Functional circuit in-situ direct writing method and functional component thereof

By constructing a microstructure array on a dielectric substrate and performing direct laser writing, the problems of insufficient binding force of functional lines and poor forming accuracy are solved, and functional lines manufacturing with high service reliability and accuracy are achieved, suitable for high-temperature and high-precision circuit applications. .

CN118905449APending Publication Date: 2024-11-08HUAZHONG UNIV OF SCI & TECH

Patent Information

Application Number
CN202410974062.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing functional line manufacturing technology has problems such as insufficient binding force, easy cracking and peeling, and poor forming accuracy, especially in high-temperature environments and high-precision circuit structure manufacturing.

Method used

Laser etching is performed on the dielectric substrate to construct the microstructure array, and write the functional slurry in situ along the microstructure array. Through laser curing, a functional line with high service reliability and accuracy is formed, and the laser etching and micro-clamping parameters are optimized. Improve interface bonding and forming accuracy.

Benefits of technology

It significantly improves the bonding force between functional lines and substrates, avoids cracking and peeling defects, improves forming accuracy and service reliability, and is suitable for high-temperature and high-precision circuit applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905449A_ABST
    Figure CN118905449A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of functional circuit preparation, and particularly discloses a functional circuit in-situ direct writing method and a functional component thereof, and the method comprises the steps: carrying out the laser etching on a dielectric substrate to construct a microstructure array, and obtaining a modified substrate; functional slurry is directly written on the modified substrate in situ along the microstructure array, and then the functional slurry is cured, so that a functional circuit with high service reliability and precision is prepared. On one hand, the specific surface area of the dielectric substrate can be greatly increased, the effective contact area between the functional slurry and the dielectric substrate is promoted, and the heterogeneous interface bonding strength between the functional circuit and the dielectric substrate is greatly improved, and on the other hand, functional slurry liquid drops can easily enter the interior of the microstructure through the laser effect, so that the performance of the dielectric substrate is improved. The solid-liquid contact area is increased, the contact angle is reduced, the surface hydrophilicity of the dielectric substrate is improved, the wettability of the functional slurry on the surface of the dielectric substrate is improved, and the quality of a functional circuit prepared in a direct writing mode of the functional slurry is further effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of functional circuit preparation, and more specifically, relates to an in-situ direct writing method for functional circuits and functional components thereof. Background Art

[0002] As microwave detection, wireless communication, smart wearable devices and other electronic products develop towards multi-function, miniaturization, conformalization and portability, the traditional conductive circuit manufacturing process represented by exposure, development and chemical etching has become increasingly unable to meet the requirements. Circuit direct writing technology represented by inkjet printing, aerosol printing and micro-pen direct writing / injection molding ~ laser micro-cladding has the characteristics of no need for mask plates, low cost and high flexibility, which can make up for the shortcomings of traditional manufacturing processes in some application scenarios.

[0003] Inkjet printing is a method of obtaining functional circuits / patterns by spraying functional ink along a preset path and depositing it on a substrate through driving methods such as piezoelectric / thermal bubbles. It has been widely used in the preparation of functional components in the fields of flexible electronic devices, sensors, and energy batteries. However, due to the low content of functional phase in the functional ink during inkjet printing, the resistivity of the conductive layer is usually significantly higher than that of the pure metal block, and the roughness and uniformity of the substrate are required to be high. Aerosol printing technology is a new type of non-contact additive manufacturing technology. It mainly uses pneumatic or ultrasonic action to atomize the functional ink to generate aerosol, which is then transported to the print head with the help of gas and accurately deposited on the substrate to obtain a functional pattern. Compared with inkjet printing, the main advantages of aerosol printing are a wide range of material applications, high conductor accuracy, and the ability to achieve curved surface processing, but this technology and equipment are basically monopolized by foreign countries and have problems such as high prices.

[0004] Micro-pen direct writing / jet forming ~ laser micro-cladding is a method in which the functional slurry is first extruded / jetted onto the substrate along a preset path to obtain a functional circuit / pattern by driving it in a manner such as air pressure / mechanical / piezoelectric, and then the surface of the functional slurry is scanned and irradiated by a laser beam to solidify and sinter it. Compared with inkjet printing and aerosol jet printing technology, the functional slurry deposited by micro-pen direct writing / jet forming technology has a higher viscosity (about 10 5 cps), the thickness of the functional circuit obtained is relatively large (about 5 to 20 μm). At the same time, high-energy laser irradiation can perform local and controllable micro-sintering of the functional slurry, thereby greatly reducing the resistivity of the functional circuit without damaging the substrate, and improving the bonding strength with the substrate. Therefore, the micro-pen direct writing / injection forming ~ laser micro-cladding method has wide applicability in the direct writing preparation of electronic circuits and functional components. However, with the increasing demand for the preparation of conformal circuits and devices in recent years, the application limitations of the above technology in certain occasions have become prominent, mainly reflected in the following three aspects:

[0005] 1. The bonding strength between the functional circuit and the substrate is not enough. Normally, when the bonding strength between the functional circuit / film layer and the dielectric substrate reaches the 5B level in the ASTM D3359~08 standard of the American Society for Testing and Materials (ASTM), it is considered to be able to meet the use requirements of general electronic circuits. However, in some special use environments, such as flat / curved circuit board pads, it is usually necessary to go through a high-temperature process (such as 260°C for reflow soldering) to achieve the mounting of surface electronic components, and the above 5B level bonding strength is far from meeting the use requirements. Especially for resin dielectric substrates with lower operating temperatures, the laser curing parameters are limited, which makes the bonding strength between the functional circuit / film layer and the substrate lower, which greatly limits the further development of this technology.

[0006] 2. The thermal expansion coefficients of the functional circuit and the substrate are poorly matched, which leads to stress concentration at the interface during the laser micro-cladding process, causing cracking, peeling and other defects in the functional circuit / film layer, seriously affecting its forming quality and service performance.

