Ta-containing cobalt-based metal glass composite material and preparation method thereof
By developing a Co-based metal glass composite material containing Ta, the thermal stability and shape and size limitation of Co-based amorphous alloys in high-frequency and high-temperature environments are solved, and the high thermal stability, hardness and corrosion resistance are improved. Suitable for electromagnetic shielding and magnetic sensor applications in high temperature environments.
Patent Information
- Application Number
- CN202410920196.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
Co-based amorphous alloys have thermal stability and shape and size limitations in high-frequency applications and high-temperature environments, which cannot meet the needs of complex magnetic materials. At the same time, their temperature range is insufficient, making it difficult to meet the requirements of modern power electronic devices and high-temperature service environments.
Develop a Co-based metal glass composite material containing Ta, with the chemical formula of Co66FexNiyTa5-x-ySi15B14, and is prepared by vacuum arc furnace and high vacuum single-roll rotary quenching belt technology to form non-ferrous and non-resistant thermal stability, hardness and corrosion resistance. Crystal structure.
The material has high thermal stability, hardness and corrosion resistance. It is suitable for electromagnetic shielded alloy coatings and magnetic sensors in high temperature environments, extending the service life of the equipment and reducing the cost of renewal.
Smart Images

Figure CN118880202A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of amorphous alloy / metallic glass materials, and relates to a cobalt-metal glass composite material having high thermal stability, thermal magnetic properties, hardness and corrosion resistance and a preparation method thereof, and specifically relates to a Ta-containing cobalt-based metallic glass composite material and a preparation method thereof. Background Art
[0002] Metallic glasses (MGs) are a new type of metal material that has gradually developed in the middle of the last century and are regarded as one of the most promising new functional materials in this century. Metallic glass is made by rapid cooling of molten metal liquid. Due to its unique internal structure, it has excellent physical and chemical properties of both metal and glass, and is also called amorphous alloy. As early as 1934, German scientist Krammer condensed metal vapor onto a low-temperature liner by vapor deposition and prepared amorphous alloy film for the first time. In the 1960s, Professor Duwez of the United States first obtained Au-Si amorphous alloy with a thickness of about 20μm by melt spinning. The atomic arrangement of amorphous alloys shows the characteristics of long-range disorder and short-range order, showing macroscopic isotropy, without defects such as dislocations and grain boundaries commonly seen in crystalline materials, and generally has ultra-high fracture toughness, high strength, high hardness, large elastic limit, wear resistance, corrosion resistance, electrical conductivity and unique self-healing ability. In addition, soft magnetic amorphous alloys also have excellent properties such as low coercivity, high magnetic permeability, and low iron loss, and have been industrially applied.
[0003] Co-based metallic glass not only has the above-mentioned excellent soft magnetic properties under high-frequency application conditions, but also has high strength, good thermal stability, insensitivity to mechanical stress and near-zero magnetostriction coefficient, which is beneficial to the stability and reliability of power electronic components. Co-based metallic glass greatly meets the needs of modern power electronic devices to develop in the direction of energy saving and high frequency, and has therefore attracted great attention. However, due to its relatively low amorphous forming ability, Co-based metallic glass cannot meet the requirements of some magnetic materials with shape and size requirements, which limits its scope of use. At the same time, with the improvement of service environment requirements, breaking through the operating temperature range of amorphous alloys is also one of the problems that need to be solved urgently. Faced with the increasingly stringent use conditions and service environment, materials are required to not only have outstanding functional characteristics, but also to pay attention to whether their comprehensive performance meets extreme service conditions. Therefore, it is imperative to develop high-performance materials that take into account multiple performance characteristics.
[0004] To this end, the development of Co-based amorphous magnetic materials suitable for large-scale promotion and use, which have a balance of thermal stability, magnetic properties, mechanical properties and corrosion resistance, has natural advantages in energy application fields, optoelectronic information and sensing fields, and alloy applications in high-temperature service environments. Summary of the invention
[0005] In order to solve the above problems, the object of the present invention is to provide a Ta-containing cobalt-based metallic glass composite material, which has outstanding thermal stability, high hardness, good magnetic properties and corrosion resistance.
[0006] It can be used as a potential raw material for metal structural parts, magnetic components or sensor components, as well as high-temperature and corrosion-resistant metal protective coatings.
[0007] Another object of the present invention is to provide a use of the Ta-containing cobalt-based metallic glass composite material.
