Heat-resistant cellulose acetate material as well as preparation method and application thereof
By graft polymerization and combination of epoxidized alkyl ester compositions, surfactants and antioxidants in cellulose diacetate, the problems of insufficient fluidity and poor heat resistance during processing are solved, and the problem of cellulose diacetate is achieved. Better thermal stability and machining capability.
Patent Information
- Application Number
- CN202411012009.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-26
AI Technical Summary
During the processing process, cellulose diacetate is prone to carbonization and poor heat resistance. The decomposition of existing plasticizers at high temperatures leads to accelerated material degradation, and lacks effective thermal stability and processing capabilities.
Using cellulose diacetate grafted polyp-dioxycyclohexanone and epoxidized alkyl ester composition, combining surfactants and antioxidants, reducing hydrogen bonding between molecular chains, improving fluidity and thermal stability, through double- The screw extrusion process prepares heat-resistant cellulose acetate materials.
It effectively reduces the glass transition temperature of cellulose diacetate, improves the fluidity and processing and forming capacity, avoids carbonization, and prevents high-temperature decomposition through antioxidants, significantly improving the thermal stability of the material.
Smart Images

Figure BDA0004964655550000031 
Figure BDA0004964655550000061 
Figure BDA0004964655550000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cellulose acetate materials, and in particular to a thermal cellulose acetate material and a preparation method and application thereof. Background Art
[0002] Cellulose acetate is the acetate ester of cellulose, a chemically modified natural polymer obtained by esterifying the hydroxyl groups in the cellulose molecule with acetate. Cellulose acetate is mainly divided into two categories: diacetate and triacetate. Its performance depends on the degree of acetylation, that is, the average number of hydroxyl groups of the glucose units of cellulose replaced by acetyl groups. Diacetate is formed by partial hydrolysis of cellulose acetate, and its degree of esterification is lower than that of triacetate. Therefore, its thermal performance is not as good as triacetate, but its dyeing performance is better than triacetate, and its moisture absorption rate is higher than that of triacetate. Triacetate is not hydrolyzed, and its degree of esterification is higher. Therefore, it has strong light and heat resistance, poor dyeing performance, and low moisture absorption rate (also known as regain).
[0003] When the degree of substitution of cellulose is less than 2.0, the molecular fluidity during melting will be reduced, the biodegradability will be poor, and the acetate fiber will carbonize at high temperature during melting. When cellulose diacetate is processed, due to the high glass transition temperature (Tg) of cellulose diacetate, its melt processing temperature even exceeds the degradation temperature (Td). Because the glass transition temperature (Tg) is close to the decomposition temperature, the temperature window for processing is very narrow, resulting in limited processing capacity. Cellulose diacetate decomposes before melt flow. Therefore, it is very important to reduce the glass transition temperature (Tg) of cellulose diacetate and improve the fluidity of cellulose diacetate. This material needs to be plasticized to improve its thermal and tensile properties. In addition, the molecular structure of cellulose diacetate contains a large number of highly polar hydroxyl groups, the hydrogen bonds between the molecular chains of cellulose diacetate are strong, the fluidity in the molten state is poor, and it is easy to carbonize and decompose under high temperature processing, and the heat resistance is poor. In order to improve the fluidity of cellulose diacetate in the molten state, a certain amount of plasticizer is often added during the processing of cellulose diacetate. In different applications, the amount of plasticizer added is usually between 15% and 35%. Commonly used plasticizers include: fatty acid esters, o-phenyl esters, citrate esters, etc., and the type and amount of plasticizers also have a certain effect on the heat resistance of cellulose diacetate. The heat resistance of the plasticizer determines its stability at high temperatures. Once the plasticizer decomposes at high temperatures, the heat resistance of cellulose diacetate will also deteriorate. The degradation of the plasticizer leads to the formation of pores on the surface of the mixture of plasticizer and cellulose diacetate, thereby accelerating the degradation process of cellulose diacetate. The reason is that a large number of cavities are generated on the surface of the mixture, providing a larger specific surface area for cellulose diacetate or providing an acidic environment for rapid degradation of cellulose diacetate, thereby promoting its degradation. Summary of the invention
[0004] In order to overcome the deficiencies of the prior art, one of the objects of the present invention is to provide a heat-resistant cellulose acetate material, which can weaken the effect of hydrogen bonds between the molecular chains of cellulose diacetate, improve the fluidity of cellulose diacetate during processing, avoid carbonization of cellulose diacetate during processing due to insufficient fluidity, reduce the glass transition temperature (Tg) of cellulose diacetate, and improve the thermal stability of cellulose diacetate during processing.