[0007] 3. The forming accuracy of functional circuits is poor. New circuit direct writing technologies all use electronic ink or functional paste to directly write circuits. Since functional pastes have a certain fluidity, when used to manufacture high-precision circuit structures, the actual line width is often greater than the preset value, and the circuit forming accuracy is poor, which seriously restricts the scope of application of this technology. Summary of the invention

[0008] In view of the defects of the prior art, the present application provides a method for in-situ direct writing of functional circuits and functional components thereof, aiming to solve the problems of insufficient bonding between the existing functional circuits and substrates, prone to defects such as cracking and peeling, and poor forming accuracy.

[0009] The present application provides a method for in-situ direct writing of functional circuits, specifically:

[0010] S1 performs laser etching on a dielectric substrate to construct a microstructure array, thereby obtaining a modified substrate;

[0011] S2 directly writes the functional slurry in situ along the microstructure array on the modified substrate, and then solidifies the functional slurry to obtain a functional circuit with high service reliability and precision.

[0012] Through the above technical scheme conceived by the present application, compared with the prior art, since the present application constructs a microstructure array on the dielectric substrate, the dielectric substrate and the functional circuit can form an interface bonding mechanism combining infiltration and mechanical bite, thereby greatly improving the interface bonding strength between the two, and it is not easy to produce defects such as cracking and peeling.

[0013] As further preferred, in step S1, when the dielectric substrate is a resin substrate, the parameters of laser etching are: laser output wavelength is 355nm, laser average output power is 0.3W~30W, pulse frequency is 100kHz~1000kHz, and laser output pulse width is 5ps~20ns.

[0014] As a further preferred embodiment, in step S1, when the dielectric substrate is a ceramic substrate, a glass substrate or a glass-ceramic substrate, the parameters of laser etching are: when the laser output wavelength is 355nm, the average laser output power is 0.5W~100W, the pulse frequency is 100kHz~1000kHz, and the laser output pulse width is 5ps~20ns; when the laser output wavelength is 532nm, the average laser output power is 20W~300W, the laser pulse frequency is 100kHz~3000kHz, and the laser output pulse width is 10ns~80ns; when the laser output wavelength is 1064nm, the average laser output power is 5W~300W, the pulse frequency is 100kHz~5000kHz, and the laser output pulse width is 100fs~40ns.

[0015] As a further preferred embodiment, in step S1, laser etching is performed on one side or both sides of the dielectric substrate.

[0016] As a further preferred embodiment, in step S2, the functional slurry is directly written by using a micro-pen direct writing, jet forming, inkjet printing or aerosol jet printing process.

[0017] As further preferred, in step S2, curing is performed by heating, the curing temperature is 50°C to 800°C, and the curing time is 10 min to 180 min.

[0018] As a further preference, in step S2, continuous laser sintering is used for curing, the laser output wavelength is 532nm or 1064nm, the laser spot is 0.02mm~5mm, the average output power is 0.5W~100W, the laser scanning speed is 0.3mm / s~100mm / s, and the overlap spacing is 0.01mm~10mm.

[0019] As a further preference, the preparation method further comprises step S3, removing redundant functional circuits on the modified substrate by laser etching process.

[0020] As further preferred, in step S3, when the laser output wavelength is 355nm, the average laser output power is 0.3W-100W, the pulse frequency is 100kHz-1000kHz, the laser output pulse width is 5ps-20ns, and the laser scanning speed is 500mm / s-4000mm / s;

[0021] When the laser output wavelength is 532nm, the average laser output power is 10W~300W, the laser pulse frequency is 100kHz~3000kHz, the laser output pulse width is 10ns~80ns, and the laser scanning speed is 1000mm / s~4000mm / s;

[0022] When the laser output wavelength is 1064nm, the average laser output power is 10W-400W, the laser pulse frequency is 100kHz-5000kHz, the laser output pulse width is 100fs-40ns, and the laser scanning speed is 1000mm / s-4000mm / s.

[0023] According to another aspect of the present application, a functional component prepared by using the above-mentioned in-situ direct writing method for functional circuits is provided.

[0024] As a further preference, the thickness of the functional circuit in the functional component is 0.002 mm to 1.5 mm.

[0025] In general, the above technical solutions conceived by this application have the following technical advantages compared with the prior art:

[0026] 1. The present application proposes to prepare a microstructure array on a dielectric substrate, which can greatly increase the specific surface area of ​​the dielectric substrate, promote the effective contact area between the functional slurry and the dielectric substrate, and help to form a strong interface effect of mutual "biting" and "embedding" at the contact interface between the two, greatly improving the heterogeneous interface bonding strength between the functional circuit and the dielectric substrate. On the other hand, the microstructure array formed under the action of laser is conducive to the storage of functional slurry droplets. At the same time, the microstructure on the surface will produce capillary force, which will enhance the adhesion of the dielectric substrate surface to the functional slurry droplets, making it very easy for the functional slurry droplets to enter the microstructure, thereby increasing the solid-liquid contact area, reducing the contact angle, and improving the hydrophilicity of the dielectric substrate surface. The wettability of the functional slurry on the dielectric substrate surface is improved, thereby effectively improving the quality of the functional circuit prepared by the functional slurry direct writing method;

[0027] 2. In particular, the present application optimizes the laser etching process parameters of dielectric substrates of different materials, which can effectively control the size parameters of the microstructure array, thereby ensuring that the subsequent functional slurry can fill or substantially fill the micropores in the microstructure array, avoiding the decrease in interface bonding strength due to gaps. For different types of dielectric substrates, the microstructure morphology size produced under the same laser parameters is different, and the changes in the microstructure during the subsequent laser micro-cladding process with the laser beam scanning are also different. Using the preferred laser etching parameters and laser micro-cladding parameters to modify the dielectric substrate and sinter the functional slurry can greatly improve the heterogeneous interface bonding strength between the functional circuit and the dielectric substrate, and ensure the heterogeneous bonding interface bonding quality;