[0008] In order to achieve the above object, the present invention provides a Ta-containing cobalt-based metallic glass composite material, wherein the chemical formula of the cobalt-based metallic glass is Co 66 Fe x Ni y Ta 5-x-y Si 15 B 14 , where x=0~3, y=0~1 (both are atomic fractions, at.%).
[0009] That is, the atomic fraction of Co is 66%, the atomic fraction of Si is 15%, the atomic fraction of B is 14%, and the sum of the atomic fractions of Fe, Ni, and Ta is 5%.
[0010] The method for preparing the Ta-containing cobalt-based metallic glass composite material comprises the following steps:
[0011] 1) weighing the required mass of Co, Fe, Ni, Ta, Si and B raw materials in the form of particles or blocks according to the atomic fraction in the chemical formula of the alloy and performing surface treatment;
[0012] 2) The prepared raw materials are melted in a vacuum arc furnace with a melting current of 180-270A for 3-5 times to form a master alloy ingot; wherein the vacuum degree in the vacuum arc furnace is 1.0×10 -3 Pa~3.0×10 -3 Pa, by filling with argon gas, repeating the vacuum operation to ensure that there is no impurity gas in the furnace chamber; at the same time, the pressure difference between the belt-spinning machine chamber and the quartz tube is controlled at 0.010~0.040Mpa;
[0013] 3) crushing the master alloy ingot described in step 2) and placing it in a quartz tube, placing the quartz tube in the induction coil of a vacuum belt spinning machine to melt the master alloy ingot, and after melting, spraying the liquid alloy onto the surface of a high-speed rotating copper roller in the vacuum belt spinning machine to quickly cool it to obtain a cobalt-based metallic glass ribbon; wherein the vacuum degree in the vacuum belt spinning machine is 1.0×10 -3 Pa~3.0×10-3 Pa; the surface linear velocity of the copper roller is 30-40 m / s.
[0014] Furthermore, the surface treatment in step 1) is to mechanically grind the particles or block raw materials to remove the surface oxide scale, and then ultrasonically clean them with acetone or alcohol for 30 seconds, and repeat the cleaning 1 to 3 times.
[0015] Furthermore, the strip-shaped cobalt-based metallic glass composite material has a thickness of 25 to 40 μm and a width of 1.0 to 2.0 mm.
[0016] The present invention also provides a use of the Ta-containing cobalt-based metallic glass composite material as a raw material for metal structural parts, magnetic components or sensor components, and high-temperature corrosion-resistant metal protective coatings.
[0017] In the preparation process, the melting current range defined in step 2) ensures the complete melting of the raw materials. If the current is too small, the element particles will not be completely melted. If the current is too large, it is easy to cause the elements to volatilize, resulting in a large error in the alloy composition. Repeated melting 3 to 5 times to ensure uniform composition of the master alloy ingot is also to avoid large differences in composition as much as possible.
[0018] The Ta-containing cobalt-based metallic glass composite material provided by the present invention comprises the high melting point element Ta, which can improve the thermal stability of the alloy; the elements Co, Fe and Ni, which have high hardness and good wear resistance, are selected, and they can make the alloy have better magnetic properties; the non-metallic elements Si and B are selected, and they can promote the formation of the amorphous structure of the alloy and help improve the glass forming ability of the alloy.
[0019] The present invention adopts high vacuum single-roller spinning quenching and spinning technology to prepare a strip-shaped Ta-containing cobalt-based metallic glass composite material. On the one hand, due to the large size difference between the atoms of each element, it is easy to form an amorphous structure. On the other hand, the rapid quenching process of the single-roller spinning machine makes the metal atoms arranged in a disordered state, and there are no local structural uneven defects such as grain boundaries, stacking faults, and segregation that crystalline metals have. Therefore, the cobalt-based metallic glass obtained by this method has good corrosion resistance. Generally speaking, a high cooling rate is conducive to rapid cooling and solidification to prepare amorphous alloys of different forms. At present, the cooling rate of amorphous alloy strips prepared by the spinning process can reach 10 5 ~10 6 K / s, generally higher than the amorphous alloy rods made by copper mold suction casting or spray casting (10 2 ~10 4 K / s and the cooling rate of small-sized amorphous materials such as amorphous alloy powder prepared by atomization (10 3 ~10 5K / s). Therefore, when the prepared strip is determined to be an amorphous structure by XRD diffraction, an amorphous alloy powder or an alloy powder of an amorphous / nanocrystalline composite structure with the same composition can be prepared by using a gas atomization or water atomization process with a slightly lower cooling rate. Furthermore, this type of composite material can also be used as a potential new electromagnetic shielding alloy coating raw material that takes into account high-temperature stability, thermal magnetic properties, corrosion resistance, and wear resistance, and can be used in extremely harsh marine environments or extremely high-temperature service environments to effectively protect the surface of major equipment components.
