Method for preparing surface active particle modified perovskite cathode by ion exchange method and application thereof
The perovskite cathode modified with surfactant particles was prepared by ion exchange method, and the perovskite lattice was filled with G metal and the formation of alloy nanoparticles were solved, which solved the catalytic performance and stability of perovskite cathode and achieved efficient CO2 electrocatalysis and long-term stability of electrode materials.
Patent Information
- Application Number
- CN202411287311.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-08
AI Technical Summary
The perovskite cathode has low catalytic performance in CO2 electrocatalytic reduction reaction, and structural damage and metal carbonate formation are prone to occur during the reduction treatment, resulting in the loss of the electrode surface active site and affecting the stability of the electrode.
The perovskite cathode modified with surfactant particles was prepared by ion exchange method. Through the precursor solution impregnation of G metal and high-temperature reducing atmosphere, alloy nanoparticles composed of G and M” were formed, and the perovskite lattice was filled, and the perovskite lattice was expanded. Reaction interface and keep structure intact.
It improves the catalytic activity of CO2 and the stability of the electrode material, enhances the anti-CO2 toxicity properties and conductivity, and improves the anti-sintering and anti-carbon deposit ability of the electrode.
Smart Images

Figure CN118910645A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid oxide electrolytic cells, and specifically relates to a method for preparing a surface active particle modified perovskite cathode by an ion exchange method and application thereof. Background Art
[0002] With the development of modern society, the consumption of traditional fossil energy such as coal, oil and natural gas is increasing day by day around the world, and the sharp increase in CO2 emissions has brought about increasingly serious climate problems. How to efficiently catalytically convert CO2 into chemical products and realize resource utilization is one of the scientific hotspots that has attracted much attention. Solid oxide electrolysis cell (SOEC) is an energy conversion device that can utilize electricity generated by renewable energy such as solar energy and wind energy, coupled with industrial waste heat, to catalytically convert CO2 into chemical raw materials such as CO. It has the advantages of high energy conversion efficiency and green environmental protection. The SOEC device consists of three parts: electrolyte, anode and cathode. The cathode undergoes a CO2 reduction reaction to produce CO and dissociated oxygen ions. The former is discharged from the tail gas as a product, and the latter is conducted to the anode through the electrolyte to produce O2 by oxygen evolution reaction. The characteristics of the electrode material determine the overall performance of SOEC. In addition to good electronic conductivity and ionic conductivity, the cathode material also needs to have excellent CO2 catalytic activity and stability.
[0003] Perovskite materials have excellent electron-ion mixed conductivity and are a common electrode material. However, their catalytic performance is low, and they need to be optimized to meet actual needs. Active particles can be loaded on the electrode surface by impregnation to improve catalytic activity, but the surface particles have poor interaction with the substrate, and particles are prone to agglomeration and sintering; using a reducing atmosphere to treat, the B-site metal ions with a strong reduction tendency are segregated from the lattice to the surface, which can improve the metal-support interaction, but on the one hand, due to the limited diffusion rate and diffusion distance, most of the B-site metal ions still exist in the bulk structure, the atomic utilization rate is low, and the number of surface active sites is limited; on the other hand, with the dissolution of the B-site metal ions, the A-site metal in the lattice is "excessive", and the A-site metal ions are easily segregated in the form of oxides, which leads to the destruction of the perovskite structure, especially in the CO2 reaction atmosphere, it is easy to generate high-resistance phases such as metal carbonates, resulting in the loss of active sites on the electrode surface and the decline of catalytic performance. Therefore, how to take into account the stability of the electrode material while constructing active sites is a key factor restricting the CO2 electrocatalytic reduction reaction. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a perovskite cathode modified with surface active particles by an ion exchange method and its application. The cathode material is an electron-ion mixed conductor, and the surface has alloy nanoparticles composed of G and M'' dissolved out, which can effectively expand the reaction triple phase interface, increase the reaction sites. At the same time, during the reduction treatment process, G fills into the perovskite lattice, playing a role in maintaining the integrity of the perovskite structure, making the surface active particle modified catalyst have both high activity and high stability, so as to be used as an excellent SOEC cathode material.