[0005] The second object of the present invention is to provide a method for preparing the heat-resistant cellulose acetate material. The method has simple steps and can be used for industrial production of the heat-resistant cellulose acetate material.
[0006] The third object of the present invention is to provide an application of the heat-resistant cellulose acetate material.
[0007] One of the purposes of the present invention is achieved by the following technical solution:
[0008] A heat-resistant cellulose acetate material, the raw materials of which include, by mass percentage: 65%-75% of diacetyl cellulose grafted with polydioxanone, 1%-2% of a surfactant, 23%-33% of an epoxidized alkyl ester composition of a compound represented by formula 1, and 1%-2% of an antioxidant;
[0009] Formula 1
[0010]
[0011] In Formula 1, R1 is an alkyl group having 8 to 20 carbon atoms containing one to three epoxy groups, and R2 is an alkyl group having 4, 5, or 8 to 10 carbon atoms.
[0012] Furthermore, the raw materials, calculated by mass percentage, include: 70% of cellulose diacetate grafted polydioxanone, 1% of a surfactant, 28% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 1% of an antioxidant.
[0013] Furthermore, the antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane or tris(2,4-di-tert-butylphenyl)phosphite.
[0014] Further, R2 in Formula 1 is selected from butyl, pentyl, 2-ethylhexyl, isononyl and 2-propylheptyl.
[0015] Furthermore, the surfactant is one of polyoxyethylene fatty acid ester, pentaerythritol, sodium oleoyloxyethanesulfonate, cetyltrimethylammonium chloride, and cocamidopropyl betaine.
[0016] Furthermore, the preparation method of the cellulose diacetate grafted polydioxanone comprises the following steps:
[0017] S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times;
[0018] S2, then add 6.69 g of p-dioxone (PDO) monomer into the strictly dried flask through a syringe, and place the strictly dried flask in a preheated oil bath at a temperature of 120° C. for 30 minutes to obtain a clear homogeneous solution system;
[0019] S3, then inject 0.84mL of stannous octoate (Sn(Oct)) under nitrogen conditions at 140℃ 2 ) solution, and react at a reaction temperature of 140° C. for 2 h;
[0020] S4. After rapidly cooling to 0°C, the crude product is dissolved in chloroform and precipitated with anhydrous methanol; the precipitate is then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain the cellulose diacetate grafted polydioxanone.
[0021] The second object of the present invention is achieved by adopting the following technical solution:
[0022] A method for producing a heat-resistant cellulose acetate material comprises the following steps:
[0023] S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 are mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture is dried in a vacuum oven at 70° C. to 90° C. for 20 to 30 hours to obtain a plasticized mixture;
[0024] S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain the heat-resistant cellulose acetate material.
[0025] Further, in step S1, the mixture is dried in a vacuum oven at 70° C. for 24 h.
[0026] A third object of the present invention is to provide an application of a thermal cellulose acetate material.
[0027] Furthermore, the thermal cellulose acetate material is used to manufacture eyeglass frames and high-end tool handles.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The present invention provides a heat-resistant cellulose acetate material. The epoxidized alkyl ester composition of the compound represented by Formula 1 is used as a plasticizer, has good thermal stability, can improve the plasticization efficiency of diacetyl cellulose, reduce the glass transition temperature (Tg) of diacetyl cellulose, and avoid carbonization of diacetyl cellulose during processing due to insufficient fluidity; in diacetyl cellulose grafted polydioxanone, the polydioxanone molecular structure of the side chain has better flexibility due to the presence of ether bonds and methylene groups, and the diacetyl cellulose grafted polydioxanone has a low crystallinity, which can weaken the effect of hydrogen bonds between the molecular chains of diacetyl cellulose, and reduce the viscosity of diacetyl cellulose. The rigidity of the molecular chain of cellulose and the lowering of the glass transition temperature (Tg) of cellulose diacetate help to improve the fluidity of cellulose diacetate during processing, making it easier to shape cellulose diacetate during processing and avoiding carbonization of cellulose diacetate due to insufficient fluidity during processing; surfactants can reduce the surface tension of cellulose diacetate when it is melted, reduce the interaction force between molecules, make cellulose diacetate easier to flow and avoid carbonization of cellulose diacetate due to insufficient fluidity during processing; antioxidants can prevent the decomposition of cellulose diacetate due to high temperature during the melting and heating process of the twin-screw extruder. DETAILED DESCRIPTION
[0030] The present invention is further described below in conjunction with specific embodiments. It should be noted that, under the premise of no conflict, the embodiments or technical features described below can be arbitrarily combined to form a new embodiment.