[0020] The cobalt-based metallic glass composite material obtained by the present invention is a completely amorphous structure or a composite structure composed of "amorphous + a small amount of crystallized phase". By adding small atomic radius elements Si and B (r(Si) = 115.3pm, r(B) = 82.0pm), the atomic radius difference between them and other elements is increased (r(Fe) = 124.1pm, r(Ni) = 124.6pm, r(Co) = 125.3pm, r(Ta) = 143.0pm), so that the alloy is more inclined to produce an amorphous structure, thereby avoiding structural defects such as dislocations and twins.
[0021] The present invention can effectively improve the thermal stability of the alloy by selecting the high melting point element Ta as the alloy component element. At the same time, the production cost of the Ta element is lower than that of the Hf element, the V element, and the Re element, which is more economical. It has been found through testing that the initial crystallization temperature of the cobalt-based metallic glass composite material containing the Ta element is above 846K. At the same time, the average Vickers microhardness of this series of alloys is higher than 935HV 0.1 , the self-corrosion current density is maintained at 10 -6 A / cm 2 The order of magnitude indicates that the actual corrosion degree of the alloy is lower. According to the MT curve test, the Curie temperature of the metal composite material is above 580K. The cobalt-based metallic glass composite material can take into account the synergistic improvement of multiple performances and can be applied to related offshore wind power generation equipment, surface protection of major key equipment components in high-temperature environments, and selection of magnetic core components of magnetic sensors in high-temperature environments, with the aim of maximizing the comprehensive performance of the material.
[0022] The beneficial effects of the present invention are:
[0023] The present invention provides a Ta-containing cobalt-based metallic glass composite material and a preparation method thereof. Compared with conventional commercial cobalt-based amorphous alloys, the material has higher thermal stability, low overall raw material cost, simple and easy operation steps, and easy process control. A new metallic glass composite material with uniform composition, excellent thermal magnetic properties, hardness and corrosion resistance can be obtained, so the material can be used as a raw material for metal structural parts, magnetic components of power equipment, and high-temperature corrosion-resistant metal protective coatings. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the XRD pattern of the cobalt-based metallic glass composite material prepared in Examples 1-5.
[0025] Figure 2 This is a SEM scan image of the cobalt-based metallic glass composite material prepared in Example 1.
[0026] Figure 3 DSC curves of the cobalt-based metallic glass composite materials prepared in Examples 1-5.
[0027] Figure 4 MT curves of the cobalt-based metallic glass composite materials prepared in Examples 1-5.
[0028] Figure 5 The hardness of the cobalt-based metallic glass composite material prepared in Examples 1-5.
[0029] Figure 6 Potentiodynamic polarization curves obtained through electrochemical testing of the cobalt-based metallic glass composite materials prepared in Examples 1-5. DETAILED DESCRIPTION
[0030] The embodiments of the present invention will be described in detail and in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more specific definition of the protection scope of the present invention. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0031] The raw materials of Co, Fe, Ni, Ta, Si and B used in the preparation of the ingots of the present invention are all commercially available raw materials with a purity higher than 99.9wt%.
[0032] The arc melting furnace used in the present invention is specifically a NMS-DRII rotary vacuum copper mold melting system developed by Chengdu Zhongke New Materials Technology Engineering Co., Ltd.
[0033] The vacuum belt spinning machine used in the present invention is specifically a swing-type small vacuum induction melting and quenching system produced by Zhongke Instrument Co., Ltd., wherein a water-cooling circulation system is provided under the copper roller of the vacuum belt spinning machine to ensure that the temperature of the copper roller is always maintained below 20°C, and the roller speed can reach a maximum of more than 4000rpm (the maximum linear speed can reach 45m / s), so that the cooling rate of the strip-shaped metallic glass can reach 10 5 ~10 6 K / s.
[0034] The following examples 1-5 prepare Co 66 Fe3Ni1Ta1Si 15 B14 ,Co 66 Fe2Ni1Ta2Si 15 B 14 ,Co 66 Fe1Ni1Ta3Si 15 B 14 ,Co 66 Ni1Ta4Si 15 B 14 and Co 66 Ta5Si 15 B 14 Five cobalt-based metallic glass composites with different compositions were simultaneously studied for their properties and microstructural characterization.
