Composite photocatalyst as well as preparation method and application thereof

By constructing a CdS QDs/Ag@AgTaO3 composite photocatalyst combined with wide and narrow bandgap, the problem of slow reaction rate of single-phase semiconductor photocatalysts in catalytic nitrophenol reaction is solved, and efficient photocatalytic performance and stability are achieved, significantly The carrier separation efficiency and catalytic reaction rate are improved.

CN118904358AInactive Publication Date: 2024-11-08河套学院
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411383078.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the photocatalytic reaction, existing single-phase semiconductor photocatalysts have problems such as narrow absorption spectrum, low carrier separation efficiency and poor photo stability, especially in the reduction reaction of pollutants such as catalytic nitrophenol, which is slower in the reaction rate.

Method used

By using the preparation method of composite photocatalyst, the carrier separation efficiency and catalytic performance are improved by constructing a CdS QDs/Ag@AgTaO3 composite that combines wide and narrow band gaps. .

Benefits of technology

The visible light absorption performance and catalytic reaction rate of the photocatalyst are significantly improved, the carrier utilization rate is enhanced, and the efficient reduction of p-nitrophenol is achieved. The catalyst shows stability and repeatability in the cycle test.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904358A_ABST
    Figure CN118904358A_ABST
Patent Text Reader

Abstract

The invention discloses a composite photocatalyst and a preparation method and application thereof, and relates to the technical field of photocatalyst preparation. S1, preparation of an Ag2O precursor; s2, preparation of AgTaO3 is carried out; s3, preparation of CdS QDs (quantum dots); s4, preparation of CdS QDs / AgTaO3 is carried out; and (S5) preparing the CdS QDs / Ag (at) AgTaO3. According to the CdS QDs / Ag-coated AgTaO3 composite photocatalyst disclosed by the invention, by accelerating e-migration, the pe-utilization rate is effectively enhanced, the effect of photo-thermal synergistic promotion of catalytic performance is achieved, and the visible light absorption performance of an AgTaO3 semiconductor is improved. Meanwhile, a cycle test experiment shows that the CdSQDs / Ag-coated AgTaO3 is stable in performance and can be repeatedly used, and the value of the CdSQDs / Ag-coated AgTaO3 in practical application is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalyst preparation, and in particular to a composite photocatalyst and a preparation method and application thereof. Background Art

[0002] Photocatalysis, as a green, safe, low-energy, efficient and environmentally friendly technology, has attracted much attention in recent years. This technology can convert renewable solar energy into high-density chemical energy and be used for pollutant treatment and energy replenishment. Under the induction of photons, photogenerated electrons (PE - ) and photogenerated holes (ph + ). Due to e - Possesses the ability to restore, + It has oxidation ability, and when pollutants adhere to the catalyst surface, corresponding photo-induced oxidation and reduction reactions can occur. Therefore, the light absorption capacity and pe of the semiconductor - With ph + The separation efficiency of photocatalytic reaction is an important factor that determines the rate of photocatalytic reaction. This is also a problem that needs to be solved and a bottleneck that needs to be broken through in the field of semiconductor photocatalysis. Most of the single-phase semiconductors studied so far have narrow absorption spectrum range and PE - and ph + The disadvantages of high recombination rate and poor photostability can be effectively solved by constructing multi-level structure semiconductors. The construction of multi-level structure semiconductors is to combine two or more semiconductors with matching energy bands to form a heterojunction photocatalyst. In principle, the energy difference formed by the composite interface will promote the e - and h + The transfer and separation of the wide bandgap semiconductors can effectively reduce the recombination between them and accelerate the catalytic reaction rate. In particular, when the wide bandgap semiconductor is combined with the narrow bandgap semiconductor with photosensitivity, it can also play the role of sensitizing the wide bandgap material.

[0003] In recent years, quantum dots have become a hot topic in the field of photocatalysis due to their unique photosensitization, photoelectrochemical properties and fast charge transfer characteristics. At present, a large amount of scientific research work is mainly focused on the catalytic performance of II-VI group cadmium-based quantum dot materials, because most cadmium-based quantum dots are direct transition bandgap semiconductors, and the optical absorption range is almost in the visible light band. They are generally combined in an ionic bond manner, are easy to prepare, have high surface activation energy, and show broad application prospects in the field of photocatalysis. In addition, cadmium-based quantum dots such as CdS, CdSe, CdTe and ZnTe, their s orbitals and p orbitals can participate in carrier transport at the same time, so the ground state electrons of this type of material are easily excited and usually have good photoelectrochemical properties. However, due to some inherent characteristics: the quantum dots are small in size and have low crystallinity, the catalyst surface often lacks active sites, and the e generated by light excitation - and h+ The separation path is short, so the photogenerated carriers can easily recombine, resulting in low activity of pure quantum dot catalysts. Through a large number of literature surveys, it can be found that combining quantum dots with other semiconductors to form heterojunctions is a solution to the lack of active sites and the improvement of pe - With ph + It is one of the commonly used strategies to improve separation efficiency, and Group II-VI cadmium-based quantum catalysts also have a good photosensitization effect on wide-bandgap semiconductors.

[0004] In order to improve the visible light absorption properties of silver tantalate and further accelerate its reduction reaction rate of p-nitrophenol, it is very meaningful to develop a composite photocatalyst for catalyzing the reduction of p-nitrophenol by sodium borohydride. Summary of the invention

