Forming method of composite material launch canister with opening in circumferential direction
Through the circumferential composite launch cylinder forming method with openings, low-temperature curing and vacuum infusion technology are used to solve the internal stress problems caused by the difference in thermal expansion of fiber reinforced composite materials, achieving a high-precision and efficient molding process, reducing costs and Improves product stability and stiffness.
Patent Information
- Application Number
- CN202411010099.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
AI Technical Summary
During the heating and curing process, fiber reinforced composite materials have different thermal expansion and shrinkage and the influence of laying angle, which leads to internal stress of the product, affecting the lightweight of military equipment and the accuracy and stability of the launch cylinder, especially the structure with openings is difficult to meet the use. need.
The composite material emission cylinder molding method is adopted to lay the epoxy resin prepreg on the inner and outer cylinder molds by low temperature curing of 90°C and heat-pressing curing. The resin is poured into the PTFE rail pad and vacuum filling. Fill, combine polyurethane foam and glass cloth to form an outer skin structure, gradually release internal stress and ensure dimensional accuracy.
It realizes high-precision composite molding, reduces processing costs and production complexity, improves the product's profile compensation ability and stiffness, and ensures the internal shape and service life of the transmitter barrel.
Smart Images

Figure CN118906494A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite material preparation, and in particular relates to a method for forming a composite material launch tube with an annular opening. Background Art
[0002] Fiber reinforced composite materials integrate the advantages of light weight, high temperature resistance, sound absorption, moisture resistance, fire resistance, corrosion resistance, high strength, etc., and are gradually used in aerospace and military products. However, fiber reinforced composite materials usually need to be heated and cured before the corresponding products can be prepared. Due to the difference in thermal expansion and contraction between the reinforcement and the matrix, as well as the influence of parameters such as the ply angle, the product itself has internal stress, so that the lightweighting of military equipment has been hindered to varying degrees. The launch tube will receive severe impact during operation, which is prone to deformation and damage, especially for example, the electromagnetic launch tube has an opening in some structures, which leads to the main interface size and the shape size accuracy of the composite molded product cannot meet the use requirements. Therefore, in view of the above problems, a high-precision preparation method for a composite launch tube with an annular partial opening is designed to solve the above problems. Summary of the invention
[0003] In view of this, the present invention aims to overcome the defects in the prior art and proposes a method for forming a composite material launch tube with an annular opening.
[0004] To achieve the above object, the technical solution created by the present invention is implemented as follows:
[0005] A method for forming a composite material launch tube with an annular opening comprises the following steps:
[0006] S1. Select 90℃ low temperature curing epoxy resin prepreg, lay it on the inner tube molding mold and outer tube molding mold respectively, cover it with auxiliary materials after laying, and put it into autoclave for curing to form the inner tube and outer tube, and the forming thickness of the inner tube is controlled to be 0.5-2mm;
[0007] S2. The outer cylinder is machined with a mold to form an opening, and a 5mm secondary processing allowance is reserved on one side of the opening position. After the machining is completed, demoulding is performed; then the outer cylinder is placed in a hot environment and cycled several times between 0 and 90°C to release the internal stress caused by thermal curing;
[0008] S3, using adhesive to bond the polytetrafluoroethylene guide rail pad to the outer wall of the inner tube;
[0009] S4, assembling the outer cylinder and the inner cylinder, and using the vacuum infusion method to completely introduce the resin into the gap between the two;
[0010] S5. After the resin in the gap is completely cured, align the openings of the inner and outer cylinders, and reserve margins in the thickness direction of the two.
[0011] S6, the inner tube is demoulded, and then the excess is cut off by manual cutting;
[0012] S7, spraying polyurethane foam on the surface of the outer cylinder, and after the foam is fully matured, machining the outer surface of the foam to form a functional layer with a heat-insulating effect;
[0013] S8. Lay several layers of EW200 glass cloth on the outer surface of the machined foam, lay vacuum infusion auxiliary materials, prepare glass fiber reinforced plastic on the foam surface, and form an outer skin structure;
[0014] S9. After curing, clean the surface auxiliary materials and then enter the grinding and painting process.
[0015] Furthermore, the inner cylinder forming mold is a metal male mold, and the outer cylinder forming mold is a metal male mold.
[0016] Furthermore, in step S7, after the polyurethane foam is sprayed on the surface of the outer cylinder, the foam outer surface is machined after waiting for more than 24 hours.
[0017] Further, in step S8, three layers of EW200 glass cloth are laid on the outer surface of the foam after machining.
[0018] Further, in step S8, a vacuum infusion method is used to prepare glass fiber reinforced plastic on the foam surface.
[0019] Furthermore, the outer cylinder is placed in a hot environment and cycled between 0 and 90° C. for 3 times.
[0020] Furthermore, in step S5, a margin of 0.5 mm is reserved in the thickness direction of the inner tube and the outer tube.