[0035] Example 1Co 66 Fe3Ni1Ta1Si 15 B 14 Preparation of Cobalt-based Metallic Glass Composites
[0036] First, the atomic fraction of the cobalt-based metallic glass composite material is converted into mass percentage, and high-purity cobalt particles, iron particles, nickel particles, tantalum particles, silicon particles and boron particles (purity not less than 99.9%) are selected as raw materials, and the oxide scale is polished and ultrasonically cleaned with acetone or alcohol, and the ingredients are mixed using a high-precision balance with an accuracy of 0.001g. The mass of the smelting ingot is 30g, so the mass of each element is w(Co)=23.963g, w(Fe)=1.032g, w(Ni)=0.363g, w(Ta)=1.115g, w(Si)=2.595g, and w(B)=0.932g.
[0037] The master alloy ingot was prepared by arc melting under vacuum and argon protection conditions, and the vacuum was repeatedly evacuated three times to 2.0×10 -3 Pa, and then 99.999% pure argon gas is introduced to the vacuum chamber until the pressure is -0.8MPa. High-purity argon gas is used as protective gas and arc medium. The melting current is 240A. Cooling water is passed during melting to prevent the water-cooled copper plate from overheating and melting. Sponge titanium is first used to adsorb the remaining impurity gas. After the gas is adsorbed, the sample is melted. It needs to be remelted 4 times to ensure the uniformity of the alloy ingot. After cooling, Co 66 Fe3Ni1Ta1Si 15 B 14 Master alloy ingot.
[0038] Co 66 Fe3Ta1Ni1Si 15 B 14The master alloy ingot was crushed, 4 g was taken into a quartz tube, and the quartz tube was placed in the induction coil of the belt spinning machine. The diameter of the quartz tube nozzle was 1 mm, and the height of the nozzle from the copper roller was 0.4 mm. The vacuum degree was drawn to 2.0×10 -3 Pa, then filled with argon, repeated vacuum operation to ensure that there is no impurity gas in the furnace chamber, and the pressure difference between the chamber of the belt spinning machine and the quartz tube is controlled at 0.020Mpa. The alloy is heated by a copper coil, and after the alloy is melted, the liquid alloy is sprayed onto a high-speed copper roller to obtain the alloy strip, wherein the surface linear speed of the copper roller is 38m / s, Co 66 Fe3Ni1Ta1Si 15 B 14 The thickness of the cobalt-based metallic glass composite is 35±5 μm.
[0039] Example 2Co 66 Fe2Ni1Ta2Si 15 B 14 Preparation of Cobalt-based Metallic Glass Composites
[0040] First, the atomic fraction of the cobalt-based metallic glass composite material is converted into mass percentage, and high-purity cobalt particles, iron particles, nickel particles, tantalum particles, silicon particles and boron particles (purity not less than 99.9%) are selected as raw materials, and the oxide scale is polished and ultrasonically cleaned with acetone or alcohol, and the ingredients are mixed using a high-precision balance with an accuracy of 0.001g. The mass of the smelting ingot is 30g, so the mass of each element is w(Co)=23.363g, w(Fe)=0.671g, w(Ni)=0.353g, w(Ta)=2.174g, w(Si)=2.530g, and w(B)=0.909g.
[0041] The master alloy ingot was prepared by arc melting under vacuum and argon protection conditions, and the vacuum was repeatedly evacuated three times to 2.0×10 -3 Pa, and then 99.999% pure argon gas is introduced to the vacuum chamber until the pressure is -0.8MPa. High-purity argon gas is used as protective gas and arc medium. The melting current is 240A. Cooling water is passed during melting to prevent the water-cooled copper plate from overheating and melting. Sponge titanium is first used to adsorb the remaining impurity gas. After the gas is adsorbed, the sample is melted. It needs to be remelted 4 times to ensure the uniformity of the alloy ingot. After cooling, Co 66 Fe2Ni1Ta2Si 15 B 14 Master alloy ingot.