[0005] In view of the above problems, the present invention provides a composite photocatalyst and a preparation method and application thereof.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: The present invention provides a method for preparing a composite photocatalyst, which specifically comprises the following steps: S1: Preparation of Ag2O precursor: Weigh AgNO3 and NaOH and dissolve them in distilled water respectively, and continue to stir until they are evenly mixed to obtain AgNO3 solution and NaOH solution respectively; then add the NaOH solution dropwise into the AgNO3 solution to form a dark brown suspension, and then age the suspension at 25°C, filter and wash it with distilled water until it is neutral, and dry it at 60°C in a vacuum oven to obtain Ag2O; S2: Preparation of AgTaO3: Accurately weigh Ag2O and Ta2O5 and dissolve them in anhydrous ethanol. Grind them with an agate mortar and pestle until the ethanol is completely volatilized to obtain a mixture. Keep the mixture at 800℃ and 1000℃ for 1h and 5h respectively at a constant heating rate. After the reaction is completed, cool it naturally to room temperature, wash it with dilute nitric acid and a large amount of distilled water, and finally dry it in an oven at 60℃ overnight to obtain AgTaO3. S3: Preparation of CdS QDs: Anhydrous CdCl2 and thioglycolic acid solution were added to distilled water and mixed evenly, and the pH was adjusted to 10.0 with NaOH, then transferred to a three-necked flask, and Na2S·9H2O was added, and heated continuously in an oil bath; finally, washed with distilled water and anhydrous ethanol, and dried to obtain a CdS QDs sample, recorded as TCQ; S4: Preparation of CdS QDs / AgTaO3: Weigh AgTaO3 solid in a beaker, add CdS QDs, then add distilled water, stir at room temperature to obtain a mixture, and dry; pour the dried mixture into an agate jar, and add 4 agate balls with a size of Φ10 and 10 agate balls with a size of Φ6; use high-energy ball milling assisted technology to obtain CdS QDs / AgTaO3 uniformly loaded with CdS, recorded as TCQ / AgTaO3; S5: Preparation of CdS QDs / Ag@AgTaO3: CdS QDs / AgTaO3 reacts with NaBH4 to form a mixed solution, which is washed with distilled water and dried to obtain CdS QDs / Ag@AgTaO3, recorded as TCQ / Ag@AgTaO3.

[0007] Furthermore, in step S1, the mass of AgNO3 is 4.62 g, the mass of NaOH is 1.5 g, the volume of distilled water is 50 mL, and the aging time is 24 h.

[0008] Furthermore, in step S2, the mass of Ag2O is 0.0927 g, the mass of Ta2O5 is 0.1768 g, the volume of anhydrous ethanol is 8 mL, and the heating rate is 5°C / min.

[0009] Furthermore, in step S3, the molar amount of anhydrous CdCl2 is 0.2mmol, the volume of thioglycolic acid solution is 150μL, the volume of distilled water is 100mL; the NaOH concentration is 1.0M; the molar amount of Na2S·9H2O is 0.6mmol; the oil bath temperature is 100°C, the continuous heating time is 2h; and the drying temperature is 60°C.

[0010] Furthermore, in step S4, the mass of AgTaO3 solid is 1 g; the mass fraction of CdS QDs is 1.0%~10%; the volume of distilled water is 50 mL, the stirring time is 12 h; the ball mill speed is 500 r / min, and the ball milling time is 0.5 h.

[0011] Furthermore, in step S5, the concentration of NaBH4 is 0.5M.

[0012] The present invention also provides a composite photocatalyst prepared by the composite photocatalyst preparation method.

[0013] The present invention also provides an application of the composite photocatalyst in catalyzing the reduction of p-nitrophenol by sodium borohydride.

[0014] Compared with the prior art, the present invention has the following beneficial effects: In the present invention, a wide-narrow bandgap combined CdS QDs / Ag@AgTaO3 composite photocatalyst is prepared by in-situ reduction and heterojunction construction, supplemented by high-energy ball milling technology. The two semiconductors are fully mixed and contacted in a short time by the high-speed operation of the ball mill and the strong impact force on the ball mill wall, which effectively improves the dispersion ability and bonding strength of the supported catalyst. At the same time, the unique crushing function makes the semiconductor have a more uniform particle size. The CdSQDs / Ag@AgTaO3 composite photocatalyst of the present invention accelerates e - Migration, effectively enhancing pe - The utilization rate is improved, achieving the effect of photothermal synergy to promote catalytic performance and improving the visible light absorption performance of AgTaO3 semiconductor. At the same time, the cycle test experiment shows that CdSQDs / Ag@AgTaO3 has stable performance and can be reused, which improves its value in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 is the XRD spectra of TCQ, Ag / TCQ, AgTaO3, xTCQ / AgTaO3, and xTCQ / Ag@AgTaO3 in the embodiments of the present invention (x=1.0, 2.5, 5.0, 7.5, 10); wherein, Figure 1 ab are XRD spectra of TCQ, Ag / TCQ, AgTaO3, and xTCQ / AgTaO3; Figure 1 cd is the XRD spectrum of xTCQ / Ag@AgTaO3; Figure 2 is a characterization diagram of AgTaO3, BM-AgTaO3, TCQ, and 5TCQ / Ag@AgTaO3 in the embodiment of the present invention; wherein, Figure 2 a is the SEM image of AgTaO3; Figure 2 b is the SEM image of BM-AgTaO3; Figure 2 cd are the TEM and HRTEM images of TCQ, respectively; Figure 2 ef are TEM and HRTEM images of 5TCQ / Ag@AgTaO3, respectively; Figure 3 is an elemental surface scan of 5TCQ / Ag@AgTaO3 in the embodiment of the present invention; wherein, Figure 3 a is the elemental scan of 5TCQ / Ag@AgTaO3; Figure 3 b is the element distribution diagram of Ag; Figure 3 c is the element distribution diagram of Ta; Figure 3 d is the element distribution diagram of O; Figure 3 e is the element distribution diagram of Cd; Figure 3 f is the element distribution diagram of S; Figure 4is the XPS spectrum of Example 5TCQ / Ag@AgTaO3 of the present invention; wherein, Figure 4 a is the full score; Figure 4 b is the XPS spectrum of Ag 3d; Figure 4 c is the XPS spectrum of Ta 4f; Figure 4 d is the XPS spectrum of O 1s; Figure 4 e is the XPS spectrum of Cd 3d; Figure 4 f is the XPS spectrum of S 2p; Figure 5 are the optical performance test results of TCQ, AgTaO3, and xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) in the embodiments of the present invention; wherein, Figure 5 a is the UV-visible diffuse reflectance graph of TCQ, AgTaO3, xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10); Figure 5 b is the calculation diagram of the band gap values ​​of TCQ and AgTaO3; Figure 6 is the p-nitrophenol (p-NP) reduction rate diagram of the present invention; wherein, Figure 6 a is a comparison chart of the catalytic performance effects of the p-NP-catalyst system and the p-NP-NaBH4 system; Figure 6 b is a comparison of the catalytic reduction of p-NP by Ag@AgTaO3, Ag@TCQ and 5TCQ / Ag@AgTaO3 under no light irradiation; Figure 6 c is the conversion rate diagram of xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) catalytic reduction of p-NP to p-AP in the absence of light; Figure 6 d is the kinetic curve fitting diagram of xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10); Figure 7 middle, Figure 7 ae is the UV-visible absorption spectrum of p-NP pollutants with the same concentration of NaBH4 (0.5M) and the same amount of 5TCQ / Ag@AgTaO3 when the initial concentration of p-NP increases from 0.01M to 0.05M; Figure 7 f is the p-NP degradation rate diagram under different NaBH4 concentrations; Figure 8 middle, Figure 8 a is the reaction rate diagram of the composite sample 5TCQ / Ag@AgTaO3 reducing p-NP under visible light; Figure 8 b is the conversion efficiency of Ag@AgTaO3 and 5TCQ / Ag@AgTaO3 for p-NPs of different concentrations within 2 min under no light and visible light irradiation; Fig. 9 This is a cyclic experimental diagram of the composite material 5TCQ / Ag@AgTaO3 of the present invention for reducing p-NP; wherein, Fig. 9 a is a graph showing the stability cycle test of p-NP reduction of 5TCQ / Ag@AgTaO3 under no light irradiation conditions; Fig. 9 b is the stability cycle test diagram of 5TCQ / Ag@AgTaO3 reducing p-NP under visible light irradiation; Fig.10 middle, Fig.10 a is the impedance test graph of AgTaO3, TCQ, xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10); Fig.10 b is the impedance test curve of xTCQ / Ag@AgTaO3 (x=5.0, 7.5, 10); Fig.10 c is the photocurrent diagram of TCQ, AgTaO3 and xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10); Fig.10 d is the Mott-Schottky plot of TCQ and AgTaO3; Fig.11 is the photoelectron valence band energy spectrum of the present invention; wherein, Fig.11 a is the photoelectron valence band spectrum of TCQ; Fig.11 b is the photoelectron valence band spectrum of AgTaO3; Fig.12 middle, Fig.12 ac are the work function calculation diagrams of TCQ, AgTaO3 and Ag respectively; Fig.12 d is the electron flow path diagram between TCQ, AgTaO3 and Ag; Fig.13 It is the interfacial electron transfer direction of the three-phase composite material 5TCQ / Ag@AgTaO3 of the present invention under the conditions of no light (a) and visible light irradiation (b). DETAILED DESCRIPTION