[0028] 3. In addition, the present application also proposes to further modify the functional circuits after sintering and solidification using a laser etching process, and remove redundant functional circuits on the modified substrate, which can further improve the circuit forming accuracy. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a flow chart of the in-situ direct writing method of the functional circuit provided by the preferred embodiment of the present application;

[0030] Figure 2 It is a laser scanning pattern when scanning and processing the surface of a PEEK (polyetheretherketone) substrate by a pulsed laser dot array scanning method in Example 1 of the present application and a microstructure array morphology obtained on the surface of a dielectric substrate, wherein (a) is a pulsed laser dot array scanning pattern, (b) is a cross-sectional morphology of the original PEEK substrate, and (c) is a cross-sectional morphology of the etched area after laser scanning;

[0031] Figure 3 The morphology of the PEEK substrate surface after laser treatment in Example 1 of the present application after micro-pen direct writing of high-temperature silver functional slurry, wherein (a) is the cross-sectional morphology of the PEEK substrate surface after laser etching after direct writing of high-temperature silver functional slurry using a micro-pen direct writing process, and (b) is the cross-sectional morphology of the slurry after continuous laser micro-cladding to form a barb structure at the interface;

[0032] Figure 4 It is a laser scanning pattern when scanning and processing on the surface of an aluminum nitride ceramic substrate by a microcircle array scanning method in Example 2 of the present application and a microstructure array morphology obtained on the surface of a dielectric substrate, wherein (a) is a microcircle array laser scanning pattern, (b) is a cross-sectional morphology of the original PI substrate, and (c) is a cross-sectional morphology of the etched area after laser scanning;

[0033] Figure 5 This is a morphology diagram of the aluminum nitride ceramic substrate surface after laser treatment in Example 2 of the present application after the conductive copper functional slurry is sprayed;

[0034] Figure 6 It is the laser scanning pattern and the microstructure array morphology obtained on the surface of the alumina ceramic substrate when scanning and processing on the surface of the alumina ceramic substrate by pulse laser dot array scanning in Example 3 of the present application, wherein (a) is the pulse laser dot array laser scanning pattern, (b) is the cross-sectional morphology of the original ceramic substrate, and (c) is the cross-sectional morphology of the laser etched area on the surface of the ceramic substrate after laser scanning.

[0035] In all drawings, the same reference numerals are used to denote the same elements or structures, wherein: 1 - dielectric substrate, 2 - modified substrate, 3 - functional slurry, 4 - functional circuit. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0037] like Figure 1 As shown, the embodiment of the present application provides a method for in-situ direct writing of a functional circuit, specifically:

[0038] S1: grinding the dielectric substrate 1 with sandpaper to obtain a surface with uniform roughness and flatness, so as to facilitate subsequent laser processing and in-situ direct writing, and then ultrasonically cleaning with acetone to remove grease and impurities on the surface of the dielectric substrate 1 to obtain a clean dielectric substrate, and then laser etching is performed on one side or both sides of the dielectric substrate 1 to construct a microstructure array on one side or both sides, thereby obtaining a modified substrate 2;

[0039] S2 uses ultrasonic cleaning to treat the modified substrate 2 to remove foreign matter and impurities generated by pulsed laser etching in the laser action area, and then uses micro-pen direct writing, injection molding, inkjet printing or aerosol printing technology to in-situ write functional slurry 3 along the microstructure array on the modified substrate 2, and then solidifies the functional slurry 3 to obtain a functional circuit 4 with high service reliability and precision.

[0040] Through the above technical scheme conceived by the present application, compared with the prior art, since the present application constructs a microstructure array on the dielectric substrate 1, the dielectric substrate 1 and the functional circuit 4 can form an interface bonding mechanism combining wetting and mechanical bite, thereby greatly improving the interface bonding force between the two, and it is not easy to produce defects such as cracking and peeling. Secondly, the design and addition of the microstructure array on the surface of the modified substrate 2 can produce capillary force on the surface functional slurry, making it very easy to enter the interior of the microstructure array, increasing the solid-liquid contact area, and thus improving the spreadability and spread consistency of the functional slurry at different positions on the surface of the modified substrate 2, and greatly improving the direct writing quality of the functional circuit. Furthermore, for the dielectric substrate 1, especially the semi-crystalline polymer resin substrate, the microstructure at the interface can also effectively release the interface stress between the functional layer and the substrate during the continuous laser micro-cladding process. During the rapid heating and rapid cooling process of continuous laser micro-cladding, due to the different thermal expansion coefficients of the substrate and the functional layer, it is very easy to generate stress in the functional layer and at the functional layer / substrate interface. The introduction of the microstructure array can make the modified substrate and the functional slurry filled in the microstructure undergo synergistic deformation during the continuous laser micro-cladding process, such as slight bending or forming a barb structure at the interface, thereby effectively improving the bonding strength while slowly releasing the tensile stress of the surface film layer, avoiding / reducing defects such as cracking and peeling on the surface of the functional circuit, and improving its service reliability.

[0041] Furthermore, for different types of dielectric substrates 1, the morphology of each micropore in the microstructure array obtained by laser etching is different. The morphology of a single microstructure in a polymer resin substrate is a coexistence of a peak-shaped cone structure and an inverted cone structure, while the microstructure in a ceramic, glass, etc. substrate is an inverted cone structure. Considering the different morphologies of the microstructures of different types of dielectric substrates, the present application proposes to use different laser etching parameters for different types of dielectric substrates.