[0042] Co 66 Fe2Ni1Ta2Si 15 B 14The master alloy ingot was crushed, 4 g was taken into a quartz tube, and the quartz tube was placed in the induction coil of the belt spinning machine. The diameter of the quartz tube nozzle was 1 mm, and the height of the nozzle from the copper roller was 0.4 mm. The vacuum degree was drawn to 2.0×10 -3 Pa, then filled with argon, repeated vacuum operation to ensure that there is no impurity gas in the furnace chamber, and the pressure difference between the chamber of the belt spinning machine and the quartz tube is controlled at 0.020Mpa. The alloy is heated by a copper coil, and after the alloy is melted, the liquid alloy is sprayed onto a high-speed copper roller to obtain the alloy strip, wherein the surface linear speed of the copper roller is 38m / s, Co 66 Fe2Ni1Ta2Si 15 B 14 The thickness of the cobalt-based metallic glass composite is 35±5 μm.
[0043] Example 3Co 66 Fe1Ni1Ta3Si 15 B 14 Preparation of Cobalt-based Metallic Glass Composites
[0044] First, the atomic fraction of the cobalt-based metallic glass composite material is converted into mass percentage, and high-purity cobalt particles, iron particles, nickel particles, tantalum particles, silicon particles and boron particles (purity not less than 99.9%) are selected as raw materials, and the oxide scale is polished and ultrasonically cleaned with acetone or alcohol, and the ingredients are mixed using a high-precision balance with an accuracy of 0.001g. The mass of the smelting ingot is 30g, so the mass of each element is w(Co)=22.792g, w(Fe)=0.327g, w(Ni)=0.344g, w(Ta)=3.181g, w(Si)=2.469g, and w(B)=0.887g.
[0045] The master alloy ingot was prepared by arc melting under vacuum and argon protection conditions, and the vacuum was repeatedly evacuated three times to 2.0×10 -3 Pa, and then 99.999% pure argon gas is introduced to the vacuum chamber until the pressure is -0.8MPa. High-purity argon gas is used as protective gas and arc medium. The melting current is 240A. Cooling water is passed during melting to prevent the water-cooled copper plate from overheating and melting. Sponge titanium is first used to adsorb the remaining impurity gas. After the gas is adsorbed, the sample is melted. It needs to be remelted 4 times to ensure the uniformity of the alloy ingot. After cooling, Co 66 Fe1Ta3Ni1Si 15 B 14 Master alloy ingot.
[0046] Co 66 Fe1Ni1Ta3Si 15 B 14The master alloy ingot was crushed, 4 g was taken into a quartz tube, and the quartz tube was placed in the induction coil of the belt spinning machine. The diameter of the quartz tube nozzle was 1 mm, and the height of the nozzle from the copper roller was 0.4 mm. The vacuum degree was drawn to 2.0×10 -3 Pa, then filled with argon, repeated vacuum operation to ensure that there is no impurity gas in the furnace chamber, and the pressure difference between the chamber of the belt spinning machine and the quartz tube is controlled at 0.020Mpa. The alloy is heated by a copper coil, and after the alloy is melted, the liquid alloy is sprayed onto a high-speed copper roller to obtain the alloy strip, wherein the surface linear speed of the copper roller is 38m / s, Co 66 Fe1Ni1Ta3Si 15 B 14 The thickness of the cobalt-based metallic glass composite is 35±5 μm.
[0047] Example 4Co 66 Ni1Ta4Si 15 B 14 Preparation of Cobalt-based Metallic Glass Composites
[0048] First, the atomic fraction of the cobalt-based metallic glass composite material is converted into mass percentage, and high-purity cobalt particles, nickel particles, tantalum particles, silicon particles and boron particles (purity not less than 99.9%) are selected as raw materials, and the oxide skin is polished and ultrasonically cleaned with acetone or alcohol, and the ingredients are mixed using a high-precision balance with an accuracy of 0.001g. The mass of the smelting ingot is 30g, so the mass of each element is w(Co)=22.248g, w(Ni)=0.336g, w(Ta)=4.140g, w(Si)=2.410g, and w(B)=0.866g.
[0049] The master alloy ingot was prepared by arc melting under vacuum and argon protection conditions, and the vacuum was repeatedly evacuated three times to 2.0×10 -3 Pa, and then 99.999% pure argon gas is introduced to the vacuum chamber until the pressure is -0.8MPa. High-purity argon gas is used as protective gas and arc medium. The melting current is 240A. Cooling water is passed during melting to prevent the water-cooled copper plate from overheating and melting. Sponge titanium is first used to adsorb the remaining impurity gas. After the gas is adsorbed, the sample is melted. It needs to be remelted 4 times to ensure the uniformity of the alloy ingot. After cooling, Co 66 Ni1Ta4Si 15 B 14 Master alloy ingot.