[0021] Compared with the prior art, the present invention has the following advantages:
[0022] The molding method provided by the invention is simple and easy to implement, the inner dimensions of the product are reliably guaranteed, the vacuum infusion process is used to fill the gap between the inner tube and the outer tube with resin, thereby ensuring the bonding quality of the inner tube and the outer tube, and the mold processing reduces the production of processing tools and reduces the processing cost; the polyurethane foam sandwich structure can effectively compensate for the outer surface to process the outer contour of the product, and the processing efficiency is high compared to the processing of fiber-reinforced composite materials, and the raw material cost is low; at the same time, the outer skin is a vacuum infusion molding process, which ensures the outer dimensions and reduces the production cost of thermal curing, and the molded skin can effectively maintain the outer surface of the product as well as the rigidity and strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments and descriptions of the present invention are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings:
[0024] Figure 1 A schematic diagram of a molded product created for the present invention;
[0025] Figure 2 This is a schematic diagram of the layer structure at the opening of the molded product created by the present invention. DETAILED DESCRIPTION
[0026] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0027] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0028] In the description of the invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installation", "connection" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the invention can be understood according to specific circumstances.
[0029] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments.
[0030] A method for forming a composite material launch tube with an annular opening, wherein the formed product is as follows Figure 1 and Figure 2 As shown, the following steps are included:
[0031] S1. Select 90℃ low-temperature curing epoxy resin prepreg, and use a winding machine to lay the sheets on the inner cylinder molding mold and the outer cylinder molding mold according to the laying parameter requirements of the structural design. After laying, cover with auxiliary materials and put into the autoclave for curing to form the inner cylinder 1 and the outer cylinder 2. The molding thickness of the inner cylinder is controlled at 0.5-2mm, and the molding thickness of the outer cylinder is 2-5 times the thickness of the inner cylinder. Since the inner cylinder has a thin molding thickness and small internal stress, the outer cylinder that is basically completely released from stress is assembled on the inner cylinder to constrain the inner cylinder, and then the inner cylinder is processed. The outer cylinder itself has a large design structural rigidity, and the inner cylinder has a small structural rigidity. Therefore, the outer cylinder can constrain the strain caused by the opening of the inner cylinder, thereby ensuring the inner contour size of the product;
[0032] S2. The outer cylinder is machined with a mold to form an opening 3, and a 5mm secondary processing allowance is reserved on one side of the opening position. After the machining is completed, the outer cylinder is demoulded; then the outer cylinder is placed in a hot environment and cycled between 0 and 90°C for several times to release the internal stress caused by thermal curing; as an example, the outer cylinder is placed in a hot environment and cycled between 0 and 90°C for 3 times.
[0033] S3. Use adhesive to bond the polytetrafluoroethylene rail pad to the outer wall of the inner tube; since polytetrafluoroethylene has the effect of self-lubrication, it can reduce the damage caused by assembly and increase the assembly efficiency, and control the thickness of the adhesive layer in each area to be basically the same;
[0034] S4, assembling the outer cylinder and the inner cylinder, and using the vacuum infusion method to completely introduce the resin into the gap between the two;
[0035] S5. After the resin in the gap is completely solidified, align the openings of the inner and outer tubes, and reserve a margin in the thickness direction of the two to avoid damage to the molding mold during processing. It should also be noted that during the application process, even if the inner tube is deformed relative to the outer tube, the friction between the inner and outer tubes is weakened while the outer tube constrains the inner tube, which effectively protects the launch tube and improves the reliability and service life of the use.
[0036] S6, the inner tube is demoulded, and then the excess is cut off by manual cutting;
[0037] The outer cylinder is machined with a mold for an opening structure. After machining, the mold is demolded to fully release the deformation. Then the inner cylinder is assembled with the outer cylinder without demolding. Before assembly, a polytetrafluoroethylene guide block is bonded to the outer surface of the inner cylinder to control the uniform assembly gap between the outer cylinder and the inner cylinder. Then, vacuum infusion resin is used for filling to bond the outer cylinder and the inner cylinder tightly together. Then, the position where the inner cylinder needs to be opened is machined without demolding, and a manual cut is reserved to avoid damage to the mold when machining. Since the outer cylinder is a structural layer, it is the structural bearing layer of the product, providing rigidity and strength. At the same time, the inner cylinder has a small thickness and small deformation after machining. The bonded outer cylinder constrains the deformation of the inner cylinder, thereby ensuring that the inner size of the product meets the use requirements.
[0038] S7. Spray polyurethane foam 4 on the surface of the outer cylinder. After the foam is fully matured, the foam outer surface is machined to form a functional layer with thermal insulation effect. In this step, the outer surface of the product assembled with the inner cylinder and the outer cylinder is sprayed with polyurethane foam. After the spraying is completed, the outer surface of the polyurethane foam is machined to ensure the outer surface of the product. This layer is a functional layer, which provides thermal insulation effect and can control the product shape contour at a low cost.
[0039] S8, laying several layers of EW200 glass cloth on the outer surface of the machined foam, laying vacuum infusion auxiliary materials, preparing glass fiber reinforced plastic on the foam surface, and forming an outer skin structure 5;
[0040] S9. After curing, clean the surface auxiliary materials and then enter the grinding and painting process.
