are solved, the safety and cycle performance of the battery are improved, the battery life is extended and the cost is reduced.

CN118867366APending Publication Date: 2024-10-29ZIJIN MINING RENEWABLE ENERGY & ADVANCED MATERIALS (CHANGSHA) CO LTD

Patent Information

Application Number
CN202410803432.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing lithium metal batteries have problems such as battery safety hazards, short cycle life, and narrow service range during the cycle process. The traditional electrolyte has insufficient flame retardant components and cannot effectively improve the safety and cycle performance of the battery.

Method used

Using a fully flame-retardant gel electrolyte, including polymerized monomers, fluorine-containing flame-retardant diluents, flame-retardant solvents, inorganic salt additives and high-concentration electrolyte systems, a solid electrolyte interface rich in inorganics is formed to reduce the loss of lithium metal. Improve battery safety and cycle performance.

Benefits of technology

It has achieved improved safety and optimized cycle performance of lithium metal batteries, extended battery life, enhanced high-temperature stability and Coulombic efficiency of batteries, and reduced electrolyte costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004904020180000081
    Figure BDA0004904020180000081
  • Figure HDA0004904020190000011
    Figure HDA0004904020190000011
  • Figure HDA0004904020190000012
    Figure HDA0004904020190000012
Patent Text Reader

Abstract

The invention provides a flame-retardant gel electrolyte, a preparation method thereof and a semi-solid lithium metal battery. The flame-retardant gel electrolyte comprises the following raw materials in parts by mass: 1-3 parts of a polymeric monomer, 35-70 parts of a diluent, 5-20 parts of a lithium salt, 15-35 parts of a solvent, 0.1-0.2 part of an initiator, 0.1-10 parts of an additive and 1-3 parts of a cross-linking agent, the diluent is a fluorine-containing flame-retardant diluent, the additive is an inorganic salt additive and / or an organic small molecule additive, the solvent is a flame-retardant solvent, and the polymeric monomer is a flame-retardant polymeric monomer. The flame-retardant gel electrolyte provided by the invention is a full-flame-retardant electrolyte, so that the safety of the lithium metal battery is qualitatively improved; and the cycle performance of the battery is relatively good, the safety of the battery is ensured while the excellent cycle performance is realized, and the development of the lithium metal battery to an application end can be promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of lithium metal batteries, and in particular to a flame retardant gel electrolyte and a preparation method thereof, and a semi-solid lithium metal battery. Background Art

[0002] New lithium metal batteries that can achieve a high specific energy of more than 400Wh / kg are regarded as the only choice for the next generation of batteries, but their safety hazards, short cycle life and narrow service range still need to be solved. During the cycle of lithium metal secondary batteries, factors such as unreasonable battery capacity design and electrode-electrolyte interface failure cause non-uniform deposition of lithium, resulting in dendrites, which in turn cause battery capacity decay and may cause short circuits, leading to thermal runaway or even explosion of the battery. Semi-solid gel electrolytes and flame-retardant electrolytes often have lower reactivity and intrinsic non-flammable properties, which can effectively increase the trigger temperature of battery thermal runaway and are expected to be used to improve the safety performance of lithium metal batteries. However, most of the reported new electrolytes contain only a small amount of flame retardant components, which cannot bring a qualitative improvement to the safety of lithium metal batteries; at the same time, because the polymerized monomers, flame retardant additives and flame retardant solvents (small molecule phosphates) introduced by them are not compatible with lithium metal negative electrodes and high-voltage positive electrodes at the same time, the battery cycle performance is poor. Only by achieving excellent cycle performance and ensuring battery safety at the same time can the development of lithium metal batteries be promoted to the application end. Summary of the invention

[0003] In order to solve the above technical problems, the present invention provides a flame retardant gel electrolyte and a preparation method thereof, and a semi-solid lithium metal battery.