[0050] Co 66 Ni1Ta4Si 15 B 14 The master alloy ingot was crushed, 4 g was taken into a quartz tube, and the quartz tube was placed in the induction coil of the belt spinning machine. The diameter of the quartz tube nozzle was 1 mm, and the height of the nozzle from the copper roller was 0.4 mm. The vacuum degree was drawn to 2.0×10-3 Pa, then filled with argon, repeated vacuum operation to ensure that there is no impurity gas in the furnace chamber, and the pressure difference between the chamber of the belt spinning machine and the quartz tube is controlled at 0.020Mpa. The alloy is heated by a copper coil, and after the alloy is melted, the liquid alloy is sprayed onto a high-speed copper roller to obtain the alloy strip, wherein the surface linear speed of the copper roller is 38m / s, Co 66 Ni1Ta4Si 15 B 14 The thickness of the cobalt-based metallic glass composite is 35±5 μm.
[0051] Example 5Co 66 Ta5Si 15 B 14 Preparation of Cobalt-based Metallic Glass Composites
[0052] First, the atomic fraction of the cobalt-based metallic glass composite material is converted into mass percentage, and high-purity cobalt particles, tantalum particles, silicon particles and boron particles (purity not less than 99.9%) are selected as raw materials. After grinding the oxide skin, they are ultrasonically cleaned with acetone or alcohol, and the ingredients are mixed using a high-precision balance with an accuracy of 0.001g. The mass of the smelting ingot is 30g, so the mass of each element is w(Co)=21.742g, w(Ta)=5.057g, w(Si)=2.355g, and w(B)=0.846g.
[0053] The master alloy ingot was prepared by arc melting under vacuum and argon protection conditions, and the vacuum was repeatedly evacuated three times to 2.0×10 -3 Pa, and then 99.999% pure argon gas is introduced to the vacuum chamber until the pressure is -0.8MPa. High-purity argon gas is used as protective gas and arc medium. The melting current is 240A. Cooling water is passed during melting to prevent the water-cooled copper plate from overheating and melting. Sponge titanium is first used to adsorb the remaining impurity gas. After the gas is adsorbed, the sample is melted. It needs to be remelted 4 times to ensure the uniformity of the alloy ingot. After cooling, Co 66 Ta5Si 15 B 14 Master alloy ingot.
[0054] Co 66 Ta5Si 15 B 14 The master alloy ingot was crushed, 4 g was taken into a quartz tube, and the quartz tube was placed in the induction coil of the belt spinning machine. The diameter of the quartz tube nozzle was 1 mm, and the height of the nozzle from the copper roller was 0.4 mm. The vacuum degree was drawn to 2.0×10 -3Pa, then filled with argon, repeated vacuum operation to ensure that there is no impurity gas in the furnace chamber, and the pressure difference between the chamber of the belt spinning machine and the quartz tube is controlled at 0.020Mpa. The alloy is heated by a copper coil, and after the alloy is melted, the liquid alloy is sprayed onto a high-speed copper roller to obtain the alloy strip, wherein the surface linear speed of the copper roller is 38m / s, Co 66 Ta5Si 15 B 14 The thickness of the cobalt-based metallic glass composite is 35±5 μm.
[0055] Example 6 Determination of properties of Ta-containing cobalt-based metallic glass composite materials
[0056] Various properties of the Ta-containing cobalt-based metallic glass composite materials prepared in Examples 1-5 were measured.
[0057] The cobalt-based metallic glass composite Co was characterized by using Bruker D8ADVANCE series X-ray diffractometer and Thermo Fisher Apreo 2C. 66 Fe3Ni1Ta1Si 15 B 14 ,Co 66 Fe2Ni1Ta2Si 15 B 14 ,Co 66 Fe1Ni1Ta3Si 15 B 14 ,Co 66 Ni1Ta4Si 15 B 14 and Co 66 Ta5Si 15 B 14 Phase analysis and microstructure morphology characterization were performed respectively. The operating voltage and current of the XRD diffractometer were 40 kV and 40 mA respectively. The X-ray source was Cu Kα (λ = 0.15406 nm) ray. The scanning speed was 1° / min and the scanning range was 30° to 90°. The results are shown in Figure 1 As shown. Figure 1 It can be seen that the five cobalt-based metallic glasses in Examples 1-5 have typical diffuse scattering peaks of amorphous structures or a composite structure composed of "amorphous + a small amount of crystallized phase", indicating that the prepared strips do have amorphous structures. Figure 2 ,As can be seen from the figure, the surface of the strip is smooth, flat and dense, and there are no obvious holes or gaps on the surface of the strip.