[0042] When the dielectric substrate 1 is a resin substrate, the parameters of laser etching are: a laser output wavelength of 355nm, an average laser output power of 0.3W to 30W, preferably 0.5W to 25W, a pulse frequency of 100kHz to 1000kHz, preferably 200kHz to 900kHz, and a laser output pulse width of 5ps to 20ns; when scanning along the pulse laser dot array path, the distance between two adjacent points is 5μm to 100μm, the number of single-point laser pulses is 10 to 1000, and when scanning along the microcircle array path, the laser scanning speed is 100mm / s to 4000mm / s, the microcircle radius is 1μm to 30μm, and the distance between adjacent microcircles is 10μm to 100μm. Correspondingly, the parameters of the microstructure array obtained after forming using the above parameters or preferred parameters are as follows: the inverted cone structure is a pit produced by the substrate material being removed by laser etching, located in the area below the surface of the original medium substrate, the bottom diameter d of the inverted cone microstructure is 5μm~100μm, and the bottom diameter d under the preferred parameters is 10μm~70μm; the depth of a single microstructure is 2μm~100μm, and the depth of the microstructure under the preferred parameters is 5μm~80μm; the spacing between adjacent microstructures is 5μm~100μm. The peak-shaped conical structure is produced by cooling after the splashes are splashed during the laser etching process. It is located above the surface of the original medium substrate. The size of the peak-shaped conical structure is related to the laser parameters. By controlling the laser parameters, the amount of splashes during the etching process can be controlled, thereby controlling the peak height and volume of the peak-shaped structure. The peak height is 1μm to 40μm, and the peak height formed by the preferred parameters is 3μm to 30μm. The peak volume increases with the increase of the laser input energy per unit volume, and the spacing between adjacent peaks is the same as the spacing between adjacent inverted cone structures formed.

[0043] When the dielectric substrate 1 is a ceramic substrate, a glass substrate or a ceramic glass substrate, the parameters of laser etching are: the laser output wavelength is 355nm, 532nm or 1064nm, when the laser output wavelength is 355nm, the average laser output power is 0.5W~100W, preferably 3W~60W, the pulse frequency is 100kHz~1000kHz, preferably 200kHz~900kHz, and the laser output pulse width is 5ps~20ns; when scanning according to the pulse laser dot array path, the distance between two adjacent points is 5μm~100μm, the number of single-point laser pulses is 10~2000, and when scanning according to the micro-circle array path, the laser scanning speed is 100mm / s~4000mm / s, the micro-circle radius is 1μm~30μm, and the distance between adjacent micro-circles is 10μm~100μm.

[0044] When the laser output wavelength is 532nm, the average laser output power is 20W~300W, preferably 60W~250W, the laser pulse frequency is 100kHz~3000kHz, preferably 100kHz~500kHz, and the laser output pulse width is 10ns~80ns; when scanning according to the pulse laser dot array path, the distance between two adjacent points is 5μm~100μm, the number of single-point laser pulses is 100~3000, and when scanning according to the micro-circle array path, the laser scanning speed is 50mm / s~3000mm / s, the micro-circle radius is 1μm~30μm, and the distance between adjacent micro-circles is 10μm~100μm.

[0045] When the laser output wavelength is 1064nm, the average laser output power is 5W~300W, preferably 7W~200W, the laser pulse frequency is 100kHz~5000kHz, preferably 200kHz~2500kHz, and the laser output pulse width is 100fs~40ns; when scanning according to the pulse laser dot array path, the distance between two adjacent points is 5μm~100μm, the number of single-point laser pulses is 100~3000, and when scanning according to the micro-circle array path, the laser scanning speed is 50mm / s~3000mm / s, the micro-circle radius is 1μm~30μm, and the distance between adjacent micro-circles is 10μm~100μm.

[0046] Correspondingly, the parameters of the microstructure array obtained after forming using the above parameters or preferred parameters are as follows: the bottom diameter d of the inverted cone microstructure is 5μm~100μm, and the bottom diameter d formed by the preferred parameters is 10μm~70μm; the depth of a single microstructure is 2μm~120μm, and the depth formed by the preferred parameters is 5μm~100μm, and the spacing between adjacent microstructures is 5μm~100μm.

[0047] Furthermore, in step S1, for a flat dielectric substrate, the laser beam can be rapidly moved by a scanning galvanometer, and the scanning path of the laser beam is a pulsed laser dot array or a microcircle array of different radii. After scanning, a microstructure array of different diameters can be obtained on the surface of the dielectric substrate; for a curved dielectric substrate, the laser beam can be dynamically focused on the surface of the curved substrate by a three-axis galvanometer. When the processing size exceeds the scanning field range of the galvanometer, the laser etching of a large-format dielectric substrate can be achieved by the coordinated movement of the scanning galvanometer and the three-axis / five-axis motion platform.

[0048] Furthermore, in step S2, curing is performed by heating, the curing temperature is 50°C to 800°C, and the curing time is 10min to 180min.

[0049] Furthermore, in step S2, when continuous laser sintering curing is adopted, the laser output wavelength is 532nm or 1064nm, the laser spot is 0.02mm-5mm, the average output power is 0.5W-100W, the laser scanning speed is 0.3mm / s-100mm / s, and the overlap spacing is 0.01mm-10mm. For different types of dielectric substrates 1, the microstructure morphology changes differently with the laser sintering process. When the dielectric substrate 1 is a resin substrate, the electronic paste in the microstructure deforms along the laser scanning direction, and a barb structure can be formed to enhance the interface bonding strength; when the dielectric substrate 1 is a ceramic, glass or ceramic glass substrate, the microstructure does not deform with the laser sintering process.

[0050] Furthermore, the preparation method further includes step S3, using a laser etching process to remove redundant functional circuits on the modified substrate 2. The ultrashort pulse laser etching is introduced to remove the redundant functional circuits 4, so that the pattern after direct writing can be further modified, the problem of low forming accuracy of the existing circuit direct writing technology can be solved, and functional circuits that meet both high service reliability and high precision requirements can be manufactured.