[0004] In the first aspect, the flame retardant gel electrolyte provided by the present invention comprises the following raw materials in parts by mass: 1 to 3 parts of polymer monomer, 40 to 70 parts of diluent, 5 to 20 parts of lithium salt, 15 to 35 parts of solvent, 0.1 to 0.2 parts of initiator, 0.1 to 10 parts of additive, and 1 to 3 parts of cross-linking agent; the diluent is a fluorine-containing flame retardant diluent, the additive is an inorganic salt additive and / or an organic small molecule additive, the solvent is a flame retardant solvent, and the polymer monomer is a flame retardant polymer monomer. The flame retardant gel electrolyte provided by the present invention is a "full flame retardant electrolyte", which brings a qualitative improvement to the safety of lithium metal batteries; and the battery cycle performance is good, achieving excellent cycle performance while ensuring the safety of the battery, which can promote the development of lithium metal batteries to the application end.

[0005] According to the present invention, in view of the fact that most of the current conventional lithium ion electrolytes and gel electrolytes are based on a flammable carbonate system, or only use a portion of non-flammable and flame-retardant components, the gel electrolyte of the present invention is a "full flame-retardant electrolyte", wherein more than 90% by mass fraction or even all components are flame-retardant or intrinsically non-flammable components (lithium salts, solvents, diluents, polymerized monomers), and its high temperature can not support combustion, and its free radical reaction at high temperature can quickly absorb heat, which is conducive to alleviating the rapid temperature rise phenomenon of the battery thermal runaway process and enhancing the battery safety performance. In addition, unlike the SEI formed by the decomposition of "lithium ion-solvent" pairs in traditional electrolytes, the electrolyte is based on a local high-concentration electrolyte system, and there are a large number of "lithium ion-anion" ion pairs, which can be preferentially decomposed on the electrode surface to form a solid electrolyte interface phase (SEI) rich in inorganic components to reduce the loss of lithium metal during the cycle process, and can achieve lithium metal deposition morphology and coulomb efficiency that are significantly better than those of conventional electrolytes, effectively prevent short circuits caused by dendrite growth, and extend the life of lithium metal full batteries. At the same time, the precursor liquid of the gel electrolyte of the present invention is a local high-concentration electrolyte with low cost, low viscosity, low reactivity, and a high proportion of flame-retardant diluent in the electrolyte, which is not only conducive to reducing the cost of the electrolyte, but also can maximize the flame retardant performance of the electrolyte and battery safety. In addition, the solvents, diluents and additives used in the electrolyte not only intrinsically withstand high pressure, but also help stabilize the interface between the positive electrode and the electrolyte, achieving ultra-high nickel positive electrode ultra-high coulomb efficiency and high capacity retention rate.

[0006] Preferably, the flame retardant diluent is selected from one or more of ethoxy (pentafluoro) cyclotriphosphazene (PFPN), pentafluoro (phenoxy) cyclotriphosphazene, hexachlorotriphosphazene, hexafluorocyclotriphosphazene, hexa(1H, 1H, 3H-perfluoropropoxy)phosphazene, hexa(2,2-difluoroethoxy)phosphazene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE), 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (TFTFE), and 2,2,2-trifluoroethyl ether (BTFE).

[0007] More preferably, the flame retardant diluent is ethoxy (pentafluoro) cyclotriphosphazene (PFPN) and / or 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (TFTFE).

[0008] In the present invention, by using flame-retardant phosphazene or non-flammable hydrofluoroether, not only the flame retardancy of the electrolyte itself can be improved, but also, such substances often have a lower highest occupied molecular orbital (HOMO), thus having an extremely wide electrochemical window and being able to withstand high-voltage electrodes; at the same time, such fluorine-containing chemicals can form an inorganic-rich solid electrolyte interphase (SEI) between lithium metal, effectively passivating the lithium metal surface and improving the battery cycle performance.

[0009] Further preferably, the flame retardant solvent is selected from one or more of 1,3-dimethylpropylene urea, trimethyl phosphate (TMP), triethyl phosphate (TEP), tripropyl phosphate, triisopropyl phosphate, tributyl phosphate, tricresyl phosphate, 1,2-bis(2-chloroethoxy)ethane, and bis[2-(2-chloroethoxy)ethyl]ether.

[0010] More preferably, the flame retardant solvent is trimethyl phosphate (TMP) and / or triethyl phosphate (TEP).