[0058] The DSC curves of the alloys of Examples 1-5 were measured using a differential scanning calorimeter (DSC 404-F3 model) from NETZSCH, Germany. The results are as follows: Figure 3 As shown. 66 Fe3Ni1Ta1Si15 B 14 ,Co 66 Fe2Ni1Ta2Si 15 B 14 ,Co 66 Fe1Ni1Ta3Si 15 B 14 ,Co 66 Ni1Ta4Si 15 B 14 and Co 66 Ta5Si 15 B 14 Onset crystallization temperature T of cobalt-based metallic glass composites x and crystallization peak temperature T p They are 846K, 854K, 862K, 874K, 885K and 847K, 856K, 865K, 876K, 887K respectively. The data show that the initial crystallization temperatures of these materials are all above 846K, while Co 66 Fe3Ni1Ta1Si 15 B 14 The initial crystallization temperature of the alloy is T x The value is higher than that of traditional common Co-based amorphous alloys such as Co 77.5 Si 13.5 B9 (~792K) is more than 50K higher. This shows that when working below 846K, the new cobalt-based metallic glass can maintain an amorphous structure and can basically meet the requirements of serving in high-temperature environments.
[0059] The MPMS produced by Quantum Design was used to measure the thermomagnetic curve of the sample. The external magnetic field was 70000 Oe, the test temperature range was from room temperature to 800 K, the heating rate was 5 K / min, and the test sample size was 2 mm × 2 mm. The MT curves of the five quenched cobalt-based metallic glass ribbons containing Ta element in Examples 1-5 are shown in Figure 2. Figure 4 As shown. Figure 4 It can be seen that under the same temperature and magnetic field conditions, as the proportion of magnetic elements such as Fe and Ni decreases, the magnetic induction intensity of Ta-containing cobalt-based amorphous alloys gradually decreases, which also leads to a decrease in its Curie temperature. 66 Fe3Ni1Ta1Si 15 B 14 ,Co 66 Fe2Ni1Ta2Si 15 B 14 ,Co 66 Fe1Ni1Ta3Si 15 B 14 ,Co 66 Ni1Ta4Si 15 B14 and Co 66 Ta5Si 15 B 14 The Curie temperatures of cobalt-based metallic glass composites are 750K, 716K, 674K, 640K, and 580K respectively.
[0060] The alloy strips in Examples 1-5 were tested using a HVS-1000A digital automatic turret micro Vickers hardness tester. The results are as follows: Figure 5 As shown, Co 66 Fe3Ta1Ni1Si 15 B 14 ,Co 66 Fe2Ta2Ni1Si 15 B 14 ,Co 66 Fe1Ta3Ni1Si 15 B 14 ,Co 66 Ta4Ni1Si 15 B 14 and Co 66 Ta5Si 15 B 14 The Vickers microhardness of cobalt-based metallic glass composites is 718HV 0.1 ,1073HV 0.1 ,796HV 0.1 ,982HV 0.1 ,1107HV 0.1 . Compared with traditional Fe 80 Compared with Al2B5P9C4 iron-based amorphous alloy strip (~770HV 0.1 ), the hardness of the Ta-containing metallic glass material provided by the present invention is similar to or higher than that of the traditional Fe-based amorphous alloy.
[0061] The corrosion resistance test of the cobalt-based metallic glass composite material was carried out using a Shanghai Chenhua 660E electrochemical workstation, wherein the corrosive solution was a 3.5wt.% NaCl solution simulating the concentration of ocean salt. The potentiodynamic polarization curves of the alloy strips in Examples 1-5 are shown in FIG. Figure 6The test process can be found in the literature (①Cheng JB, Feng Y, Yan C, et al. Development and Characterization of Al-Based Amorphous Coating [J]. JOM, 2020, 72 (3), 745-753. ②HUNG SB, WANG CJ, CHEN YY, et al. Thermal corrosion properties of V-Nb-Mo-Ta-W and V-Nb-Mo-Ta-W-Cr-B high entropy alloy coatings [J]. Surface and Coatings Technology, 2019, 375: 802-809.), and the results are shown in Table 1.