[0005] In order to achieve the above object, the technical solution of the present invention is as follows:
[0006] On the one hand, the present invention provides a method for preparing a perovskite cathode modified with surface active particles by an ion exchange method. The perovskite oxide with the chemical formula La 0.6 Sr 0.4 M’ 1-x M” x O 3-δ is impregnated with a precursor solution of G metal, and after being calcined in high-temperature air and treated in a high-temperature reducing atmosphere in sequence, a perovskite electrode modified with surface active particles is obtained; wherein, 0 < x < 1, and δ is the oxygen vacancy content;
[0007] The active particles are alloy nanoparticles composed of G and M'';
[0008] In the perovskite electrode modified with surface active particles, the perovskite lattice contains G element.
[0009] In the above technical solution, further, M’ is one or more of Cr, Mn, Ti, V, Zr.
[0010] In the above technical solution, further, M” is one or more of Co, Ni.
[0011] In the above technical solution, further, the metal G is Fe; the precursor solution of G metal is an aqueous solution of nitrate or inorganic acid salt of G metal.
[0012] In the present invention, through the impregnation of the precursor solution of G metal, the filling of G element into the perovskite lattice structure, and at the same time promoting the dissolution of M” metal, alloy nanoparticles composed of G and M” are formed on the surface of the perovskite oxide.
[0013] In the above technical solution, further, the method specifically includes the following steps:
[0014] (1) Mix La 0.4 Ce 0.6 O 2-δ (LDC) powder with an ethyl cellulose-terpineol mixture to obtain an LDC interlayer slurry, and coat it on La by spin coating0.8 Sr 0.2 Ga 0.8 Mg 0.2 O 3-δ (LSGM) electrolyte side, calcined to obtain LDC separator;
[0015] (2) La 0.6 Sr 0.4 M' 1-x M” x O 3-δ The powder is ground, and the ethyl cellulose-pinene alcohol mixture is added and stirred evenly to obtain a cathode slurry;
[0016] (3) uniformly coating the cathode slurry obtained in step (2) on the surface of the LDC interlayer by screen printing, brushing or spin coating, and calcining at 1000-1200° C. in air for 2-5 h to obtain a perovskite cathode skeleton;
[0017] (4) The precursor solution of metal G is impregnated into the perovskite cathode skeleton obtained in step (3) by a microinjection method, calcined in air, and then treated in a reducing gas to obtain a perovskite cathode modified with surface active particles.
[0018] In the above technical solution, further, in the step (4), the microinjection method includes immersing the entire solution at one time and repeatedly immersing the solution multiple times.
[0019] In the above technical solution, further, in step (4), the calcination temperature is 300-1000° C., and the calcination time is 0.5-10 h.
[0020] In the above technical solution, further, in step (4), the reducing gas is a mixed gas of Ar, He, and H2;
[0021] The flow rate of the reducing gas is 70-250 mL cm -2 min -1 ; The treatment temperature is 500-1000℃ and the treatment time is 1-10h.
[0022] In the above technical solution, further, La 0.6 Sr 0.4 M' 1-x M” x O 3-δ Perovskite oxides are prepared by the following method:
[0023] According to La 0.6 Sr 0.4 M' 1-x M” x O 3-δThe stoichiometric ratio of perovskite is as follows: La precursor, Sr precursor, M' precursor and M" precursor are dissolved in water, a complexing agent is added to form a mixed solution, ammonia water is added to adjust the pH of the solution to 8, heated and stirred at 60-80 ° C to evaporate to form a sol, and then self-propagating combustion occurs to obtain a primary powder, which is transferred to a high-temperature furnace and calcined at 1000-1400 ° C for 2-20 hours to obtain La 0.6 Sr 0.4 M' 1-x M” x O 3-δ Perovskite oxides.
[0024] In the above technical solution, further, the complexing agent is citric acid and ethylenediaminetetraacetic acid; the ratio of the total molar number of citric acid, ethylenediaminetetraacetic acid and metal ions is 1:1.5:1.
[0025] Another aspect of the present invention provides a perovskite cathode modified with surface active particles prepared by the above method.
[0026] The present invention also provides a use of the above-mentioned surface active particle modified perovskite cathode in the preparation of a solid oxide electrolytic cell.
[0027] In the above technical solution, it is further used for CO2 electrocatalytic reduction reaction.