[0011] In the present invention, by using the phosphate ester solvent, the phosphorus free radicals can capture hydrogen free radicals during the combustion process, thereby preventing the combustion reaction from proceeding and achieving a flame retardant effect. At the same time, the phosphate ester solvent has a high solubility for lithium salts and has better high-voltage performance than the ether electrolyte widely used in lithium metal batteries.

[0012] Further preferably, the additive is selected from one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC), bisfluoroethylene carbonate (DFEC), diethylene sulfate (DTD), lithium nitrate (LiNO3), magnesium bistrifluoromethanesulfonyl imide (Mg(TFSI)2), and zinc bistrifluoromethanesulfonyl imide (Zn(TFSI)2).

[0013] More preferably, the additive is lithium nitrate (LiNO 3 ), fluoroethylene carbonate (FEC) and / or magnesium bis(trifluoromethanesulfonyl)imide (Mg(TFSI) 2 ).

[0014] More preferably, the mass ratio of the lithium nitrate, fluoroethylene carbonate and magnesium bis(trifluoromethanesulfonyl)imide is 1:10-30:1-5, preferably 1:20-25:1.5-2.5.

[0015] In the present invention, the film-forming property of SEI can be enhanced by adding fluorocarbonate FEC, and Mg(TFSI)2 can react with lithium metal bulk to form Li-Mg binary alloy, thereby alleviating the volume strain during lithium metal deposition, while enhancing its bulk conductivity and slowing down the growth of lithium metal dendrites.

[0016] Preferably, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoroacetate, lithium nitrate, lithium tetrafluoroborate, and lithium difluorooxalatoborate.

[0017] More preferably, the lithium salt is lithium bis(fluorosulfonyl)imide and / or lithium nitrate.

[0018] More preferably, the cross-linking agent is selected from one or more of poly(ethylene glycol) diacrylate (PEGDA), polyethylene glycol methyl ether acrylate (PEGMEA), and pentaerythritol tetraacrylate (PETEA).

[0019] More preferably, the flame retardant polymerizable monomer is pentaerythritol tetraacrylate, triallyl phosphate, diethyl allyl phosphate, diethyl vinyl phosphonate or dimethyl vinyl phosphonate.

[0020] In the present invention, by adding cross-linkable pentaerythritol tetraacrylate (PETEA) and triallyl phosphate (TAP), a cross-linked polymer network can be formed to gel the electrolyte; and TAP, as a phosphate ester, has certain flame retardant properties, which can further enhance the flame retardancy of the electrolyte.

[0021] More preferably, the initiator includes azobisisobutyronitrile (AIBN), azobisisoheptanenitrile, dibenzoyl peroxide (BPO), dimethyl azobisisobutyrate, tert-butyryl peroxide or tert-butyryl peroxide.

[0022] Preferably, the flame retardant gel electrolyte comprises the following raw materials in parts by weight: 1 to 3 parts of polymer monomer, 35 to 50 parts of diluent, 8 to 20 parts of lithium salt, 15 to 35 parts of solvent, 0.1 to 0.2 parts of initiator, 0.1 to 6 parts of additive, and 1 to 3 parts of cross-linking agent.

[0023] Further preferably, the flame retardant gel electrolyte comprises the following raw materials in parts by mass: 1-2 parts of polymer monomer, 38-50 parts of flame retardant diluent, 15-20 parts of lithium salt, 25-35 parts of solvent, 0.1-0.2 parts of initiator, 4-6 parts of additives, and 1-3 parts of cross-linking agent.

[0024] The fully flame-retardant electrolyte for lithium metal batteries provided by the present invention has a preferred combination of conductivity comparable to that of liquid electrolytes, a very wide electrochemical window, can stabilize the lithium metal negative electrode interface, and has an intrinsically non-flammable property. -2 The Ni92 assembled battery test showed that its capacity retention rate could reach up to 98.5% after 100 cycles (0.33C / 1C charge and discharge), and the average coulombic efficiency after stabilization was higher than 99.9%.