[0051] When the laser output wavelength is 355nm, the average laser output power is 0.3W~100W, the pulse frequency is 10kHz~1000kHz, the laser output pulse width is 5ps~20ns, and the laser scanning speed is 500mm / s~4000mm / s;

[0052] When the laser output wavelength is 532nm, the average laser output power is 10W~300W, the laser pulse frequency is 10kHz~3000kHz, the laser output pulse width is 10ns~80ns, and the laser scanning speed is 1000mm / s~4000mm / s;

[0053] When the laser output wavelength is 1064nm, the average laser output power is 10W to 400W, the laser pulse frequency is 50kHz to 5000kHz, the laser output pulse width is 100fs to 40ns, and the laser scanning speed is 1000mm / s to 4000mm / s.

[0054] According to another aspect of the present application, a functional component prepared by using the above-mentioned in-situ direct writing method for functional circuits is provided.

[0055] Furthermore, the thickness of the functional circuit in the functional component is 0.002 mm to 1.5 mm, preferably 0.005 mm to 0.05 mm.

[0056] The technical solution provided in this application is further described below based on specific embodiments.

[0057] Example 1

[0058] In this example, the ultraviolet pulse laser etching process is first used to scan the surface of the PEEK substrate according to the planned path to obtain a microstructure array, and then a micro-pen direct writing method is used to directly write a high-temperature silver conductive paste on the surface of the dielectric substrate etched with the microstructure array, and then the functional paste is heated, dried and continuously laser micro-cladding sintered. The implementation steps include:

[0059] (1) Selecting a 3D printing melt-molded polymer resin PEEK substrate with a thickness of 1 mm;

[0060] (2) The PEEK substrate was ground using 400#, 1000#, and 2000# sandpapers in sequence to obtain a surface with uniform roughness and a smooth surface, and then ultrasonically cleaned with acetone for 10 min to remove grease and impurities on the surface of the dielectric substrate;

[0061] (3) A pulsed laser dot array scanning is performed on the surface of the PEEK substrate using an ultraviolet picosecond laser to obtain a microstructure array on the surface. The laser scanning pattern is as follows: Figure 2 As shown in (a), the initial cross-sectional morphology of the PEEK substrate is Figure 2 As shown in (b), the cross-sectional morphology of the etched area after laser scanning is as follows Figure 2 As shown in (c), during the scanning process using a pulsed laser dot array, the laser output wavelength is 355nm, the laser pulse frequency is 500kHz, the laser pulse width is 10ps, the laser average output power is 0.8W, the distance s between two consecutive engraving points is 30μm, the number of single-point pulse dots is 300, and the inverted cone microstructure diameter d is 15μm, the depth h2 is 17μm, the peak-shaped microstructure height h3 is 12μm, and the spacing s between adjacent microstructures is 30μm;

[0062] (4) ultrasonically cleaning the etched 3D printed PEEK substrate with acetone and alcohol for 10 minutes in sequence to remove foreign matter and impurities generated by etching in the laser action area;

[0063] (5) A micro-pen direct writing process is used to directly write high-temperature silver functional paste on the surface of the PEEK substrate after UV picosecond laser etching. The direct writing thickness h1 is 25 μm. The cross-sectional morphology after direct writing is as follows: Figure 3 As shown;

[0064] (6) Preliminary drying of the functional slurry after direct writing is performed by oven heating, the drying temperature is 120° C., and the drying time is 30 min;

[0065] (7) An infrared continuous fiber laser is used to perform micro-cladding sintering on the high-temperature silver functional slurry, wherein the sintering parameters are: laser output wavelength 1064nm, spot diameter 1mm, laser output power 25W, and laser scanning speed 2mm / s.

[0066] (8) A UV picosecond laser is used to etch and modify the functional circuits / patterns that have been sintered and solidified, and the functional circuits / patterns that are larger than a preset value after direct writing are removed, wherein the etching parameters are: laser output wavelength 355nm, laser pulse frequency 900kHz, laser pulse width 10ps, laser average output power 16W, and laser scanning speed 2000mm / s.

[0067] Example 2

[0068] In this example, an ultraviolet pulse laser etching process is first used to scan the surface of an aluminum nitride ceramic substrate along a microcircle array path to obtain a microstructure array, and then a spray molding method is used to directly write a low-temperature silver functional slurry on the surface of the aluminum nitride ceramic substrate etched with the microstructure array, and then the functional slurry is heated, dried, and continuously laser micro-cladding sintered. The implementation steps include:

[0069] (1) Selecting an injection molded aluminum nitride ceramic substrate with a thickness of 1 mm;

[0070] (2) The aluminum nitride ceramic substrate was ground using 400#, 1000#, and 2000# sandpapers in sequence to obtain a surface with uniform roughness and a smooth surface, and then ultrasonically cleaned with acetone for 10 minutes to remove grease and impurities on the surface of the dielectric substrate;

[0071] (3) Using an ultraviolet nanosecond laser to perform microcircular array scanning processing on the surface of the aluminum nitride ceramic substrate to obtain a microstructure array on the surface. The laser scanning pattern is as follows: Figure 4 As shown in (a), the initial cross-sectional morphology of the aluminum nitride ceramic substrate is as follows Figure 4 As shown in (b), the cross-sectional morphology of the etched area after laser scanning is as follows Figure 4 As shown in (c), during the scanning process using a microcircle array, the laser output wavelength is 355nm, the laser pulse frequency is 100kHz, the laser pulse width is 15ns, the laser average output power is 18W, the laser scanning speed is 2000mm / s, the radius r of a single microcircle is 5μm, the spacing s between two consecutive microcircles is 50μm, the obtained microstructure diameter d is 25μm, the depth h220μm, and the spacing s between adjacent microstructures is 50μm;

[0072] (4) ultrasonically cleaning the etched PEEK resin substrate with acetone and alcohol for 10 minutes in sequence to remove foreign matter and impurities generated by etching in the laser action area;

[0073] (5) The conductive copper electronic paste is directly written on the surface of the PI substrate after infrared femtosecond laser etching by using the spray forming direct writing process. The cross-sectional morphology after the functional paste is directly written on the surface of the modified aluminum nitride ceramic substrate is as follows: Figure 5 As shown, the direct writing thickness h1 is 20 μm, and the cross-sectional morphology does not change after laser micro-cladding;

[0074] (6) Preliminary drying of the functional slurry after direct writing is performed in an oven at a drying temperature of 80° C. for 30 min;

[0075] (7) An infrared continuous fiber laser is used to perform micro-cladding sintering on the functional slurry, wherein the sintering parameters are: laser output wavelength 1064 nm, spot diameter 1 mm, laser output power 15 W, and laser scanning speed 2 mm / s.