[0016] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0017] The instruments, reagents, materials, etc. involved in the following examples, unless otherwise specified, are all conventional instruments, reagents, materials, etc. in the prior art and can be obtained through regular commercial channels. The experimental methods, detection methods, etc. involved in the following examples, unless otherwise specified, are all conventional experimental methods, detection methods, etc. in the prior art.

[0018] Example 1 This embodiment provides a composite photocatalyst, and the preparation method thereof specifically comprises the following steps: S1: Preparation of Ag2O precursor: Weigh 4.62g AgNO3 and 1.5g NaOH and dissolve them in 50mL distilled water respectively, and stir them continuously until they are evenly mixed to obtain AgNO3 solution and NaOH solution respectively; then add the NaOH solution dropwise into the AgNO3 solution to form a dark brown suspension, and then age the suspension at 25°C for 24h, filter and wash with distilled water until it is neutral, and dry it in vacuum at 60°C to obtain Ag2O; S2: Preparation of AgTaO3: Accurately weigh 0.0927g Ag2O and 0.1768g Ta2O5 and dissolve them in 8mL anhydrous ethanol, grind them with an agate mortar and pestle until the ethanol is completely volatilized to obtain a mixture; keep the mixture at 800℃ and 1000℃ for 1h and 5h respectively at a heating rate of 5℃ / min, cool it naturally to room temperature after the reaction is completed, wash it with dilute nitric acid and a large amount of distilled water, and finally dry it in an oven at 60℃ overnight to obtain AgTaO3; S3: Preparation of CdS QDs: 0.2mmol anhydrous CdCl2 and 150μL thioglycolic acid solution were added to 100mL distilled water and mixed evenly, and the pH was adjusted to 10.0 with 1.0M NaOH, then transferred to a three-necked flask, 0.6mmol Na2S·9H2O was added, and heated in a 100℃ oil bath for 2h; finally, washed with distilled water and anhydrous ethanol, and dried at 60℃ to obtain a CdS QDs sample, recorded as TCQ; S4: Preparation of CdS QDs / AgTaO3: Weigh 1g of AgTaO3 solid in a beaker, add TCQ at a mass fraction of 1.0%, then add 50mL of distilled water, stir at room temperature for 12h to obtain a mixture, and dry it; pour the dried mixture into an agate jar, and add 4 agate balls with a specification of Φ10 and 10 agate balls with a specification of Φ6; use high-energy ball milling assisted technology (speed of 500r / min, time of 0.5h) to obtain CdS QDs / AgTaO3 uniformly loaded with TCQ, recorded as 1.0TCQ / AgTaO3; S5: Preparation of CdS QDs / Ag@AgTaO3: CdS QDs / AgTaO3 reacts with 0.5MNaBH4 during the reduction of p-nitrophenol to form a mixed solution, and the mixed solution is washed with distilled water and dried to obtain CdS QDs / Ag@AgTaO3 (elemental silver is in situ grown on CdS QDs / AgTaO3), recorded as 1.0TCQ / Ag@AgTaO3.

[0019] Example 2 The difference from Example 1 is that in step S4, TCQ is added at a mass fraction of 2.5% to obtain 2.5TCQ / AgTaO3; and in step S5, 2.5TCQ / Ag@AgTaO3 is obtained.

[0020] Example 3 The difference from Example 1 is that TCQ is added at a mass fraction of 5.0% in step S4 to obtain 5.0TCQ / AgTaO3; and 5.0TCQ / Ag@AgTaO3 is obtained in step S5.

[0021] Example 4 The difference from Example 1 is that in step S4, TCQ is added at a mass fraction of 7.5% to obtain 7.5TCQ / AgTaO3; and in step S5, 7.5TCQ / Ag@AgTaO3 is obtained.

[0022] Example 5 The difference from Example 1 is that in step S4, TCQ is added at a mass fraction of 10% to obtain 10TCQ / AgTaO3; and in step S5, 10TCQ / Ag@AgTaO3 is obtained.

[0023] Comparative Example 1 TCQ, preparation method is the same as step S3 of Example 1.

[0024] Comparative Example 2 AgTaO3, preparation method is the same as step S2 of Example 1.