[0041] The inner cylinder forming mold is a metal positive mold, and the outer cylinder forming mold is a metal positive mold. The inner cylinder is formed by a metal positive mold, and the thermal expansion relationship between the metal mold and the product curing is fully considered to ensure that the inner diameter of the product meets the use requirements after curing. The thickness of the inner cylinder is controlled at 0.5-2mm. This thickness can not only reduce the deformation caused by the later opening processing, but also provide a certain support strength. This structure is the product inner contour dimension guarantee layer. The outer cylinder is also formed by a metal positive mold, and the thermal expansion relationship between the metal mold and the product curing is fully considered to ensure the assembly relationship with the inner cylinder. This structure is the product structure layer and plays the main mechanical bearing.
[0042] The inner cylinder formed by the present invention is used to ensure the inner contour, the outer cylinder is used as a load-bearing structure, the functional layer on the surface of the outer cylinder is used as a thermal insulation layer, and the outer skin structure can maintain the outer contour. In step S7, after spraying polyurethane foam on the surface of the outer cylinder, wait for more than 24 hours, and then machine the outer surface of the foam. In step S8, 3 layers of EW200 glass cloth are laid on the outer surface of the foam after machining. In step S8, glass fiber reinforced plastic is prepared on the foam surface by vacuum infusion. In step S5, a 0.5mm margin is reserved in the thickness direction of the inner cylinder and the outer cylinder.
[0043] The molding method provided by the invention is simple and easy to implement, the inner dimensions of the product are reliably guaranteed, the vacuum infusion process is used to fill the gap between the inner tube and the outer tube with resin, thereby ensuring the bonding quality of the inner tube and the outer tube, and the mold processing reduces the production of processing tools and reduces the processing cost; the polyurethane foam sandwich structure can effectively compensate for the outer surface to process the outer contour of the product, and the processing efficiency is high compared to the processing of fiber-reinforced composite materials, and the raw material cost is low; at the same time, the outer skin is a vacuum infusion molding process, which ensures the outer dimensions and reduces the production cost of thermal curing, and the molded skin can effectively maintain the outer surface of the product as well as the rigidity and strength.
[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for forming a composite material launch tube with an annular opening, characterized in that: The steps include: S1. Select 90℃ low temperature curing epoxy resin prepreg, lay it on the inner tube molding mold and outer tube molding mold respectively, cover it with auxiliary materials after laying, and put it into autoclave for curing to form the inner tube and outer tube, and the forming thickness of the inner tube is controlled to be 0.5-2mm; S2. The outer cylinder is machined with a mold to form an opening, and a 5mm secondary processing allowance is reserved on one side of the opening position. After the machining is completed, demoulding is performed; then the outer cylinder is placed in a hot environment and cycled several times between 0 and 90°C to release the internal stress caused by thermal curing; S3, using adhesive to bond the polytetrafluoroethylene guide rail pad to the outer wall of the inner tube; S4, assembling the outer cylinder and the inner cylinder, and using the vacuum infusion method to completely introduce the resin into the gap between the two; S5. After the resin in the gap is completely cured, the inner tube opening is processed corresponding to the outer tube opening position, and margins are reserved in the thickness direction of the inner tube and the outer tube; S6, the inner tube is demoulded, and then the excess is cut off by manual cutting; S7, spraying polyurethane foam on the surface of the outer cylinder, and after the foam is fully matured, machining the outer surface of the foam to form a functional layer with a heat-insulating effect; S8. Lay several layers of EW200 glass cloth on the outer surface of the machined foam, lay vacuum infusion auxiliary materials, prepare glass fiber reinforced plastic on the foam surface, and form an outer skin structure; S9. After curing, clean the surface auxiliary materials and then enter the grinding and painting process.
2. The method for forming a composite material launch tube with an annular opening according to claim 1, characterized in that: The inner cylinder forming mold is a metal male mold, and the outer cylinder forming mold is a metal male mold.
3. The method for forming a composite material launch tube with an annular opening according to claim 1, characterized in that: In step S7, after the polyurethane foam is sprayed on the surface of the outer cylinder, wait for more than 24 hours and then machine the foam outer surface.
4. The method for forming a composite material launch tube with an annular opening according to claim 1, characterized in that: In step S8, three layers of EW200 glass cloth are laid on the outer surface of the machined foam.
5. The method for forming a composite material launch tube with an annular opening according to claim 1, characterized in that: In step S8, a vacuum infusion method is used to prepare glass fiber reinforced plastic on the foam surface.
6. The method for forming a composite material launch tube with an annular opening according to claim 1, characterized in that: The outer cylinder is placed in a hot environment and cycled between 0 and 90°C for 3 times.
7. The method for forming a composite material launch tube with an annular opening according to claim 1, characterized in that: In step S5, a margin of 0.5 mm is reserved in the thickness direction of the inner tube and the outer tube.