[0076] (8) An ultraviolet pulse laser is used to etch and modify the above-mentioned sintered and solidified functional circuits / patterns to remove the functional circuits / pattern parts that are larger than the preset value after direct writing, wherein the etching parameters are: laser output wavelength of 355nm, laser pulse frequency of 100kHz, laser pulse width of 15ns, laser average output power of 18W, and laser scanning speed of 3000mm / s.

[0077] Example 3

[0078] In this example, a green light pulse laser etching process is first used to scan the surface of an alumina ceramic substrate along a pulse laser dot array path to obtain a microstructure array, and then an inkjet printing method is used to directly write a ruthenium oxide resistor slurry on the surface of the alumina ceramic substrate etched with the microstructure array, and then the functional slurry is heated, dried, and continuously laser micro-cladding sintered. The implementation steps include:

[0079] (1) Select an alumina ceramic substrate with a thickness of 1 mm;

[0080] (2) using acetone to ultrasonically clean the ceramic substrate for 10 min to remove grease and impurities on the surface of the substrate;

[0081] (3) A nanosecond green laser is used to perform pulsed laser dot array scanning processing on the surface of the ceramic substrate to obtain a microstructure array on the surface. The laser scanning pattern is as follows: Figure 6 As shown in (a), the initial cross-sectional morphology of the ceramic substrate is Figure 6 As shown in (b), the cross-sectional morphology of the etched area after laser scanning is as follows Figure 6 As shown in (c), during the scanning process using a pulsed laser dot array, the laser output wavelength is 532nm, the laser pulse frequency is 500kHz, the laser pulse width is 40ns, the laser average output power is 150W, the distance s between two consecutive engraving points is 60μm, the number of single-point pulse dots is 250, and the diameter d of the obtained single microstructure is 20μm, the depth h2 is 30μm. The spacing s between adjacent microstructures is 60μm;

[0082] (4) ultrasonically cleaning the etched alumina ceramic substrate with acetone and alcohol for 10 minutes in sequence to remove foreign matter and impurities generated by etching in the laser action area;

[0083] (5) using an inkjet printing process to directly write ruthenium oxide resistor slurry on the surface of the ceramic substrate after ultraviolet picosecond laser etching, and the direct writing thickness h1 is 40 μm;

[0084] (6) Preliminary drying of the functional slurry after direct writing is performed by oven heating, the drying temperature is 120° C., and the drying time is 60 min;

[0085] (7) An infrared continuous fiber laser is used to perform continuous laser micro-cladding sintering on the ruthenium oxide resistor slurry, wherein the sintering parameters are: laser output wavelength 1064nm, spot diameter 1mm, laser output power 30W, and laser scanning speed 1mm / s.

[0086] (8) A green light pulse laser is used to etch and modify the above-mentioned sintered and solidified functional circuits / patterns to remove the functional circuits / patterns that are larger than the preset value after direct writing, wherein the etching parameters are: laser output wavelength 532nm, laser pulse frequency 500kHz, laser pulse width 40ns, laser average output power 90W, and laser scanning speed 1000mm / s.

[0087] Example 4

[0088] In this example, an infrared pulse laser etching process is first used to scan the surface of a glass ceramic substrate along a microcircle array path to obtain a microstructure array, and then aerosol printing is used to directly write a conductive copper electronic slurry on the surface of the glass ceramic substrate etched with the microstructure array, and then the functional slurry is heated, dried, and continuously laser micro-cladding sintered. The implementation steps include:

[0089] (1) Select a glass ceramic substrate with a thickness of 1 mm;

[0090] (2) using acetone to ultrasonically clean the ceramic substrate for 10 min to remove grease and impurities on the surface of the substrate;

[0091] (3) Using an infrared femtosecond laser to perform microcircle array scanning processing on the surface of the above glass ceramic substrate to obtain a microstructure array on its surface. During the microcircle array scanning processing, the laser output wavelength is 1064nm, the laser pulse frequency is 3000kHz, the laser pulse width is 300fs, the laser average output power is 200W, the laser scanning speed is 800mm / s, the distance between two consecutive engraving points is 40μm, the microcircle radius r is 20μm, and the diameter d of the obtained single microstructure is 30μm, and the depth h is 220μm. The spacing s between adjacent microstructures is 40μm;

[0092] (4) ultrasonically cleaning the etched glass ceramic substrate with acetone and alcohol for 10 minutes in sequence to remove foreign matter and impurities generated by etching in the laser action area;

[0093] (5) Using an aerosol jet printing process to directly write low-temperature silver electronic ink on the surface of a ceramic substrate etched by a UV picosecond laser, the thickness of the direct writing is 15 μm;

[0094] (6) Preliminary drying of the functional slurry after direct writing is performed by oven heating, the drying temperature is 60° C., and the drying time is 120 min;

[0095] (7) An infrared continuous fiber laser was used to perform continuous laser micro-cladding sintering on low-temperature silver electronic ink, wherein the sintering parameters were: laser output wavelength of 1064 nm, spot diameter of 2 mm, laser output power of 40 W, and laser scanning speed of 10 mm / s.