[0031] Cellulose diacetate was purchased from Sichuan Pushi Cellulose Acetate Co., Ltd., Changning, China; the acetylation content was about 40%, and the average acetylation degree (DS) of cellulose diacetate was 2.41 as determined by 1H-NMR; the average particle size (d50) of the powder was 250 μm, and the specific gravity was 1.20-1.32 g·cm -3 ; The glass transition temperature is about 198°C, and the melting temperature is between 230-250°C; Cellulose diacetate is used after vacuum drying at 70°C for more than 72 hours;
[0032] p-Dioxanone (PDO) in CaH 2 Dry on ice for 48 hours and distill under reduced pressure twice immediately before use. Sn(Oct) 2 ), chloroform, anhydrous methanol, toluene, and acetone were purchased from Sinopharm Chemical Reagent Co., Ltd.;
[0033] The antioxidants tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane and tris(2,4-di-tert-butylphenyl)phosphite were purchased from Hubei Xinrunde Chemical Co., Ltd.;
[0034] TA differential thermal scanner DSC Q200 was purchased from Shenzhen Xinyichuang Technology Co., Ltd.;
[0035] Thermogravimetric analyzer NetzschTG 209F1 was purchased from Hangzhou Hanze Instrument Co., Ltd.
[0036] The molecular chain of cellulose diacetate is rigid for the following reasons: first, its molecules are polar and the interaction between molecular chains is very strong; second, the six-membered pyran ring structure in cellulose diacetate makes internal rotation difficult; finally, hydrogen bonds can be formed both within and between molecules, especially intramolecular hydrogen bonds, which prevent the glycosidic bonds from rotating, thereby greatly increasing its rigidity.
[0037] Example 1
[0038] The present embodiment provides a heat-resistant cellulose acetate material, wherein the raw materials include, by mass percentage: 70% of cellulose diacetate grafted polydioxanone, 1% of surfactant fatty acid polyoxyethylene ester, 28% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 1% of an antioxidant.
[0039] Formula 1
[0040]
[0041] Among them, the antioxidant can prevent the decomposition of cellulose diacetate caused by high temperature during the melting and heating process of the twin-screw extruder.
[0042] In this embodiment, the antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane, that is, antioxidant 1010.
[0043] In Formula 1, R1 is an isononyl group having 8 carbon atoms and containing an epoxy group; and R2 is selected from a butyl group.
[0044] In this embodiment, the preparation method of cellulose diacetate grafted polydioxanone comprises the following steps:
[0045] S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times;
[0046] S2. Then, 6.69 g of p-dioxone (PDO) monomer was added to the strictly dried flask through a syringe, and the strictly dried flask was placed in a preheated oil bath at a temperature of 120° C. for 30 min to obtain a clear homogeneous solution system;
[0047] S3, then inject 0.84mL of stannous octoate Sn(Oct) at 140℃ under nitrogen conditions 2 The solution was reacted at a reaction temperature of 140°C for 2h;
[0048] S4. After rapidly cooling to 0°C, the crude product was dissolved in chloroform and precipitated with anhydrous methanol; the precipitate was then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain cellulose diacetate grafted with polydioxanone.
[0049] Poly(p-dioxanone) (PPDO) is an important aliphatic polyester. 2 ) was used to carry out the graft copolymerization of p-dioxanone (PDO) and cellulose diacetate by ring-opening polymerization.