[0025] In a second aspect, the method for preparing the flame retardant gel electrolyte provided by the present invention comprises: 1) Mixing a flame retardant solvent and a lithium salt, stirring at a temperature of 20 to 65° C., to obtain a first solution.

[0026] 2) Mixing the first solution with the additive, heating and stirring for 2 to 3 hours to obtain a second solution.

[0027] 3) Mixing the second solution with a flame retardant diluent to obtain a third solution.

[0028] 4) The third solution is mixed with the flame retardant polymerizable monomer and stirred, an initiator is added, and the mixture is stirred to obtain a gel electrolyte precursor solution.

[0029] 5) heating the gel electrolyte precursor solution at 60-70° C. for 12-18 hours.

[0030] Preferably, the gel electrolyte precursor is used to wet the positive electrode, negative electrode and separator of the button battery, the button battery is assembled, left to stand for 12 to 24 hours, and heated at 60 to 70° C. for 12 to 18 hours; or a certain amount of gel electrolyte precursor is injected into the soft-pack battery, left to stand for 12 to 24 hours, and heated at 60 to 70° C. for 12 to 18 hours.

[0031] In a third aspect, the semi-solid lithium metal battery provided by the present invention comprises the flame-retardant gel electrolyte or the flame-retardant gel electrolyte obtained by the preparation method of the flame-retardant gel electrolyte.

[0032] The polymerization precursor solution of the present invention comprises a high-concentration electrolyte and a local high-concentration electrolyte system, rather than just an ordinary medium- and low-concentration electrolyte. The solvation structure of this type of electrolyte contains a large number of contact ion pairs and ion aggregates, and the proportion of free solvent molecules is extremely low, extending the solvation-enhanced non-flammability. Previous studies focused on flame retardant additives, the amount of which is often small (mass fraction <10%), and one or more of the solvents (carbonates or ethers), polymerization monomers and other components used are still highly flammable (such as CN117080544A). The solvents, additives, and monomers in the electrolyte of the present invention are all intrinsically non-flammable or flame-retardant components, which can achieve better flame retardant effects and battery safety performance. Previous studies have also found it difficult to achieve stable circulation of medium- and high-nickel ternary positive electrodes (such as CN114976236A) while achieving electrolyte non-flammability, as well as a stable lithium metal negative electrode interface (lithium metal deposition / stripping efficiency is higher than 99.0%, and ideally should be higher than 99.5%). The electrolyte of the present invention is based on a non-flammable small molecule solvent and a high-concentration electrolyte system, with the addition of a non-flammable diluent, a film-forming additive, and a high-voltage resistant and flame-retardant polymer monomer. It can not only achieve a highly reversible lithium metal negative electrode, but also withstand an extremely high battery cut-off voltage. At the same time, the polymer cross-linking network solidifies the gel electrolyte and has a certain mechanical strength, which not only helps to inhibit the formation of lithium dendrites, but also prevents the safety hazards caused by electrolyte leakage. Previous studies have also found it difficult to achieve lithium metal batteries at high current densities (≥1mA cm -2 ) (e.g. CN116253823A, ≤0.3mA cm -2 ), it is difficult to support a large surface load of positive electrode (≥3mAh cm -2) Charge and discharge at high rates (≥1C). Based on the special solvation configuration of the electrolyte in the local high-concentration system, lithium ions can be directly deposited on the negative electrode side and embedded in the positive electrode material without desolvation. At the same time, compared with traditional medium and low concentration liquid or semi-solid electrolytes, the electrolyte involved in the present invention forms a thinner, denser and inorganic salt-rich SEI film and CEI film, which has a smaller membrane resistance to lithium ions.