[0096] (8) An infrared pulse laser is used to etch and modify the above-mentioned sintered and solidified functional circuits / patterns to remove the functional circuits / pattern parts that are larger than the preset value after direct writing, wherein the etching parameters are: laser output wavelength 1064nm, laser pulse frequency 3000kHz, laser pulse width 300fs, laser average output power 120W, and laser scanning speed 3000mm / s.

[0097] Example 5

[0098] The same as Example 1, except that in step (3), the laser scanning mode is pulsed laser dot array scanning, the laser output wavelength is 355 nm, the laser pulse frequency is 100 kHz, the laser pulse width is 5 ps, the laser average output power is 30 W, the distance s between two consecutive engraving points is 100 μm, the number of single-point pulse dots is 10, the obtained inverted cone microstructure has a diameter d of 25 μm, a depth h2 of 5 μm, a peak-shaped microstructure height h3 of 5 μm, and a spacing s between adjacent microstructures of 100 μm.

[0099] Example 6

[0100] The same as Example 1, except that in step (3), the laser scanning mode is pulsed laser dot array scanning, the laser output wavelength is 355 nm, the laser pulse frequency is 100 kHz, the laser pulse width is 20 ns, the laser average output power is 0.3 W, the distance s between two consecutive engraving points is 5 μm, the number of single-point pulse dots is 1000, the obtained inverted cone microstructure has a diameter d of 5 μm, a depth h2 of 25 μm, a peak-shaped microstructure height h3 of 3 μm, and a spacing s between adjacent inverted cone microstructures of 5 μm.

[0101] Example 7

[0102] The same as Example 1, except that in step (3), the laser scanning mode is microcircle array scanning, the laser output wavelength is 355 nm, the laser pulse frequency is 200 kHz, the laser pulse width is 10 ps, ​​the laser average output power is 25 W, the radius r of a single microcircle is 1 μm, the laser scanning speed is 3000 mm / s, the spacing between adjacent microcircles is 100 μm, and the obtained inverted cone microstructure has a diameter d of 35 μm, a depth h2 of 75 μm, and a spacing s between adjacent inverted cone microstructures of 100 μm.

[0103] Example 8

[0104] The same as Example 1, except that in step (3), the laser scanning mode is microcircle array scanning, the laser output wavelength is 355 nm, the laser pulse frequency is 900 kHz, the laser pulse width is 10 ps, ​​the laser average output power is 0.5 W, the radius r of a single microcircle is 30 μm, the laser scanning speed is 100 mm / s, the spacing between adjacent microcircles is 100 μm, and the obtained inverted cone microstructure has a diameter d of 65 μm, a depth h2 of 12 μm, and a spacing s between adjacent inverted cone microstructures of 100 μm.

[0105] Example 9

[0106] The same as Example 2, except that in step (3), during the scanning process using a microcircle array, the laser output wavelength is 355 nm, the laser pulse frequency is 200 kHz, the laser pulse width is 5 ps, the laser average output power is 100 W, the laser scanning speed is 4000 mm / s, the radius r of a single microcircle is 1 μm, the spacing s between two consecutive microcircles is 50 μm, the obtained microstructure diameter d is 32 μm, the depth h2 is 28 μm, and the spacing s between adjacent microstructures is 50 μm.

[0107] Example 10

[0108] The same as Example 2, except that in step (3), during the scanning process using a microcircle array, the laser output wavelength is 355 nm, the laser pulse frequency is 1000 kHz, the laser pulse width is 12 ps, the laser average output power is 0.5 W, the laser scanning speed is 100 mm / s, the radius r of a single microcircle is 30 μm, the spacing s between two consecutive microcircles is 80 μm, the obtained microstructure diameter d is 65 μm, the depth h2 is 5 μm, and the spacing s between adjacent microstructures is 80 μm.

[0109] Embodiment 11

[0110] The same as Example 2, except that in step (3), during the scanning process using a microcircle array, the laser output wavelength is 355 nm, the laser pulse frequency is 900 kHz, the laser pulse width is 10 ns, the laser average output power is 3 W, the laser scanning speed is 2000 mm / s, the radius r of a single microcircle is 15 μm, the spacing s between two consecutive microcircles is 100 μm, the obtained microstructure diameter d is 34 μm, the depth h2 is 37 μm, and the spacing s between adjacent microstructures is 100 μm.

[0111] Example 12

[0112] Same as Example 3, only in step (3), a nanosecond green laser is used to perform pulsed laser dot array scanning processing on the surface of the ceramic substrate, the laser output wavelength is 532nm, the laser pulse frequency is 100kHz, the laser pulse width is 10ns, the laser average output power is 300W, the distance s between two consecutive engraving points is 100μm, the number of single-point pulse dot is 100, and the diameter d of the obtained single microstructure is 40μm, and the depth h2 is 18μm. The spacing s between adjacent microstructures is 100μm;

[0113] Example 13

[0114] The same as Example 3, only in step (3), a nanosecond green light laser is used to perform pulsed laser dot array scanning processing on the surface of the above-mentioned ceramic substrate. The laser output wavelength is 532nm, the laser pulse frequency is 3000kHz, the laser pulse width is 80ns, the laser average output power is 20W, the distance s between two consecutive engraving points is 70μm, the number of single-point pulse dots is 3000, the diameter d of the obtained single microstructure is 40μm, the depth h2 is 85μm, and the spacing s between adjacent microstructures is 70μm.

[0115] Embodiment 14

[0116] The same as Example 3, only in step (3), a nanosecond green light laser is used to perform pulsed laser dot array scanning processing on the surface of the above-mentioned ceramic substrate. The laser output wavelength is 532nm, the laser pulse frequency is 1000kHz, the laser pulse width is 40ns, the laser average output power is 60W, the distance s between two consecutive engraving points is 5μm, the number of single-point pulse dots is 200, the diameter d of the obtained single microstructure is 4μm, the depth h2 is 7μm, and the spacing s between adjacent microstructures is 5μm.