[0050] This embodiment provides a method for preparing a heat-resistant cellulose acetate material, comprising the following steps:
[0051] S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 were mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture was dried in a vacuum oven at 70° C. for 24 hours to obtain a plasticized mixture;
[0052] S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain a heat-resistant cellulose acetate material.
[0053] The crystallinity of cellulose diacetate (CDA) is affected by the degree of acetylation and the processing process. According to research, cellulose forms cellulose triacetate (CTA) after acetylation, and its crystal form changes and the crystallinity decreases. Furthermore, the cellulose diacetate obtained after the hydrolysis of cellulose triacetate has a clear advantage in amorphous regions, which means that the crystallinity of cellulose diacetate is further reduced.
[0054] Example 2
[0055] This embodiment provides a heat-resistant cellulose acetate material, wherein the raw materials include, by mass percentage: 75% of cellulose diacetate grafted polydioxanone, 1% of a surfactant pentaerythritol, 23% of an epoxidized alkyl ester composition of a compound represented by formula 1, and 1% of an antioxidant;
[0056] Formula 1
[0057]
[0058] Among them, the antioxidant can prevent the decomposition of cellulose diacetate caused by high temperature during the melting and heating process of the twin-screw extruder.
[0059] In this embodiment, the antioxidant is tris(2,4-di-tert-butylphenyl)phosphite, namely antioxidant 168.
[0060] In Formula 1, R1 is an alkyl group of 20 carbon atoms containing two epoxy groups; and R2 is selected from a pentyl group.
[0061] The preparation method of cellulose diacetate grafted polydioxanone in this embodiment comprises the following steps:
[0062] S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times;
[0063] S2. Then, 6.69 g of p-dioxone (PDO) monomer was added to the strictly dried flask through a syringe, and the strictly dried flask was placed in a preheated oil bath at a temperature of 120° C. for 30 min to obtain a clear homogeneous solution system;
[0064] S3, then inject 0.84mL of stannous octoate (Sn(Oct)) under nitrogen conditions at 140℃ 2 ) solution, and react at a reaction temperature of 140° C. for 2 h;
[0065] S4. After rapidly cooling to 0°C, the crude product was dissolved in chloroform and precipitated with anhydrous methanol; the precipitate was then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain cellulose diacetate grafted with polydioxanone.
[0066] This embodiment provides a method for preparing a heat-resistant cellulose acetate material, comprising the following steps:
[0067] S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 were mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture was dried in a vacuum oven at 85° C. for 20 hours to obtain a plasticized mixture;
[0068] S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain a heat-resistant cellulose acetate material.
[0069] Example 3
[0070] This embodiment provides a heat-resistant cellulose acetate material, wherein the raw materials include, by mass percentage: 65% of cellulose diacetate grafted polydioxanone, 2% of a surfactant sodium oleyloxyethanesulfonate, 31% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 2% of an antioxidant;
[0071] Formula 1
[0072]
[0073] Among them, the antioxidant can prevent the decomposition of cellulose diacetate caused by high temperature during the melting and heating process of the twin-screw extruder.
[0074] In this embodiment, the antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane.
[0075] R1 in Formula 1 is an alkyl group of 15 carbon atoms containing three epoxy groups; and R2 is selected from 2-ethylhexyl.
[0076] The preparation method of cellulose diacetate grafted polydioxanone in this embodiment comprises the following steps:
[0077] S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times;
[0078] S2. Then, 6.69 g of p-dioxone (PDO) monomer was added to the strictly dried flask through a syringe, and the strictly dried flask was placed in a preheated oil bath at a temperature of 120° C. for 30 min to obtain a clear homogeneous solution system;
[0079] S3, then inject 0.84mL of stannous octoate (Sn(Oct)) under nitrogen conditions at 140℃ 2 ) solution, and react at a reaction temperature of 140° C. for 2 h;
[0080] S4. After rapidly cooling to 0°C, the crude product was dissolved in chloroform and precipitated with anhydrous methanol; the precipitate was then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain cellulose diacetate grafted with polydioxanone.
[0081] This embodiment provides a method for preparing a heat-resistant cellulose acetate material, comprising the following steps:
[0082] S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 were mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture was dried in a vacuum oven at 90° C. for 30 hours to obtain a plasticized mixture;
[0083] S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain a heat-resistant cellulose acetate material.