[0028] The beneficial effects of the present invention are:
[0029] The perovskite cathode prepared by the present invention has a composite nanostructure, and the three-phase interface can be effectively expanded by modifying the surface active particles, the reaction sites can be increased, and the CO2 catalytic activity can be improved. The filling of the perovskite lattice structure by the G element can stabilize the perovskite matrix structure while promoting the dissolution of the M" metal, thereby improving the CO2 poisoning resistance of the electrode material and effectively improving the stability of the electrode material. The perovskite cathode of the present invention has good electrical conductivity and anti-sintering and anti-carbon deposition capabilities. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the XRD spectrum of the LSCC sample modified with surfactant particles in Example 1;
[0031] Figure 2 Surface morphologies of LSCC and LSCC samples modified with surface CoFe particles in Example 1, wherein a is the surface morphology of LSCC, and b is the surface morphology of LSCC modified with surface CoFe particles;
[0032] Figure 3 is a scanning electron microscope image of a cross section of the solid oxide electrolytic cell of Example 2;
[0033] Figure 4The CO2 electrolysis performance diagram of the solid oxide electrolytic cell of Example 2 and Comparative Example 1, wherein a is the linear sweep voltammetry curve and b is the chronoamperometric curve. DETAILED DESCRIPTION
[0034] The present invention is described in detail below by way of examples, but the scope of the claims of the present invention is not limited by these examples. Meanwhile, the examples only provide partial conditions for achieving this purpose, and do not mean that these conditions must be met to achieve this purpose.
[0035] Example 1
[0036] The preparation of a perovskite cathode modified with surface CoFe active particles comprises the following steps:
[0037] (1) According to La 0.6 Sr 0.4 Cr 0.9 Co 0.1 O 3-δ The stoichiometric ratio of (LSCC) was 7.7942 g of lanthanum nitrate hexahydrate, 2.5396 g of strontium nitrate, 8.4032 g of chromium nitrate nonahydrate, 2.6193 g of cobalt nitrate hexahydrate, and 18.9126 g of citric acid monohydrate were dissolved in deionized water, 17.5344 g of ethylenediaminetetraacetic acid was added, and ammonia water was added dropwise to adjust the pH value of the solution to 8, and the solution was heated and stirred at 80°C until it was in a gel state, and the gel was heated in a heating furnace until self-propagating combustion occurred to obtain LSCC primary powder, which was transferred to a muffle furnace and calcined at 1300°C for 10 hours to obtain LSCC powder;
[0038] (2) According to La 0.4 Ce 0.6 O 2-δ The stoichiometric ratio of (LDC) was 8.6602 g of lanthanum nitrate hexahydrate, 13.0266 g of cerium nitrate nonahydrate and 5.6303 g of glycine were dissolved in deionized water, heated at 70°C with stirring until the solution was evaporated to dryness and self-propagating combustion occurred, the powder was collected and calcined at 800°C in a muffle furnace for 2 h to obtain LDC primary powder, ball milled at a speed of 450 r / min for 12 h, and sieved through a 160-mesh sieve to obtain LDC powder;
[0039] (3) The doped lanthanum gallate electrolyte La 0.8 Sr 0.2 Ga 0.8 Mg 0.2 O 3-δ The (LSGM) powder was dry pressed under a pressure of 200 MPa and calcined at 1450 °C for 10 h to form a dense electrolyte;
[0040] (4) 2.50 g of LDC powder was mixed with 9.30 g of 6 wt.% ethyl cellulose-pinene alcohol mixture, heated at 60°C and stirred evenly, and then spin-coated on the surface of LSGM electrolyte at a speed of 2000 r / min, and calcined at 1200°C for 2 h to obtain an LDC interlayer;
[0041] (5) grinding the LSCC powder obtained in step (1), adding a mixture of ethyl cellulose-pinene alcohol having a mass fraction of 6 wt.%, and stirring evenly to obtain a cathode slurry;
[0042] (6) applying the cathode slurry on the surface of the LDC interlayer obtained in step (4), and calcining at 1100° C. for 2 h to obtain a perovskite cathode skeleton;
[0043] (7) Weigh 1.01 g of ferric nitrate nonahydrate powder and dissolve it in deionized water to make a volume of 10 ml to obtain 0.25 mol / L -1 of ferric nitrate solution;
[0044] (8) The ferric nitrate solution obtained in step (7) is impregnated into the perovskite electrode skeleton obtained in step (6) by a microinjection method, and the impregnation solution is dried under an infrared lamp. The impregnated Fe content is 3 wt % of the mass of the LSCC electrode. The electrode is calcined at 800 ° C. in air for 2 h, and then treated at 800 ° C. in a 5% H2 / Ar atmosphere for 5 h to obtain a perovskite cathode modified with surface CoFe active particles.