[0062] Table 1 Electrochemical parameters of polarization curve fitting
[0063]
[0064] In Table 1, the self-corrosion current density represents the actual corrosion rate. The smaller the self-corrosion current density, the lower the corrosion degree under the same conditions. The self-corrosion potential represents the corrosion tendency. Under the same conditions, the higher the self-corrosion potential, the lower the corrosion tendency. The larger the polarization resistance, the less likely the material is to corrode. When evaluating the quality of a material, various parameters are considered comprehensively. Among them, the self-corrosion current density can mainly indicate the corrosion resistance of the material. The smaller the corrosion rate, the better the corrosion resistance of the material.
[0065] from Figure 6 As can be seen from Table 1, with the increase of Ta content, the self-corrosion current density of the cobalt-based metallic glass composite material shows a trend of gradual decrease, and the self-corrosion potential of the alloy ranges from -0.566 to -0.623 V. corr =-1.050V, I corr =639.0μA·cm -2 ), 316L stainless steel (E corr =-0.203V, I corr =20.0μA·cm -2 ), the developed cobalt-based metallic glass composite material has a more positive corrosion potential than T10 steel, and a lower current density than T10 steel and 316L stainless steel, indicating that the metallic glass composite material provided in the present application has a lower corrosion tendency and a smaller actual corrosion rate in the corrosive environment of 3.5wt.% NaCl solution, and therefore has a better corrosion resistance.
[0066] It can be seen from the above embodiments that the new cobalt-based metallic glass composite material provided by the present invention has good corrosion resistance, high hardness, strong thermal stability and good thermal magnetic properties, so that it can be used as a raw material for surface protective coatings of large-scale equipment (such as marine ships, key components serving in high-temperature environments in the aerospace field, etc.) that need to have multiple performance characteristics such as corrosion resistance, high hardness, and electromagnetic shielding. At the same time, the raw materials involved in the present invention are all common raw materials in the field, the operating steps are simple and easy, the process is easy to control, and metallic glass materials with uniform composition and outstanding comprehensive performance can be obtained. There is no need to replace all the components of the equipment, but by performing surface protection on the components of major equipment, its service life can be extended and its renewal cost can be reduced, which is more advantageous in terms of economic applicability.
[0067] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A Ta-containing cobalt-based metallic glass composite material, characterized in that: The chemical formula of this metal material is Co 66 Fe x Ni y Ta 5-x-y Si 15 B 14 , where x and y represent atomic fractions, x = 0 to 3, y = 0 to 1; The method for preparing the cobalt-based metallic glass composite material comprises the following steps: 1) weighing the required mass of Co, Fe, Ni, Ta, Si and B raw materials in the form of particles or blocks according to the atomic fraction in the chemical formula of the alloy and performing surface treatment; 2) The prepared raw materials are melted in a vacuum arc furnace with a melting current of 180-270A for 3-5 times to form a master alloy ingot; wherein the vacuum degree in the vacuum arc furnace is 1.0×10 -3 Pa~3.0×10 -3 Pa, by filling with argon gas, repeating the vacuum operation to ensure that there is no impurity gas in the furnace chamber; at the same time, the pressure difference between the belt-spinning machine chamber and the quartz tube is controlled at 0.010~0.040Mpa; 3) crushing the master alloy ingot described in step 2) and placing it in a quartz tube, placing the quartz tube in the induction coil of a vacuum belt spinning machine to melt the master alloy ingot, and after melting, spraying the liquid alloy onto the surface of a high-speed rotating copper roller in the vacuum belt spinning machine to quickly cool it to obtain a cobalt-based metallic glass ribbon; wherein the vacuum degree in the vacuum belt spinning machine is 1.0×10 -3 Pa~3.0×10 -3 Pa; the surface linear velocity of the copper roller is 30-40 m / s.
2. The Ta-containing cobalt-based metallic glass composite material according to claim 2, characterized in that: The surface treatment in step 1) is to mechanically polish the particles or blocks of the raw material to remove the surface oxide skin, and then use acetone or alcohol to perform ultrasonic cleaning for 30 seconds, and repeat the cleaning 1 to 3 times.
3. The Ta-containing cobalt-based metallic glass composite material according to claim 2, characterized in that: The alloy strip has a thickness of 25 to 40 μm and a width of 1.0 to 2.0 mm.
4. Use of the Ta-containing cobalt-based metallic glass composite material according to claim 1 as a raw material for metal structural parts, magnetic components or sensor components, and high-temperature corrosion-resistant metal protective coatings.
Citation Information
Cited By
Ta and Cu synergistically strengthened fine-grain high-toughness soft magnetic stainless steel, profile comprising same and preparation method of profile
CN121428430A