[0084] Example 4
[0085] This embodiment provides a heat-resistant cellulose acetate material, wherein the raw materials include, by mass percentage: 64% of cellulose diacetate grafted polydioxanone, 1% of surfactant cetyltrimethylammonium chloride, 33% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 2% of an antioxidant;
[0086] Formula 1
[0087]
[0088] Among them, the antioxidant can prevent the decomposition of cellulose diacetate caused by high temperature during the melting and heating process of the twin-screw extruder.
[0089] In this embodiment, the antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane.
[0090] In Formula 1, R1 is an alkyl group having 10 carbon atoms and containing an epoxy group; and R2 is selected from an isononyl group.
[0091] The preparation method of cellulose diacetate grafted polydioxanone in this embodiment comprises the following steps:
[0092] S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times;
[0093] S2. Then, 6.69 g of p-dioxone (PDO) monomer was added to the strictly dried flask through a syringe, and the strictly dried flask was placed in a preheated oil bath at a temperature of 120° C. for 30 min to obtain a clear homogeneous solution system;
[0094] S3, then inject 0.84mL of stannous octoate (Sn(Oct)) under nitrogen conditions at 140℃ 2 ) solution, and react at a reaction temperature of 140° C. for 2 h;
[0095] S4. After rapidly cooling to 0°C, the crude product was dissolved in chloroform and precipitated with anhydrous methanol; the precipitate was then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain cellulose diacetate grafted with polydioxanone.
[0096] This embodiment provides a method for preparing a heat-resistant cellulose acetate material, comprising the following steps:
[0097] S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 were mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture was dried in a vacuum oven at 70° C. for 24 hours to obtain a plasticized mixture;
[0098] S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain a heat-resistant cellulose acetate material.
[0099] Further, in step S1, the mixture is dried in a vacuum oven at 70° C. for 24 h.
[0100] Example 5
[0101] This embodiment provides a heat-resistant cellulose acetate material, wherein the raw materials include, by mass percentage: 64% of cellulose diacetate grafted polydioxanone, 2% of surfactant cocamidopropyl betaine, 33% of an epoxidized alkyl ester composition of a compound represented by formula 1, and 1% of an antioxidant;
[0102] Formula 1
[0103]
[0104] Among them, the antioxidant can prevent the decomposition of cellulose diacetate caused by high temperature during the melting and heating process of the twin-screw extruder.
[0105] In this embodiment, the antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane.
[0106] R1 in Formula 1 is an alkyl group of 18 carbon atoms containing two epoxy groups; and R2 is selected from 2-propylheptyl.
[0107] The preparation method of cellulose diacetate grafted polydioxanone in this embodiment comprises the following steps:
[0108] S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times;
[0109] S2. Then, 6.69 g of p-dioxone (PDO) monomer was added to the strictly dried flask through a syringe, and the strictly dried flask was placed in a preheated oil bath at a temperature of 120° C. for 30 min to obtain a clear homogeneous solution system;
[0110] S3, then inject 0.84mL of stannous octoate (Sn(Oct)) under nitrogen conditions at 140℃ 2 ) solution, and react at a reaction temperature of 140° C. for 2 h;
[0111] S4. After rapidly cooling to 0°C, the crude product was dissolved in chloroform and precipitated with anhydrous methanol; the precipitate was then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain cellulose diacetate grafted with polydioxanone.
[0112] This embodiment provides a method for preparing a heat-resistant cellulose acetate material, comprising the following steps:
[0113] S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 were mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture was dried in a vacuum oven at 70° C. for 24 hours to obtain a plasticized mixture;
[0114] S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain a heat-resistant cellulose acetate material.
[0115] Further, in step S1, the mixture is dried in a vacuum oven at 70° C. for 24 h.
[0116] Comparative Example 1
[0117] The difference from Example 1 is that Comparative Example 1 provides cellulose diacetate.
[0118] Comparative Example 2
[0119] The difference from Example 1 is that the heat-resistant cellulose acetate material provided in Comparative Example 1 comprises, in terms of mass percentage, 70% of cellulose diacetate, 1% of surfactant fatty acid polyoxyethylene ester, 28% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 1% of an antioxidant 1010.