[0117] Embodiment 15

[0118] Same as Example 4, only in step (3), an infrared femtosecond laser is used to perform microcircle array scanning processing on the surface of the glass ceramic substrate to obtain a microstructure array on its surface. During the microcircle array scanning processing, the laser output wavelength is 1064nm, the laser pulse frequency is 5000kHz, the laser pulse width is 100fs, the laser average output power is 300W, the laser scanning speed is 3000mm / s, the distance between two consecutive engraving points is 30μm, the microcircle radius r is 1μm, and the diameter d of the obtained single microstructure is 34μm, and the depth h2 is 72μm. The spacing s between adjacent microstructures is 30μm.

[0119] Example 16

[0120] Same as Example 4, only in step (3), an infrared femtosecond laser is used to perform microcircle array scanning processing on the surface of the glass ceramic substrate to obtain a microstructure array on its surface. During the microcircle array scanning processing, the laser output wavelength is 1064nm, the laser pulse frequency is 100kHz, the laser pulse width is 40ns, the laser average output power is 5W, the laser scanning speed is 50mm / s, the distance between two consecutive engraving points is 100μm, the microcircle radius r is 30μm, and the diameter d of the obtained single microstructure is 62μm, and the depth h2 is 27μm. The spacing s between adjacent microstructures is 100μm.

[0121] Embodiment 17

[0122] The same as Example 4, only in step (3), an infrared femtosecond laser is used to perform microcircle array scanning processing on the surface of the above-mentioned glass ceramic substrate to obtain a microstructure array on its surface. During the microcircle array scanning processing, the laser output wavelength is 1064nm, the laser pulse frequency is 500kHz, the laser pulse width is 300fs, the laser average output power is 7W, the laser scanning speed is 100mm / s, the distance between two consecutive engraving points is 25μm, the microcircle radius r is 5μm, the obtained single microstructure diameter d is 14μm, the depth h2 is 23μm, and the adjacent microstructure spacing s is 25μm.

[0123] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A method for in-situ direct writing of functional circuits, characterized in that: The in-situ direct writing method of the functional circuit is specifically as follows: S1 performs laser etching on a dielectric substrate to construct a microstructure array, thereby obtaining a modified substrate; S2 directly writes the functional slurry in situ along the microstructure array on the modified substrate, and then solidifies the functional slurry to obtain a functional circuit with high service reliability and precision.

2. The in-situ direct writing method for functional circuits according to claim 1, characterized in that: In step S1, when the dielectric substrate is a resin substrate, the parameters of laser etching are: laser output wavelength is 355nm, laser average output power is 0.3W-30W, pulse frequency is 100kHz-1000kHz, and laser output pulse width is 5ps-20ns.

3. The functional circuit in-situ direct writing method according to claim 1, characterized in that: In step S1, when the dielectric substrate is a ceramic substrate, a glass substrate or a glass-ceramic substrate, the parameters of laser etching are: when the laser output wavelength is 355nm, the average laser output power is 0.5W~100W, the pulse frequency is 100kHz~1000kHz, and the laser output pulse width is 5ps~20ns; when the laser output wavelength is 532nm, the average laser output power is 20W~300W, the laser pulse frequency is 100kHz~3000kHz, and the laser output pulse width is 10ns~80ns; when the laser output wavelength is 1064nm, the average laser output power is 5W~300W, the pulse frequency is 100kHz~5000kHz, and the laser output pulse width is 100fs~40ns.

4. The in-situ direct writing method for functional circuits according to claim 1, characterized in that: In step S1, laser etching is performed on one side or both sides of the dielectric substrate.

5. The in-situ direct writing method for functional circuits according to claim 1, characterized in that: In step S2, the functional slurry is directly written by using a micro-pen direct writing, jet forming, inkjet printing or aerosol printing process.

6. The in-situ direct writing method for functional circuits according to claim 1, characterized in that: In step S2, curing is performed by heating, the curing temperature is 50°C to 800°C, and the curing time is 10min to 180min.

7. The functional circuit in-situ direct writing method according to claim 1, characterized in that: In step S2, continuous laser sintering is used for curing, the laser output wavelength is 532nm or 1064nm, the laser spot is 0.02mm~5mm, the average output power is 0.5W~100W, the laser scanning speed is 0.3mm / s~100mm / s, and the overlap spacing is 0.01mm~10mm.

8. The in-situ direct writing method for functional circuits according to claim 1, characterized in that: The preparation method further comprises step S3, using a laser etching process to remove redundant functional circuits on the modified substrate.

9. The in-situ direct writing method for functional circuits according to claim 8, characterized in that: In step S3, when the laser output wavelength is 355nm, the average laser output power is 0.3W-100W, the pulse frequency is 100kHz-1000kHz, the laser output pulse width is 5ps-20ns, and the laser scanning speed is 500mm / s-4000mm / s; When the laser output wavelength is 532nm, the average laser output power is 10W~300W, the laser pulse frequency is 100kHz~3000kHz, the laser output pulse width is 10ns~80ns, and the laser scanning speed is 1000mm / s~4000mm / s; When the laser output wavelength is 1064nm, the average laser output power is 10W-400W, the laser pulse frequency is 100kHz-5000kHz, the laser output pulse width is 100fs-40ns, and the laser scanning speed is 1000mm / s-4000mm / s.

10. A functional component prepared by the in-situ direct writing method for functional circuits as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Microstructured tool and method of making same using laser ablation

    CN101410324A

  • Method and device for efficiently preparing high-performance coating layer

    CN112323061A

  • AlN ceramic copper-clad substrate with firmly combined copper layer and ceramic substrate and preparation method of AlN ceramic copper-clad substrate

    CN115557798A

  • Ultrashort laser micro-texture printing

    US20090268265A1

  • Method for structuring a substrate surface

    US20200198048A1

Cited By

  • Laser double-sided etching stress control method and system for quartz crystal

    CN119839457A