[0045] Depend on Figure 1 As can be seen from the XRD spectrum shown, the characteristic peaks of CoFe alloy were detected in the perovskite sample. Figure 2 This is a scanning electron microscope image of LSCC perovskite. From the surface morphology, it can be seen that the original LSCC surface is smooth, while a large amount of CoFe metal nanoparticles are dissolved on the surface of the modified LSCC.
[0046] Example 2
[0047] La modified with surface CoFe active particles 0.6 Sr 0.4 Cr 0.9 Co 0.1 O 3-δ As cathode material, a solid oxide electrolytic cell is prepared, comprising the following steps:
[0048] (1) According to La 0.6 Sr 0.4 Cr 0.9 Co 0.1 O 3-δIn a stoichiometric ratio, 7.7942 g of lanthanum nitrate hexahydrate, 2.5396 g of strontium nitrate, 8.4032 g of chromium nitrate nonahydrate, 2.6193 g of cobalt nitrate hexahydrate, and 18.9126 g of citric acid monohydrate were dissolved in deionized water, 17.5344 g of ethylenediaminetetraacetic acid was added, and ammonia water was added dropwise to adjust the pH value of the solution to 8, and the solution was heated and stirred at 80°C until it was in a gel state, and the gel was heated in a heating furnace until self-propagating combustion occurred to obtain LSCC primary powder, which was transferred to a muffle furnace and calcined at 1300°C for 10 hours to obtain LSCC powder;
[0049] (2) According to La 0.4 Ce 0.6 O 2-δ The stoichiometric ratio of (LDC) was 8.6602 g of lanthanum nitrate hexahydrate, 13.0266 g of cerium nitrate nonahydrate and 5.6303 g of glycine were dissolved in deionized water, heated at 70°C with stirring until the solution was evaporated to dryness and self-propagating combustion occurred, the powder was collected and calcined at 800°C in a muffle furnace for 2 h to obtain LDC primary powder, ball milled at a speed of 450 r / min for 12 h, and sieved through a 160-mesh sieve to obtain LDC powder;
[0050] (3) The doped lanthanum gallate electrolyte La 0.8 Sr 0.2 Ga 0.8 Mg 0.2 O 3-δ The (LSGM) powder was dry pressed under a pressure of 200 MPa and calcined at 1450 °C for 10 h to form a dense electrolyte;
[0051] (4) 2.50 g of LDC powder was mixed with 9.30 g of 6 wt.% ethyl cellulose-pinene alcohol mixture, heated at 60 °C and stirred evenly, and then spin-coated on both sides of the LSGM electrolyte at a speed of 2000 r / min, and calcined at 1200 °C for 2 h to obtain an LDC interlayer;
[0052] (5) grinding the LSCC powder obtained in step (1), adding a mixture of ethyl cellulose-pinene alcohol having a mass fraction of 6 wt.%, and stirring evenly to obtain a cathode slurry;
[0053] (6) Apply cathode slurry on the LDC interlayer surface on one side and La on the other side. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ -Gd 0.2 Ce 0.2 O 2-δ (LSCF-GDC) anode slurry, calcined at 1100 °C for 2 h;
[0054] (7) Weigh 1.01 g of ferric nitrate nonahydrate powder and dissolve it in deionized water to make a volume of 10 ml to obtain 0.25 mol / L -1 of ferric nitrate solution;
[0055] (8) using a microinjection method to impregnate the iron nitrate solution obtained in step (7) into the LSCC electrode, and drying the impregnation solution under an infrared lamp, wherein the Fe content of the impregnation is 3 wt% of the mass of the LSCC electrode;
[0056] (9) The battery obtained in step (8) was loaded into a top-to-top tubular reactor (with a diameter of 15 mm), the temperature was raised to a reaction temperature of 800°C, and calcined for 2 h. A 5% by volume H2 and Ar mixed gas was introduced into the cathode gas chamber, and the mixture was treated at 800°C for 2 h. The atmosphere was changed to a 5% by volume N2 and CO2 mixed gas. The anode gas chamber was exposed to air and connected to an electrochemical workstation to test the linear sweep voltammetric curve and the chronoamperometric curve.