[0025] Comparative Example 3 BM-AgTaO3, the preparation method is as follows: weigh 1g AgTaO3 solid into a beaker, add 50mL distilled water, and stir at room temperature for 12h; pour the dried mixture into an agate jar, and add 4 agate balls with a specification of Φ10 and 10 agate balls with a specification of Φ6; use high-energy ball milling assisted technology (speed of 500r / min, time of 0.5h) to obtain BM-AgTaO3.

[0026] Comparative Example 4 CdS QDs / Ag (Ag / TCQ) was prepared by ultrasonically dispersing 50 mg of TCQ solid powder in a quartz tube containing 50 mL of distilled water, adding 5% AgNO3 by mass, reacting under a 500 W xenon lamp for 0.5 h, washing with deionized water, and drying at 60 °C to obtain CdS QDs / Ag, recorded as Ag / TCQ.

[0027] Comparative Example 5 Ag@AgTaO3, the preparation method is: 0.1g / L AgTaO3 and 0.5M NaBH4 directly react to form a mixed solution, the mixed solution is washed with distilled water and dried to obtain an in-situ generated Ag@AgTaO3 composite.

[0028] The materials of the above embodiments and comparative examples were tested as follows: 1. Structure and morphology of photocatalysts (1) XRD detection XRD detection was performed on xTCQ / AgTaO3, xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) prepared in Examples 1-5, TCQ in Comparative Example 1, AgTaO3 in Comparative Example 2, and Ag / TCQ in Comparative Example 4.

[0029] Figure 1 ab are the XRD spectra of AgTaO3 and xTCQ / AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) samples. It can be seen that after adding different amounts of TCQ in the high-energy ball milling-assisted preparation process, the characteristic diffraction peaks of the composite TCQ / AgTaO3 remain consistent with AgTaO3 without deviation, and no other impurity peaks appear. Figure 1 a It can be clearly seen that the diffraction peak intensity of 5TCQ / AgTaO3 is lower than that of AgTaO3, which may be due to the pulverization of the sample during the ball milling process, resulting in a decrease in the crystallinity of the composite sample. There are three reasons why the TCQ crystal diffraction peak is covered by AgTaO3: (1) The particle size difference between TCQ and AgTaO3 is too large; (2) The loading content of TCQ is very low; (3) The dispersion of TCQ on AgTaO3 is high. On the other hand, it also shows that the crystal structure of AgTaO3 has not changed due to ball milling or combination with TCQ.

[0030] Figure 1 cd is the XRD spectrum of the xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) three-phase composite. In addition to the newly discovered diffraction peak of elemental Ag that is consistent with the data of the standard card JCPDS 087-0718, the other signal peaks are consistent with the AgTaO3 sample without any deviation, indicating that the crystal structure of AgTaO3 has not changed, which also indirectly indicates that its structure is relatively stable. In addition, no diffraction peak of TCQ was found in the xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) composite sample, indicating that the reduction process of elemental Ag did not change the structure of the catalyst. Figure 1 In d, it can be found that the diffraction peak intensity of silver element is very low, which may be due to the high dispersion of Ag element on AgTaO3.

[0031] (2) Structural characterization In order to have a deep understanding of the composition and morphology of the composite samples, AgTaO3, BM-AgTaO3, TCQ and 5TCQ / Ag@AgTaO3 composite samples were characterized by SEM, TEM and HRTEM.

[0032] contrast Figure 2 a (AgTaO3) and Figure 2 b (BM-AgTaO3) It can be clearly seen that the grain size of BM-AgTaO3 treated by high-energy ball milling technology is significantly reduced compared with that of untreated AgTaO3. The reason is that the strong impact of the ball mill (agate ball) and the inner wall of the ball mill on the catalyst breaks up the larger blocks of AgTaO3, and the XRD diffraction results also confirm this conclusion. In principle, ball milling technology treatment will reduce the particle size of BM-AgTaO3 samples, which is conducive to the uniform loading of TCQ samples.

[0033] Figure 2 c is the TEM image of TCQ, which shows that TCQ is composed of highly uniformly dispersed small grains. Figure 2 d), it can be further confirmed that the particle size of TCQ is about 5nm, and the (1 1 1) plane with a lattice spacing of 0.332nm is preferentially exposed. Compared with the BM-AgTaO3 sample with a particle size between 500nm and 1μm, the two have a large size difference, so no diffraction peak of TCQ is observed in the XRD pattern of the composite sample.

[0034] Figure 2 e is the TEM image of the three-phase composite sample 5TCQ / Ag@AgTaO3. It can be seen that there are many TCQ and Ag particles loaded on the BM-AgTaO3 sample. The slightly larger ones are Ag particles, and the slightly smaller ones are TCQ quantum dots. From the inset in the upper left corner, it can be seen that the size of the metal Ag is about 10nm. Observe carefully Figure 2 f It can be found that there are three obviously different lattice fringes in the HRTEM image of the 5TCQ / Ag@AgTaO3 sample. After processing with Digital Micrograph software, d=0.237nm, d=0.278nm and d=0.332nm were obtained, which correspond to Ag (1 1 1), AgTaO3 (1 0 4) and TCQ (1 1 1) crystal planes, respectively, which strongly confirms the formation of 5TCQ / Ag@AgTaO3.

[0035] (3) Element surface scanning test An elemental surface scanning test was performed on 5TCQ / Ag@AgTaO3. The elemental surface scanning test can intuitively show the distribution of each element in each area.

[0036] from Figure 3 It can be seen that the composite material 5TCQ / Ag@AgTaO3 mainly contains Ag, Ta, O, Cd, and S, and all elements are evenly distributed on the sample. From the concentrated areas of the bright spots in the figure, it can be determined that the main substances present are mainly Ag, Ta and O ( Figure 3 bd), Cd and S followed ( Figure 3 ef), further indicating that the content of TCQ in the composite sample is relatively low. Figure 3 The element distribution diagram of Cd and S in ef shows that TCQ is highly dispersed on the surface of AgTaO3. High-energy ball milling allows TCQ and AgTaO3 to effectively contact and combine. At the same time, the strong impact between the ball milling beads and the ball milling jar is used to efficiently crush the AgTaO3 sample, exposing more of its surface, providing more loading space and sites for the TCQ sample, and effectively improving the composite efficiency of the two materials. The element mapping test once again strongly confirmed the successful preparation of the 5TCQ / Ag@AgTaO3 composite material.