[0120] Comparative Example 3
[0121] The difference from Example 1 is that the heat-resistant cellulose acetate material provided in Comparative Example 1 comprises, by mass percentage, 98% of cellulose diacetate grafted polydioxanone, 1% of surfactant fatty acid polyoxyethylene ester, and 1% of antioxidant 1010.
[0122] Comparative Example 4
[0123] The difference from Example 1 is that the heat-resistant cellulose acetate material provided in Comparative Example 1 comprises, in terms of mass percentage, 1% of surfactant fatty acid polyoxyethylene ester, 98% of the epoxidized alkyl ester composition of the compound represented by Formula 1, and 1% of antioxidant 1010.
[0124] Comparative Example 5
[0125] The difference from Example 1 is that the heat-resistant cellulose acetate material provided in Comparative Example 1 comprises, in terms of mass percentage, 70% of cellulose diacetate grafted polydioxanone, 28% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 2% of an antioxidant 1010.
[0126] Experimental Example 1
[0127] Determination of glass transition temperature
[0128] Differential scanning calorimetry (DSC) was performed using TA Instruments DSC Q200. Measurements were made in a sealed aluminum pan at a scanning rate of 20°C / min under a nitrogen atmosphere, and calibrated to an indium standard metal. The samples of Examples 1-5 and Comparative Examples 1-5 were first cooled to -50°C in the first heating scan, heated to 140°C, maintained at 140°C for 5 minutes to eliminate the effects of the thermal history, and then quenched to -50°C. The samples of Examples 1-5 and Comparative Examples 1-5 were again heated from -50°C to 190°C for a second heating scan, and the glass transition temperature Tg and melting temperature Tm were determined by thermal maps. Examples 1-5 and Comparative Examples 1-5 require at least 3 measurements on average, and the measurement results are shown in Table 1.
[0129] Determination of thermal stability
[0130] Thermogravimetric analyzer NetzschTG 209F1 was used to study the thermal stability of Examples 1-5 and Comparative Examples 1-5. 5-10 mg of the sample was heated on a platinum pan under a nitrogen atmosphere, the scanning temperature range was set to 25°C to 700°C, and the heating rate was 10°C / min. The results of the thermogravimetric (DTG) analysis were measured by measuring the percentage of mass loss of the sample at the measurement temperature. At least 3 measurements were required for Examples 1-5 and Comparative Examples 1-5, and the measurement results are shown in Table 1.
[0131] Table 1
[0132]
[0133]
[0134] Note: Ti is the initial degradation temperature of the sample; T20% is the temperature at which the sample loses 20% of its weight; T50% is the temperature at which the sample loses 50% of its weight
[0135] It can be seen from Table 1 that the glass transition temperature Tg of Examples 1-5 is significantly lower than that of Comparative Examples 1-5, and the Ti value, T20% value, and T50% value are significantly higher than those of Comparative Examples 1-5, indicating that Examples 1-5 have good thermal stability and heat resistance; the glass transition temperature Tg of Comparative Examples 2-4 is significantly higher than that of Examples 1-5, and the Ti value, T20% value, and T50% value are significantly lower than those of Examples 1-5, indicating that on the one hand, cellulose diacetate grafted with polydioxanone can weaken the effect of hydrogen bonds between the molecular chains of cellulose diacetate, reduce the rigidity of the molecular chains of cellulose diacetate, and improve the fluidity of cellulose diacetate during processing, making cellulose diacetate easier to shape during processing, and avoiding cellulose diacetate from being deformed due to insufficient fluidity. Carbonization occurs during the processing. On the other hand, the diacetate cellulose grafted with polydioxanone and the epoxidized alkyl ester composition coordinately reduce the glass transition temperature Tg of the diacetate cellulose, improve the fluidity of the diacetate cellulose during the processing, make the diacetate cellulose easier to shape during the processing, and avoid the diacetate cellulose from carbonizing during the processing due to insufficient fluidity; the glass transition temperature Tg of comparative example 5 is greater than that of embodiment 1, and the Ti value, T20% value, and T50% value are less than those of embodiment 1, indicating that the surfactant can reduce the surface tension of the diacetate cellulose when it is melted, reduce the interaction force between molecules, make the diacetate cellulose easier to flow, and avoid the diacetate cellulose from carbonizing during the processing due to insufficient fluidity.