[0057] Figure 3 This is a scanning electron microscope image of the cross section of the SOEC full cell. It can be seen that SOEC has a sandwich structure, from top to bottom, it is LSCF-GDC anode, LSGM electrolyte, LDC separator and LSCC+3Fe cathode.
[0058] from Figure 4 a is the CO2 electrolysis performance of the solid oxide electrolytic cell of Comparative Example 1 and Example 2. It can be seen that the CO2 electrolysis current density of the solid oxide electrolytic cell using LSCC modified with surface CoFe active particles as electrodes is significantly improved; Figure 4 From the chronoamperometric curve of (b), the stability of the solid oxide electrolytic cell with LSCC modified with surface CoFe active particles as electrode is significantly improved.
[0059] Comparative Example 1
[0060] Take La 0.6 Sr 0.4 Cr 0.9 Co 0.1 O 3-δ As cathode material, a solid oxide electrolytic cell is prepared, comprising the following steps:
[0061] (1) According to La 0.6 Sr 0.4 Cr 0.9 Co 0.1 O 3-δIn a stoichiometric ratio, 7.7942 g of lanthanum nitrate hexahydrate, 2.5396 g of strontium nitrate, 8.4032 g of chromium nitrate nonahydrate, 2.6193 g of cobalt nitrate hexahydrate, and 18.9126 g of citric acid monohydrate were dissolved in deionized water, 17.5344 g of ethylenediaminetetraacetic acid was added, and ammonia water was added dropwise to adjust the pH value of the solution to 8, and the solution was heated and stirred at 80°C until it was in a gel state, and the gel was heated in a heating furnace until self-propagating combustion occurred to obtain LSCC primary powder, which was transferred to a muffle furnace and calcined at 1300°C for 10 hours to obtain LSCC powder;
[0062] (2) According to La 0.4 Ce 0.6 O 2-δ The stoichiometric ratio of (LDC) was 8.6602 g of lanthanum nitrate hexahydrate, 13.0266 g of cerium nitrate nonahydrate and 5.6303 g of glycine were dissolved in deionized water, heated at 70°C with stirring until the solution was evaporated to dryness and self-propagating combustion occurred, the powder was collected and calcined at 800°C in a muffle furnace for 2 h to obtain LDC primary powder, ball milled at a speed of 450 r / min for 12 h, and sieved through a 160-mesh sieve to obtain LDC powder;
[0063] (3) The doped lanthanum gallate electrolyte La 0.8 Sr 0.2 Ga 0.8 Mn 0.2 O 3-δ The (LSGM) powder was dry pressed under a pressure of 200 MPa and calcined at 1450 °C for 10 h to form a dense electrolyte;
[0064] (4) 2.50 g of LDC powder was mixed with 9.30 g of 6 wt.% ethyl cellulose-pinene alcohol mixture, heated at 60 °C and stirred evenly, and then spin-coated on both sides of the LSGM electrolyte at a speed of 2000 r / min, and calcined at 1200 °C for 2 h to obtain an LDC interlayer;
[0065] (5) grinding the LSCC powder obtained in step (1), adding a mixture of ethyl cellulose-pinene alcohol having a mass fraction of 6 wt.%, and stirring evenly to obtain a cathode slurry;
[0066] (6) Apply cathode slurry on the LDC interlayer surface on one side and La on the other side. 0.6 Sr 0.4 Co 0.2 Fe 0.8 O 3-δ -Gd 0.2 Ce 0.2 O 2-δ (LSCF-GDC) anode slurry, calcined at 1100 °C for 2 h;
[0067] (7) The battery obtained in step (6) is loaded into a top-to-top tubular reactor (with a diameter of 15 mm), and the temperature is raised to a reaction temperature of 800°C. A mixed gas of N2 and CO2 with a volume fraction of 5% is introduced into the cathode gas chamber, and the anode gas chamber is exposed to air. The battery is connected to an electrochemical workstation, and the linear sweep voltammetric curve and the chronoamperometric curve are tested.