[0033] The beneficial effects of the present invention are at least that: the flame-retardant gel electrolyte of the present invention is a "full flame-retardant electrolyte", which can be non-combustible at high temperature, and its free radical reaction at high temperature can quickly absorb heat, which is conducive to alleviating the rapid temperature rise phenomenon of the battery thermal runaway process and enhancing the battery safety performance. In addition, the flame-retardant gel electrolyte is based on a local high-concentration electrolyte system, and there are a large number of "lithium ion-anion" ion pairs, which can preferentially decompose on the electrode surface to form a solid electrolyte interface phase (SEI) rich in inorganic components to reduce the loss of lithium metal during the cycle process, and can achieve lithium metal deposition morphology and coulomb efficiency that are significantly better than traditional electrolytes, effectively prevent short circuits caused by dendrite growth, and extend the life of lithium metal full batteries. At the same time, the precursor liquid of the flame-retardant gel electrolyte of the present invention is a local high-concentration electrolyte, low-cost, low-viscosity, low-reactivity, and the flame-retardant diluent accounts for the highest proportion in the electrolyte, which is not only conducive to reducing the cost of the electrolyte, but also can maximize the flame retardant performance of the electrolyte and battery safety. In addition, the solvents, diluents and additives used in the flame-retardant gel electrolyte are not only intrinsically resistant to high voltage, but can also help stabilize the interface between the positive electrode and the electrolyte, achieving ultra-high nickel positive electrode ultra-high coulombic efficiency and high capacity retention rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0035] Figure 1 These are photos of the combustion test of the gel electrolyte precursor solution provided in the embodiments and comparative examples of the present invention.

[0036] Figure 2 These are photos of the gel electrolyte combustion test provided for the embodiments and comparative examples of the present invention.

[0037] Figure 3 Scanning electron microscope photos of the lithium metal deposition morphology in different gel electrolyte precursor solutions provided in the embodiments of the present invention. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] Take 10.7g (10mL) of triethyl phosphate (TEP) as solvent, dissolve 6g of lithium bis(fluorosulfonyl)imide (LiFSI) in TEP, stir at 60°C until completely dissolved, add 0.069g of LiNO3 to the above solution, stir until it is fully dissolved, and obtain precursor solution 1. Add 15.6g of ethoxy(pentafluoro)cyclotriphosphazene to the above precursor solution 1, stir and mix evenly to obtain a precursor solution. Add 0.4g of pentaerythritol tetraacrylate (PETEA) and 0.8g of triallyl phosphate (TAP), stir at room temperature for 2h to form a transparent uniform solution, then add 0.04g of dibenzoyl peroxide (BPO), stir until it is completely dissolved, obtain a polymerization precursor solution and store at low temperature. Heat in a 70°C constant temperature box for 12h to allow the polymerization precursor solution to fully polymerize.

[0041] Example 2

[0042] In Example 1, "0.069 g LiNO3" was changed to "0.069 g LiNO3, and 1.65 g FEC", and other conditions remained unchanged.

[0043] Example 3

[0044] The additive "0.069 g LiNO3" in Example 1 was changed to "0.069 g LiNO3, 0.146 g Mg(TFSI)2, and 1.65 g FEC", and other conditions remained unchanged.

[0045] Example 4

[0046] The ethoxy (pentafluoro) cyclotriphosphazene (PFPN) in Example 1 was replaced with 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether (TFTFE).

[0047] Example 5

[0048] The TEP in Example 1 was changed to trimethyl phosphate (TMP).

[0049] Example 6

[0050] The 6 g LiFSI in Example 1 was replaced with 3 g lithium hexafluorophosphate (LiPF6), and other conditions remained unchanged.

[0051] Example 7

[0052] The 6 g LiFSI in Example 1 was replaced with 6 g lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), and other conditions remained unchanged.

[0053] Example 8

[0054] The “pentaerythritol tetraacrylate (PETEA) with a mass of 0.4 g and triallyl phosphate (TAP) with a mass of 0.8 g” in Example 1 was changed to “pentaerythritol tetraacrylate (PETEA) with a mass of 0.6 g”, and other conditions remained unchanged.

[0055] Comparative Example 1

[0056] The TEP in Example 1 was changed to dimethyl carbonate (DMC), and ethoxy (pentafluoro) cyclotriphosphazene (PFPN) was not added.

[0057] Comparative Example 2

[0058] In Example 1, ethoxy (pentafluoro) cyclotriphosphazene (PFPN) was not added, and the other parts remained unchanged.