[0037] 2. Chemical composition and valence state analysis (XPS analysis) The surface structure and chemical valence of semiconductors have a great influence on the performance of catalytic reactions, because all catalytic reactions occur on the surface of semiconductors. XPS, as an important surface analysis technique, can provide rich information such as elemental composition, atomic valence and molecular structure for chemical reactions. Based on this, XPS analysis of 5TCQ / Ag@AgTaO3 was performed.

[0038] like Figure 4 As shown in a, in the XPS spectrum of 5TCQ / Ag@AgTaO3, in addition to the same Ag, Ta, and O as AgTaO3, Cd and S also exist, proving that TCQ and AgTaO3 are successfully compounded. C (284.6 eV) is an impurity element introduced during the test to correct the test errors caused by the instrument and environment. Figure 4 b shows that in the 5TCQ / Ag@AgTaO3 composite, monovalent Ag + It coexists with zero-valent Ag, and a group of diffraction peaks at 373.6 eV and 367.6 eV are assigned to Ag. + 3d 3 / 2 and Ag + 3d 5 / 2 , another set of diffraction peaks at 374.5 eV and 368.5 eV are related to Ag 0 3d 3 / 2 and Ag 0 3d 5 / 2 Corresponding. Figure 4In c, the XPS spectrum of Ta 4f is a set of double peaks with binding energies at 27.50 eV and 25.65 eV, which correspond to Ta 5+ 4f 5 / 2 and Ta 5+ 4f 7 / 2 The O 1s is fitted into three diffraction peaks located at 530.2 eV, 531.7 eV and 532.5 eV respectively ( Figure 4 d), which are identified as lattice oxygen, surface adsorbed hydroxyl oxygen and defect oxygen according to the position of binding energy. In addition, the high-resolution XPS spectrum of Cd 3d was obtained from the XPS spectrum of 5TCQ / Ag@AgTaO3 sample. Figure 4 e shows that the signal peaks of Cd appear at binding energies of 411.35 eV and 404.6 eV, corresponding to Cd 2+ 3d 3 / 2 and Cd 2+ 3d 5 / 2 .exist Figure 4 In the S2pXPS spectrum of f, S exists in two states, namely the SO bond at 162.3 eV and the S-Cd bond at 161.1 eV.

[0039] 3. Optical performance The size of the semiconductor band gap is one of the key factors that determine the efficiency of photocatalytic reactions. Figure 5 As shown in Figure a, the light absorption of AgTaO3 is mainly concentrated in the ultraviolet range of 200 nm-365 nm, and the absorption band of TCQ can extend to 600 nm. When AgTaO3 and TCQ are combined by high-energy ball milling and form a three-phase complex with the in-situ reduced metal Ag, a new absorption band appears between 400 nm and 550 nm in the absorption spectrum, and the tail band absorption of the complex extends to after 800 nm. It can be seen that as the TCQ loading increases, the light absorption capacity of the complex gradually increases, indicating that the photosensitization of TCQ is the main reason for the increase in the intensity of the UV-visible diffuse reflectance absorption spectrum of the composite sample. Figure 5 b is the tauc diagram of AgTaO3 and TCQ. Since they are both direct transition semiconductors, the band gap value can be calculated by the formula αhν=A(hν-E g ) 2 In the formula, α and ν represent the absorption coefficient and the incident light frequency, respectively. h and A are Planck constants and physical constants related to material properties. E g is the band gap energy value to be calculated. Use (αhν) 2 By plotting against hν and using the linear extrapolation method, the band gap values ​​of AgTaO3 and TCQ are obtained to be 2.42 eV and 3.40 eV, respectively.

[0040] 4. Photocatalytic performance Catalytic reduction of p-nitrophenol test: In order to investigate the visible light catalytic activity of the prepared composite, this experiment selected excess NaBH4 as a hydrogen source to reduce p-nitrophenol (p-NP) as a model reaction to study the relationship between xTCQ / Ag@AgTaO3 photocatalytic material and reduction rate. The specific experimental contents are as follows: First, 0.5M NaBH4 was added to 50mL of an aqueous solution containing 5mg of the catalyst and mixed and stirred for 10min. Then 0.3mL of p-NP of different concentrations (0.01M-0.05M) was added to the above mixed solution, and the results were immediately measured and recorded on a UV-visible spectrophotometer at regular time intervals. The cyclic test is to wash and centrifuge the used catalyst, dry it, and use it in the next experiment.

[0041] Figure 6 a is a comparison of the catalytic performance of adding 0.03 M p-nitrophenol (p-NP) and catalyst 5TCQ / Ag@AgTaO3 and adding 0.03 M p-NP and 0.5 M NaBH4, and the inset is the UV-visible absorption spectrum of the corresponding reaction. Obviously, in the reduction reaction without adding catalyst or NaBH4, the concentration of p-NP hardly changes, indicating that NaBH4 and catalyst are important substances that induce the reaction. Figure 6 b is the ability of Ag / TCQ, Ag@AgTaO3 and 5TCQ / Ag@AgTaO3 to catalytically reduce p-NP in the absence of light. It can be found that the photocatalytic activity of the three-phase composite material 5TCQ / Ag@AgTaO3 is significantly improved compared with the two-phase composites Ag@AgTaO3 and Ag@TCQ. The experimental results show that 0.03 M p-NP can be completely reduced to p-aminophenol (p-AP) within only 8 minutes, which is 34% and 76% higher than the rates of Ag@AgTaO3 and Ag@TCQ under the same experimental conditions, respectively. Figure 6 c is the conversion rate diagram of the catalytic reduction of p-NP to p-AP in the absence of light by the prepared three-phase composite sample, among which the TCQ / Ag@AgTaO3 composite sample with a TCQ loading mass fraction of 5% has the highest catalytic reduction activity. When the TCQ content in the composite is increased again, the conversion rate of p-NP decreases instead. This phenomenon shows that excessive crystal interface effects will hinder the e - migration and separation, thus significantly reducing the catalytic performance of the composite material. Figure 6d is the kinetic fitting curve of the three-phase composite sample. Due to the excessive use of NaBH4, the reaction is regarded as a pseudo-first-order kinetic model determined by a single factor. The results show that the fitting value is highly consistent with the pseudo-first-order kinetic equation. The kinetic degradation rate fitting constants k of the composite material xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10) are 0.2362, 0.3266, 0.5663, 0.2772 and 0.09017 min, respectively. -1 .