[0136] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A heat-resistant cellulose acetate material, characterized in that: The raw materials include, by mass percentage, 65%-75% of cellulose diacetate grafted polydioxanone, 1%-2% of a surfactant, 23%-33% of an epoxidized alkyl ester composition of a compound represented by formula 1, and 1%-2% of an antioxidant; Formula 1 In Formula 1, R1 is an alkyl group having 8 to 20 carbon atoms containing one to three epoxy groups, and R2 is an alkyl group having 4, 5, or 8 to 10 carbon atoms.
2. A thermal cellulose acetate material according to claim 1, characterized in that: The raw materials, calculated by mass percentage, include: 70% of cellulose diacetate grafted polydioxanone, 1% of a surfactant, 28% of an epoxidized alkyl ester composition of a compound represented by Formula 1, and 1% of an antioxidant.
3. A thermal cellulose acetate material according to claim 1, characterized in that: The antioxidant is tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)]methane or tris(2,4-di-tert-butylphenyl)phosphite.
4. The thermal cellulose acetate material according to claim 1, characterized in that: R2 in Formula 1 is selected from the group consisting of butyl, pentyl, 2-ethylhexyl, isononyl and 2-propylheptyl.
5. The thermal cellulose acetate material according to claim 1, characterized in that: The surfactant is one of polyoxyethylene fatty acid ester, pentaerythritol, sodium oleyloxyethanesulfonate, cetyltrimethylammonium chloride and cocamidopropyl betaine.
6. The thermal cellulose acetate material according to claim 1, characterized in that: The preparation method of cellulose diacetate grafted polydioxanone comprises the following steps: S1. Add 2.0 g of cellulose diacetate into a strictly dried flask and purge it with dry nitrogen three times; S2, then add 6.69 g of p-dioxanone monomer into the strictly dried flask through a syringe, and place the strictly dried flask in a preheated oil bath at a temperature of 120° C. for 30 min to obtain a clear homogeneous solution system; S3, then inject 0.84 mL of stannous octoate solution under nitrogen conditions at 140° C., and react at a reaction temperature of 140° C. for 2 h; S4. After rapidly cooling to 0°C, the crude product is dissolved in chloroform and precipitated with anhydrous methanol; the precipitate is then extracted with toluene and acetone for 48 hours for purification; and vacuum dried at 60°C to constant weight to obtain the cellulose diacetate grafted polydioxanone.
7. A method for preparing a heat-resistant cellulose acetate material according to any one of claims 1 to 6, characterized in that: The following steps are involved: S1. At room temperature, cellulose diacetate grafted polydioxanone and an epoxidized alkyl ester composition of a compound represented by Formula 1 are mixed in a high-speed mechanical stirrer for 2 minutes according to the formula amount, and then the mixture is dried in a vacuum oven at 70° C. to 90° C. for 20 to 30 hours to obtain a plasticized mixture; S2. Add the plasticized mixture into a twin-screw extruder, then add an antioxidant and a surfactant into the twin-screw extruder, and after melt extrusion, slice the cellulose diacetate grafted with polydioxanone to produce particles to obtain the heat-resistant cellulose acetate material.
8. The method for preparing a thermal cellulose acetate material according to claim 7, characterized in that: In step S1, the mixture is dried in a vacuum oven at 70°C for 24 hours.
9. Use of a thermal cellulose acetate material according to any one of claims 1 to 6, characterized in that: The thermal cellulose acetate material is used for manufacturing spectacle frames and high-grade tool handles.
Citation Information
Patent Citations
Chitin / polydioxide cyclohexanone graft copolymer and its production
CN101029093A
Starch acetate / PPDO-grafted copolymer, preparation method and application thereof
CN101337994A
Starch acetate-polydioxanone graft copolymer / inorganic particulate nano composite material and preparation method thereof
CN101717528A
Preparation method of modified cellulose acetate
CN103193938A
Cellulose diacetate grafted copolymer capable of achieving melt spinning and preparation method thereof
CN105803556A