[0059] Comparative Example 3

[0060] The "mass of 0.4 g of pentaerythritol tetraacrylate (PETEA) and 0.8 g of triallyl phosphate (TAP)" in Example 1 was changed to "mass of 0.6 g of pentaerythritol tetraacrylate (PETEA) and 1.2 g of triallyl phosphate (TAP)", and other conditions remained unchanged.

[0061] Experimental Example 1

[0062] 1) Add 9 g of nickel 9 series ternary material (Ni92), 0.5 g of conductive carbon black and 0.5 g of polyvinylidene fluoride into 10 ml of NMP solution, stir (rotation speed 1000 rpm) for 10 min to prepare a slurry.

[0063] 2) The slurry was coated on aluminum foil and baked at 80°C in vacuum for 12 h to obtain a Ni92 positive electrode sheet with a loading of 12 mg / cm 2 .

[0064] 3) The Ni92 positive electrode sheet was cut into discs with a diameter of 14 mm, and a 50 μm thick lithium metal disc was used as the anode. The polymerization precursor solution provided in different embodiments or comparative examples was injected, and a CR2032 button battery was assembled. The battery was heated at 70°C for 12 h to allow the electrolyte to fully polymerize. The constant current charge and discharge test was performed at 0.33C / 1C for 100 cycles, and then the capacity retention rate was compared.

[0065] Experimental Example 2

[0066] 1) A 200 μm thick lithium metal foil (14 mm in diameter) was used as the anode and a smooth copper foil (16 mm in diameter) was used as the cathode. The polymerization precursor solution provided in different embodiments or comparative examples was injected to assemble a CR2032 button cell (lithium-copper half-cell). The cell was heated at 70° C. for 12 h to allow the electrolyte to fully polymerize. A constant current charge and discharge test (cycle current 0.5 mA cm -2 , constant discharge capacity per cycle 1mAh cm -2 ), cycled 120 times, and took the average coulombic efficiency of the 20th to 120th cycles as the lithium metal efficiency of the electrolyte.

[0067] like Figure 1 As shown, Comparative Example 1 using the flammable solvent DMC and without adding PFPN is highly flammable when not polymerized and can be ignited by heating with an ignition gun, while Comparative Example 2 and Example 1 using the phosphate ester TEP are not flammable, and Example 1 adding PFPN emits white smoke when heated by an igniter, indicating that a strong endothermic reaction occurs therein.

[0068] like Figure 2 As shown, the electrolyte of Comparative Example 1 is still highly flammable after thermally initiated polymerization, but the intensity of the burning flame is less than that of the liquid state. On the one hand, it is because the in-situ polymerization solidifies it and reduces the activity of the electrolyte. On the other hand, the added flame retardant monomer has a certain degree of flame retardant effect. The electrolytes described in Comparative Example 2 and Example 1 are not flammable after polymerization, but the polymerized electrolyte of Comparative Example 2 will appear charred black after ignition and heating, while the polymerized electrolyte of Example 1 can maintain its original appearance.

[0069] like Figure 3 As shown, the electrolytes of Comparative Examples 1 and 2 cannot induce planar island deposition of lithium metal and may even induce dendrites, while the electrolyte of Example 1 can achieve a better deposition morphology of lithium metal, indicating that PFPN-type fluorine-containing diluents have a good stabilizing effect on the lithium metal interface.

[0070] In the cycle performance of Table 1, the electrolyte of Example 1 can ensure a longer battery cycle life (higher capacity retention rate). Table 1

[0071]

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A flame retardant gel electrolyte, characterized in that: The invention comprises the following raw materials in parts by weight: 1 to 3 parts of polymer monomer, 35 to 70 parts of diluent, 5 to 20 parts of lithium salt, 15 to 35 parts of solvent, 0.1 to 0.2 parts of initiator, 0.1 to 10 parts of additive and 1 to 3 parts of cross-linking agent; the diluent is a fluorine-containing flame retardant diluent, the additive is an inorganic salt additive and / or an organic small molecule additive, the solvent is a flame retardant solvent, and the polymer monomer is a flame retardant polymer monomer.