[0068] The above embodiments are only preferred embodiments of the present invention and are not intended to limit the implementation methods. The protection scope of the present invention shall be subject to the scope defined in the claims. Other different forms of changes or modifications may be made based on the above description. Obvious changes or modifications derived therefrom are still within the protection scope of the present invention.
Claims
1. A method for preparing a perovskite cathode modified with surface active particles by an ion exchange method, characterized in that: The perovskite oxide with the chemical formula La 0.6 Sr 0.4 M’ 1-x M” x O 3-δ is impregnated with a precursor solution of G metal. After being subjected to high-temperature air calcination and high-temperature reducing atmosphere treatment in sequence, a perovskite cathode modified with surface active particles is obtained; where 0 < x < 1 and δ is the oxygen vacancy content; The active particles are alloy nanoparticles composed of G and M”; In the perovskite cathode of the surface-modified active particles, the perovskite contains G element in the crystal lattice.
2. The method for preparing a surface active particle modified perovskite cathode by ion exchange method according to claim 1, characterized in that: The M' is one or more of Cr, Mn, Ti, V, and Zr.
3. The method for preparing a surface active particle modified perovskite cathode by ion exchange method according to claim 1, characterized in that: The M" is one or more of Co and Ni.
4. The method for preparing a surface active particle modified perovskite cathode by ion exchange method according to claim 1, characterized in that: The metal G is Fe; The precursor solution of the G metal is an aqueous solution of a nitrate or an inorganic acid salt of the G metal.
5. The method for preparing a perovskite cathode modified with surface active particles by ion exchange method according to claim 1, characterized in that: The method comprises the following steps: (1) La 0.4 Ce 0.6 O 2-δ The powder was mixed with an ethyl cellulose-terpineol mixture to obtain an LDC interlayer slurry, which was then applied to the La 0.8 Sr 0.2 Ga 0.8 Mg 0.2 O 3-δ On the electrolyte side, calcination is performed to obtain an LDC separator; (2) La 0.6 Sr 0.4 M' 1-x M” x O 3-δ The powder is ground, and the ethyl cellulose-pinene alcohol mixture is added and stirred evenly to obtain a cathode slurry; (3) uniformly coating the cathode slurry obtained in step (2) on the surface of the LDC interlayer by screen printing, brushing or spin coating, and calcining at 1000-1200° C. in air for 2-5 h to obtain a perovskite cathode skeleton; (4) The precursor solution of metal G is impregnated into the perovskite electrode skeleton obtained in step (3) by a microinjection method, calcined in air, and then treated in a reducing gas to obtain a perovskite cathode modified with surface active particles.
6. The method for preparing a surface-active particle-modified perovskite cathode by an ion exchange method according to claim 5, wherein in step (4), the calcination temperature is 300-1000°C and the calcination time is 0.5-10h.
7. The method for preparing a surface-active particle-modified perovskite cathode by an ion exchange method according to claim 5, wherein in step (4), the reducing gas is a mixed gas of H2 and Ar or He; The flow rate of the reducing gas is 70-250 mL cm -2 min -1 ; The treatment temperature is 500-1000℃ and the treatment time is 1-10h.
8. A perovskite cathode modified with surface active particles obtained by the method according to any one of claims 1 to 7.
9. Use of the surface active particle modified perovskite cathode according to claim 8 in the preparation of a solid oxide electrolytic cell.
Citation Information
Cited By
Perovskite type fuel electrode, preparation method thereof and reversible solid oxide battery
CN119601685A
Perovskite dissolved metal nanoparticle composite material with nanofiber structure, preparation method and application of perovskite dissolved metal nanoparticle composite material in electrocatalytic methane conversion
CN119913557A
Perovskite type mixed conductor film with metal precipitated on surface, method for electrically driving in-situ precipitation of metal nanoparticles and application of perovskite type mixed conductor film
CN120082932A
Solid oxide electrolytic cell sheet anode material as well as preparation method and application thereof
CN120505660A