[0042] In order to achieve a more efficient and economical catalytic reduction of p-NP, this experiment investigated the catalytic reduction activity of 5TCQ / Ag@AgTaO3 composite with the optimal loading ratio for p-NP pollutants with different concentrations. Figure 7 ae is the UV-visible absorption spectrum of p-NP pollutants with the same concentration of NaBH4 (0.5M) and the same amount of 5TCQ / Ag@AgTaO3 when the initial concentration of p-NP increases from 0.01 M to 0.05 M. Obviously, as the concentration of p-NP increases, the UV-visible absorption intensity of the catalytic system gradually increases. When the corresponding p-NP concentrations are 0.01M, 0.02M, 0.03M, 0.04M and 0.05M, the time for 5TCQ / Ag@AgTaO3 to catalytically reduce and remove p-NP is 6min, 8min, 11min, 16min and 23min respectively. From the experimental results, the composite with the best ratio has a good removal effect on p-NP pollutants of different concentrations. However, it is obvious that when the concentration of pollutants in the solution increases, the catalytic activity of the composite material is significantly suppressed. This is because when the amount of catalyst is constant, the amount of active substances produced under the same experimental conditions is fixed. As the concentration of reactants in the solution increases, the p-NP pollutants in the catalytic system will compete with the limited reactive species, resulting in insufficient reactions, which is manifested as a decrease in the reaction rate. In this process, in addition to considering the relationship between the amount of catalyst and the concentration of reactants (p-NP) and the reaction rate, NaBH4 is also an important factor that cannot be ignored in triggering the reaction. It can be seen that in the p-NP reduction system without NaBH4, the rate of the catalytic reaction is almost zero ( Figure 6 a), however, the large-scale use of NaBH4 will cause harm to the water environment, so the reasonable exploration of the minimum amount of NaBH4 used to trigger this reaction is of great significance to the practical application of this study. Figure 7 f It can be found that with the change of NaBH4 dosage, the reaction activity gradually increases, indicating that in the hydrogenation catalytic reduction of p-NP experiment, NaBH4 not only provides hydrogen protons for the reaction, but also acts as e -The role of the carrier. Since the electronegativity of B is smaller than that of H, the hydrogen in NaBH4 carries a partial negative charge. When the solution contains p-NP, the e - The negative hydrogen will attack the positively charged nitro nitrogen in p-NP, quickly reducing p-NP to p-AP. - When the carrier (NaBH4) decreases, the rate of the catalytic reaction will naturally slow down. However, when the concentration of NaBH4 is too high, the increase in the catalytic reaction rate is not obvious, because the active sites involved in the reaction will be covered by too much adsorbed NaBH4.

[0043] Figure 8 a is the reaction rate diagram of 5TCQ / Ag@AgTaO3 reducing p-NP with different concentrations (0.01 M~0.05 M) under visible light. It can be found that when the catalyst dosage (0.1 g·L −1 When the concentration of TCQ / Ag@AgTaO3 and NaBH4 concentration (0.5 M) are constant, the time for 5TCQ / Ag@AgTaO3 to reduce 0.01 M, 0.02 M, 0.03 M, 0.04 M and 0.05 M p-NP is increased to 2 min, 3 min, 4.5 min, 7 min and 15 min respectively, which is 20%~40% higher than the rate under no light conditions. This experimental phenomenon shows that TCQ can improve the visible light catalytic activity of AgTaO3 and further accelerate the catalytic reduction rate of p-NP with the help of light synergy. Figure 8 b is a bar graph of the conversion efficiency of Ag@AgTaO3 and 5TCQ / Ag@AgTaO3 within 2 min of reaction under lightless and visible light (λ≧420 nm). It can be found that the photocatalytic performance of Ag@AgTaO3 has hardly been improved, mainly due to its weak visible light absorption capacity and inability to effectively utilize the wide range of visible light in sunlight. It is worth noting that compared with the lightless condition, the performance of 5TCQ / Ag@AgTaO3 in reducing 0.01M p-NP under visible light increased by 40% within 2 min, indicating that the composite material can not only effectively improve the efficiency of catalytic reduction of p-NP, but also enhance the visible light absorption capacity of wide-bandgap AgTaO3, realizing the photothermal synergy to accelerate the catalytic reaction.

[0044] In addition, catalyst stability is usually also considered as a major item in practical evaluation. Fig. 9 a is the effect diagram of 5TCQ / Ag@AgTaO3 after 10 cycles of p-NP reduction under lightless conditions. It can be found that the catalytic performance has not changed significantly, indicating that 5TCQ / Ag@AgTaO3 has not changed in the catalytic reaction and has excellent thermal catalytic stability. Fig. 9b is the stability cycle test diagram of 5TCQ / Ag@AgTaO3 reducing p-NP under visible light irradiation. Compared with the thermal reaction without light irradiation, the conversion efficiency of p-NP decreased slightly to about 3.7% after 8 cycles. This may be due to the pH generated by TCQ after light irradiation. + The sulfur itself was oxidized, resulting in a decrease in the photocatalytic performance of 5TCQ / Ag@AgTaO3.