2. The flame retardant gel electrolyte according to claim 1, characterized in that: The flame retardant diluent is selected from one or more of ethoxy (pentafluoro) cyclotriphosphazene, pentafluoro (phenoxy) cyclotriphosphazene, hexachlorotripolyphosphazene, hexafluorocyclotriphosphazene, hexa(1H, 1H, 3H-perfluoropropoxy)phosphazene, hexa(2,2-difluoroethoxy)phosphazene, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, and 2,2,2-trifluoroethyl ether.

3. The flame retardant gel electrolyte according to claim 1 or 2, characterized in that: The flame retardant solvent is selected from one or more of 1,3-dimethylpropyleneurea, trimethyl phosphate, triethyl phosphate, tripropyl phosphate, triisopropyl phosphate, tributyl phosphate, tricresyl phosphate, 1,2-bis(2-chloroethoxy)ethane, and bis[2-(2-chloroethoxy)ethyl]ether.

4. The flame retardant gel electrolyte according to any one of claims 1 to 3, characterized in that: The additive is selected from one or more of fluoroethylene carbonate, vinylene carbonate, bisfluoroethylene carbonate, vinyl sulfate, lithium nitrate, magnesium bistrifluoromethanesulfonyl imide, and zinc bistrifluoromethanesulfonyl imide.

5. The flame retardant gel electrolyte according to any one of claims 1 to 4, characterized in that: The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium trifluoroacetate, lithium nitrate, lithium tetrafluoroborate, and lithium difluorooxalatoborate.

6. The flame retardant gel electrolyte according to any one of claims 1 to 5, characterized in that: The crosslinking agent is selected from one or more of poly(ethylene glycol) diacrylate, polyethylene glycol methyl ether acrylate, and pentaerythritol tetraacrylate.

7. The flame retardant gel electrolyte according to any one of claims 1 to 6, characterized in that: The flame retardant polymer monomer is triallyl phosphate, diethyl allyl phosphate, diethyl vinyl phosphonate or dimethyl vinyl phosphonate.

8. The flame retardant gel electrolyte according to any one of claims 1 to 7, characterized in that: The initiator includes azobisisobutyronitrile, azobisisoheptanenitrile, dibenzoyl peroxide, dimethyl azobisisobutyrate, tert-butyryl peroxide or tert-butyryl peroxide.

9. The method for preparing the flame retardant gel electrolyte according to any one of claims 1 to 8, characterized in that: include: 1) mixing a flame retardant solvent and a lithium salt, and stirring at a temperature of 20 to 65° C. to obtain a first solution; 2) mixing the first solution with the additive, heating and stirring for 2 to 3 hours to obtain a second solution; 3) mixing the second solution with a flame retardant diluent to obtain a third solution; 4) mixing the third solution with the flame retardant polymerizable monomer, adding an initiator, and stirring to obtain a gel electrolyte precursor solution; Optionally, 5) heating the gel electrolyte precursor solution at 60-70° C. for 12-18 hours.

10. A semi-solid lithium metal battery, characterized in that: The invention relates to a flame retardant gel electrolyte comprising the flame retardant gel electrolyte according to any one of claims 1 to 8 or the flame retardant gel electrolyte obtained by the preparation method of the flame retardant gel electrolyte according to claim 9.

Citation Information

Patent Citations

  • Flame-retardant gel electrolyte for lithium metal as well as preparation method and application of flame-retardant gel electrolyte

    CN114976236A

  • Method for preparing high-fluorine flame-retardant electrolyte suitable for metal lithium battery

    CN116253823A

  • Preparation method of flame-retardant gel electrolyte

    CN117080544A

Cited By

  • Multi-effect flame-retardant in-situ gel polymer electrolyte and application thereof

    CN120127206A

  • Lithium metal battery low-enthalpy-change high-safety semi-solid electrolyte and preparation method and application thereof

    CN120767402A

  • Semi-solid battery and preparation method thereof

    CN121507079A

  • Flame-retardant gel electrolyte, preparation method thereof and lithium ion battery containing electrolyte

    CN121507084A

  • Local high-concentration flame-retardant gel polymer electrolyte, battery and preparation method thereof

    CN121662964A