[0045] 5. Study on the photocatalytic mechanism In semiconductor photocatalytic reactions, the migration and separation rates of carriers are important factors that affect the photocatalytic reaction rate after light absorption. In order to clarify the reasons for the improved photocatalytic activity of the three-phase composite sample, electrochemical impedance spectroscopy and transient photocurrent tests were used to verify their relationship with the photocatalytic activity. Fig.10 As shown in a, in the impedance test of the three-electrode system, the curvature radius of all composite samples is smaller than that of a single semiconductor, indicating that TCQ-modified Ag@AgTaO3 can effectively accelerate the migration rate of carriers, reduce the interfacial charge transport barrier, and promote e - and h + Separation. Fig.10 b shows that the 5TCQ / Ag@AgTaO3 composite material has the smallest curvature radius compared to other catalysts, which is consistent with the activity test results of the sample, indicating that the migration and separation rate of carriers are closely related to and proportional to the performance of the catalytic reaction. Generally, the photocurrent density under light and dark environments can well characterize the sample's response to light and pe - With ph + separation situation. Fig.10 c is the photocurrent diagram of TCQ, AgTaO3 and xTCQ / Ag@AgTaO3 (x=1.0, 2.5, 5.0, 7.5, 10). It can be found that 5TCQ / Ag@AgTaO3 has the highest photoexcitation current density, indicating that its pe - and ph + The above experimental data strongly illustrate two points: (1) pe - and ph + The separation rate is not completely related to the light absorption performance. For example, although the 10TCQ / Ag@AgTaO3 composite material has the strongest visible light absorption performance, the excessive crystal interface effect seriously hinders the e - Rapid migration, so that it can be completed in a limited time - and h + The rapid recombination caused by the Coulomb electrostatic force leads to the effective e - The number is decreasing. (2)e - Migration rate can indirectly determine pe - and ph+ The separation rate, and pe - and ph + The separation rate of pe can directly determine the photocatalytic reaction rate. - and ph + The recombination speed is very fast. Usually, in the absence of external field, the diffusion speeds of the two are not the same. The faster e - The migration speed means that there are more active e - , thus having a higher chance of escaping h + Attraction. - and h + Generally speaking, they are active species that directly participate in the reaction, and the number of them can directly determine the activity of the catalytic reaction. In addition, the CB potential of the semiconductor is also one of the key factors that determine its reducing properties, which determines the activity of the photocatalytic reaction to a certain extent. Clarifying the energy band potential of the semiconductor is of great significance for the study of the photocatalytic mechanism. According to the Mott-Schottky test, accurate information about the value of the semiconductor flat band potential can be obtained, and the energy band position of the semiconductor can be directly calculated in combination with the UV-visible diffuse reflectance spectrum. Fig.10 d is the Mott-Schottky curve of TCQ and AgTaO3. The positive slope in the figure shows that both TCQ and AgTaO3 are n-type semiconductors. Therefore, the CB potential of the semiconductor can be inferred based on the experimentally measured values. Usually, affected by the surface state of the semiconductor electrode, the experimentally measured flat band potential value will be 0.1 V~0.2 V lower than the CB potential value. Therefore, the flat band potential values ​​of TCQ and AgTaO3 can be inferred to be -0.88 V and -0.70 V, respectively. Figure 5 The bandgap width value of b can be obtained that the VB potentials of TCQ and AgTaO3 are 1.54 V and 2.7 V, respectively.

[0046] Although we have a comprehensive understanding of the energy band potential of TCQ and AgTaO3 through electrochemical Mott-Schottky tests and band gap value calculations, we still cannot make an accurate judgment on the charge transfer mode and relationship between TCQ, Ag and AgTaO3. According to the viewpoint of solid-state physics, the Fermi level of composite semiconductors plays a decisive role in the structure of heterojunction type and the migration mode of carriers. When two substances with different Fermi levels come into contact with each other, they are affected by the distribution and concentration of carriers. -It will spontaneously move from a high energy level to a low energy level. For composite semiconductors, clarifying the role of each component in the photocatalytic reaction is extremely important for the exploration of the photocatalytic mechanism and the construction of efficient composite photocatalysts. In order to have a more accurate insight and a deeper understanding of the photocatalytic mechanism of TCQ / Ag@AgTaO3, the valence band photoelectron spectroscopy (VBXPS) of semiconductors TCQ and AgTaO3 was performed. According to the physical meaning of the VBXPS curve, it indicates that the semiconductor VB ground state e - The relative relationship between the position and the Fermi level, so the Fermi level value is equal to the valence band value (E V ) minus the VBXPS value. Fig.11 a and Fig.11 As shown in (b), the VBXPS tangent values ​​of TCQ and AgTaO3 are 1.4 eV and 2.75 eV, respectively. Combined with their VB energy level positions, it can be inferred that the corresponding Fermi levels are 0.14 eV and -0.05 eV, respectively.

[0047] As we all know, DFT is of great significance for estimating the system energy, band structure, charge transfer and work function value of semiconductors, especially the electronic structure of materials, work function or energy changes of reaction systems obtained through CASTEP calculations. Although there is a certain deviation between the theoretical calculation results and the experimental values, DFT can give relatively accurate results in most cases. This information is helpful for us to deeply understand the electronic structure of semiconductors, the distribution of carriers and the migration laws between the interfaces of complexes, and has guiding significance for the construction of efficient composite photocatalysts and in-depth exploration of the mechanism of photocatalysis. According to the viewpoint of solid state physics, the size of the work function value of a substance indicates the value of e - Break free from the constraints of the nucleus and become free - Minimum energy required. Fig.12 a, b and c are the work function calculation diagrams of TCQ, AgTaO3 and Ag respectively. From the DFT results, the work function of TCQ (1 1 1) crystal plane is 3.543 eV, the work function of AgTaO3 (1 0 4) crystal plane is 2.974 eV, and the work function of metal Ag (11 1) crystal plane is 3.460 eV. By comparing the calculation results, it is obvious that the work function values ​​of TCQ and Ag are relatively close, with a difference of only 0.083 eV, indicating that the Fermi levels of the two are also very close. Therefore, when the two come into contact with each other, the interface e - The driving force of migration is insufficient, which is manifested as slow carrier migration rate and low photocatalytic reaction activity, which successfully explains why TCQ is not very active after loading metal Ag. For the convenience of explanation and comparison, we convert the potential of the vacuum energy level to the standard hydrogen electrode potential. According to the empirical formula E eV =-4.5-E sV (Where EeV Represents the vacuum energy level potential value, E sV represents the standard hydrogen electrode potential), as well as the conversion relationship between the work function value and the Fermi level, it can be inferred that the Fermi level values ​​of TCQ, AgTaO3 and Ag are -0.96 eV, -1.53 ​​eV and -1.04 eV respectively. Fig.12 d is the Fermi level relationship diagram of various substances calculated based on the DFT calculation results. It can be found that the highest value of AgTaO3 is -1.53 ​​eV, and the values ​​of TCQ and metal Ag are comparable. When TCQ, Ag and AgTaO3 are in contact, e - It will transfer from AgTaO3 to TCQ and metal Ag until their Fermi levels converge to reach thermodynamic equilibrium. At this time, AgTaO3 is positively charged, while metal Ag and TCQ are negatively charged. Since the nitro group has a strong electron-withdrawing effect, p-NP selectively adsorbs on the surface of Ag and TCQ, which will help accelerate the catalytic reaction.

[0048] Based on the above experimental results and theoretical calculations, we proposed a possible catalytic mechanism for the improvement of the p-NP reduction performance of the composite sample TCQ / Ag@AgTaO3 under lightless and visible light excitation. Usually, the electron movement inside a single substance has no definite orbit, but after the formation of a complex, due to the uneven distribution of carriers and the difference in Fermi level, the electrons in the contacting semiconductors and semiconductors and metals occupy completely different highest quantum state energies. At this time, the system will undergo directional migration according to the size of the chemical potential until the electron filling energy level state is consistent and reaches thermodynamic equilibrium, that is, it has a unified Fermi level. Fig.13 a is the absence of light, free e - Schematic diagram of the transfer path between TCQ, Ag and AgTaO3. Since the Fermi level of AgTaO3 is higher than that of TCQ and Ag, once they come into contact, e - It will diffuse from the high-energy level of AgTaO3 to the low-energy level of TCQ and Ag, forming a composite reaction system with multiple reactive sites to synergistically promote p-NP catalytic reduction. In this process, the Fermi level of AgTaO3 will be lowered, while the Fermi levels of TCQ and Ag will be raised until they reach a flat state. For TCQ and Ag, their Fermi levels are equivalent, so in the absence of external forces, e - The migration driving force is small and can be ignored compared with AgTaO3. Therefore, the main reason for the improvement of TCQ / Ag@AgTaO3 performance in the absence of light is the increase in active sites. - The Fermi level will gradually reach equilibrium due to the directional migration of AgTaO3 and the establishment of a built-in electric field from AgTaO3 to TCQ. Fig.13 b, PE on TCQ semiconductor CB under visible light- Driven by the built-in electric field, the charge is transferred to the CB of AgTaO3, and then affected by the Fermi level, it is transferred to the surface of metal Ag for catalytic reduction reaction. This charge transfer method can effectively enhance the e - and h + The spatial separation rate is due to the built-in electric field of TCQ and AgTaO3 which can effectively promote the pe - The Schottky barrier formed between AgTaO3 and metal Ag can effectively prevent the migration of e - and h + This carrier transfer mechanism plays a positive role in the catalytic reaction and promotes the photothermal synergistic reduction of p-NP by TCQ / Ag@AgTaO3.

[0049] The above experimental phenomena and theoretical calculation results show that the composite photocatalyst formed by combining two semiconductors with similar Fermi levels with another semiconductor with different Fermi levels can achieve multi-electron transfer and multi-active site catalysis under different reaction conditions. In the absence of light, TCQ and metal Ag can simultaneously serve as active sites for the p-NP reduction reaction, synergistically promoting the catalytic reaction. When under visible light, the e of VB on TCQ - is excited to its CB, the e - The CB migrated to AgTaO3 under the driving force of the built-in electric field, and finally gathered on the Ag nanoparticles due to the difference in Fermi level. The rectifying effect of the Schottky barrier between Ag and AgTaO3 further improved the separation efficiency of carriers and achieved fast and efficient reduction of p-NP.

[0050] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a composite photocatalyst, Features: The specific steps include: S1: Ag 2 Preparation of O precursor: weigh AgNO 3 and NaOH were dissolved in distilled water and stirred continuously until the mixture was uniform to obtain AgNO 3 solution and NaOH solution; then add the NaOH solution dropwise into the AgNO 3 A dark brown suspension was formed in the solution, and then the suspension was aged at 25°C, filtered and washed with distilled water until neutral, and dried in a vacuum at 60°C to obtain Ag. 2 O; S2: AgTaO 3 Preparation: Accurately weigh Ag 2 O and Ta 2 O 5 Dissolve in anhydrous ethanol and grind with an agate mortar and pestle until the ethanol is completely volatilized to obtain a mixture; keep the mixture at 800℃ and 1000℃ for 1h and 5h respectively at a constant heating rate, cool to room temperature naturally after the reaction, wash with dilute nitric acid and a large amount of distilled water, and finally dry in an oven at 60℃ overnight to obtain AgTaO 3 ; S3: Preparation of CdS QDs: Prepare anhydrous CdCl 2 Add the thioglycolic acid solution to distilled water and mix well. Adjust the pH to 10.0 with NaOH. Then transfer to a three-necked flask and add Na 2 S·9H 2 O, continue heating in an oil bath; finally wash with distilled water and anhydrous ethanol and dry to obtain CdS QDs; S4: CdS QDs / AgTaO 3 Preparation: Weigh AgTaO 3 The solid was placed in a beaker, CdS QDs were added, and then distilled water was added, stirred at room temperature to obtain a mixture, and dried; the dried mixture was poured into an agate jar, and 4 agate balls with a specification of Φ10 and 10 agate balls with a specification of Φ6 were added at the same time; CdS QDs / AgTaO uniformly loaded with CdS QDs was obtained by high-energy ball milling assisted technology 3 ; S5: CdS QDs / Ag@AgTaO 3 Preparation: CdS QDs / AgTaO 3 With NaBH 4 The mixed solution was washed with distilled water and dried to obtain CdS QDs / Ag@AgTaO 3 .

2. A method for preparing a composite photocatalyst according to claim 1, Features: In step S1, AgNO 3 The mass of is 4.62g, the mass of NaOH is 1.5g, the volume of distilled water is 50mL; the aging time is 24h.

3. The method for preparing a composite photocatalyst according to claim 1, Features: In step S2, Ag 2 The mass of O is 0.0927g, Ta 2 O 5 The mass of is 0.1768 g, the volume of anhydrous ethanol is 8 mL, and the heating rate is 5 °C / min.

4. The method for preparing a composite photocatalyst according to claim 1, Features: In step S3, anhydrous CdCl 2 The molar weight is 0.2mmol, the volume of thioglycolic acid solution is 150μL, the volume of distilled water is 100mL; the concentration of NaOH is 1.0M; Na 2 S·9H 2 The molar amount of O is 0.6 mmol; the oil bath temperature is 100°C, the continuous heating time is 2 h; and the drying temperature is 60°C.

5. The method for preparing a composite photocatalyst according to claim 1, Features: In step S4, AgTaO 3 The mass of the solid is 1 g; the mass fraction of CdS QDs is 1.0%~10%; the volume of distilled water is 50 mL, and the stirring time is 12 h; the speed of the ball mill is 500 r / min, and the ball milling time is 0.5 h.

6. The method for preparing a composite photocatalyst according to claim 1, Features: In step S5, NaBH 4 The concentration is 0.5M.

7. A composite photocatalyst prepared by the method for preparing a composite photocatalyst as claimed in any one of claims 1 to 6.

8. Use of the composite photocatalyst as claimed in claim 7 in catalyzing the reduction of p-nitrophenol by sodium borohydride.

Citation Information

Patent Citations

  • Catalyst for producing hydrogen by visible light catalytic decomposition of hydrogen sulfide and preparation method thereof

    CN114100633A