Sodium-ion battery positive electrode material as well as preparation method and application thereof
By doping titanium and calcium elements on the positive electrode material of sodium ion battery to form a cladding layer, the problem of poor stability and circulation performance of the material in the air is solved, and higher air stability and circulation performance are achieved, reducing the Manufacturing costs and greenhouse gas emissions.
Patent Information
- Application Number
- CN202410982551.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-08
AI Technical Summary
The stability and circulation performance of sodium ion battery positive electrode materials in the air are poor, and they are easy to react with carbon dioxide and water in the air, resulting in loss of active Na and degradation of battery cycle performance. The electrode slurry gel jelly increases manufacturing cost and greenhouse gas emissions.
Using a coating layer containing titanium and calcium, the content of titanium is higher than that of calcium, and a titanium gradient doping structure is formed through the sintering process. The titanium element reacts with residual alkali to form a fast ion conductor, and the calcium element forms a protective coating to reduce the secondary. Reaction and invasion of water and carbon dioxide improve the air stability and circulation performance of the material.
It significantly reduces the residual alkali content, slows down side reactions, improves the air stability and circulation performance of the positive electrode material, reduces the cost of using drying and dehumidification equipment, improves sodium ion transmission and capacity, and improves the overall performance of the material.
Smart Images

Figure CN118919685A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] Sodium-ion batteries are considered to be one of the sustainable alternatives to lithium-ion batteries due to their abundant resources and wide distribution. They are widely used in energy storage systems, especially electric vehicles. At present, the most promising cathode material for sodium-ion batteries is O3 layered oxide, but it easily reacts with carbon dioxide and water in the surrounding air, resulting in partial extraction of Na and the formation of residual alkali (NaOH, Na2CO3 or NaHCO3) on the surface of the particles, which not only leads to the loss of active Na and destroys the layered structure, but also has poor cyclability of sodium-ion batteries; at the same time, it also attacks the fluorine in the polyvinylidene fluoride (PVDF) binder, causing the electrode slurry to gel; in addition, during the charge and discharge process, the residual alkali reacts with the electrolyte to generate carbon dioxide, methane, hydrogen and other gases, resulting in battery volume expansion and further deterioration of cycle performance.
[0003] In the traditional cathode material manufacturing process, the existing mature lithium-ion manufacturing technology and infrastructure can be used to alleviate the above problems; for example, in the preparation process of cathode materials, grinding, screening, iron removal and sealing steps after annealing require the use of a drying room; the battery production process, including electrode preparation, battery assembly and electrochemical activation steps, should be carried out in a controlled environment to minimize exposure to air; due to the sensitivity of liquid electrolytes, the use of drying rooms in the battery assembly process has been standardized, but energy consumption accounts for 29.37% of the total manufacturing energy consumption, resulting in a significant increase in manufacturing costs and large-scale greenhouse gas emissions, which runs counter to the sustainable development goals of sodium-ion batteries.
[0004] Therefore, how to effectively optimize and modify the positive electrode materials of sodium ion batteries to improve their air stability and cycle performance is one of the technical problems that urgently need to be solved in this field. Summary of the invention
[0005] In view of this, the present invention provides a sodium ion battery positive electrode material to solve the problems of poor air stability and cycle performance of existing materials.
[0006] The present invention also provides a method for preparing the above-mentioned sodium ion battery positive electrode material.
[0007] In a first aspect, the present invention provides a sodium ion battery positive electrode material, comprising a base material and a coating layer coated on the outer surface of the base material, wherein the coating layer contains calcium and titanium elements, and based on the mass of the base material, the titanium content is higher than the calcium content, and the calcium content is 0.1wt%-0.5wt%, and the titanium content is 0.2wt%-1.0wt%.
[0008] In an optional embodiment, based on the mass of the matrix material, the calcium content is 0.1wt%-0.3wt%, and the titanium content is 0.3wt%-0.7wt%.
[0009] In an optional embodiment, the chemical formula of the matrix material is Na 1+a Ni b Fe c Mn 1-b-c O2, where 0.02≤a≤0.10, 0.2≤b≤0.4, 0.3≤c≤0.5.
[0010] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps:
[0011] (1) mixing a sodium source, a nickel source, an iron source, and a manganese source and sintering them once to obtain a matrix material;
[0012] (2) mixing the matrix material, titanium source and calcium source and performing secondary sintering to obtain;
[0013] The secondary sintering temperature is 750°C-900°C.
[0014] In an optional embodiment, the molar ratio of the sodium element in the sodium source, the nickel element in the nickel source, the iron element in the iron source, and the manganese element in the manganese source is 1.02-1.10: 0.2-0.4: 0.3-0.5: 0.3-0.5.
[0015] In an optional embodiment, the mass ratio of the matrix material, the titanium element in the titanium source, and the calcium element in the calcium source is 100:0.2-1.0:0.1-0.5.
[0016] In an optional embodiment, the sodium source includes at least one of sodium carbonate, sodium hydroxide, sodium bicarbonate, and sodium acetate.
[0017] In an optional embodiment, the nickel source includes at least one of nickel oxide, nickel hydroxide, nickel oxyhydroxide, and nickel acetate.
[0018] In an optional embodiment, the iron source includes at least one of ferric oxide, ferrosoferric oxide, and ferric acetate.
[0019] In an optional embodiment, the manganese source includes at least one of manganese dioxide, manganese trioxide, manganese tetraoxide, and manganese acetate.
[0020] In an optional embodiment, the titanium source includes at least one of titanium dioxide, titanium monoxide, titanium trioxide, and titanium oxalate.
[0021] In an optional embodiment, the calcium source includes at least one of calcium carbonate, calcium oxide, calcium hydroxide, and calcium oxalate.
[0022] In an optional embodiment, the primary sintering step includes: first heating the temperature to 900°C-1050°C at a heating rate of 1°C / min-5°C / min and sintering for 10h-24h, and then cooling the temperature to room temperature at a cooling rate of 0.5°C / min-1.5°C / min, and the sintering atmosphere is air.
[0023] In an optional embodiment, the secondary sintering step includes: first heating to 750°C-900°C at a heating rate of 1°C / min-5°C / min and sintering for 5h-10h, and then cooling to room temperature at a cooling rate of 0.5°C / min-1.5°C / min, and the sintering atmosphere is air.
[0024] In a third aspect, the present invention provides application of the above-mentioned sodium ion battery positive electrode material in a sodium ion battery.
[0025] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0026] 1. The positive electrode material for sodium ion battery provided by the present invention comprises a base material and a coating layer coated on the outer surface of the base material, wherein the coating layer comprises calcium and titanium, and the content of the titanium element is higher than the content of the calcium element based on the mass of the base material, and the content of the calcium element is 0.1wt%-0.5wt%, and the content of the titanium element is 0.2wt%-1.0wt%. The coating layer of the present invention comprises calcium and titanium elements, which are combined with the residual alkali on the surface of the base material to form a coating layer, which greatly reduces the residual alkali content, improves the side reaction between the material surface and the electrolyte, effectively slows down the flatulence problem caused by the side reaction, has excellent air stability and cycle performance, and the positive electrode slurry prepared by the positive electrode material has good stability at an ambient humidity below 20%, reduces the amount of moisture and other substances adsorbed by the positive electrode material in the air, and can greatly reduce the cost of using drying and dehumidification equipment; specifically:
[0027] The titanium element is coated on the outer surface of the base material and can combine with the residual alkali on the surface of the base material to form fast ion conductor sodium titanate, which greatly reduces the residual alkali on the surface of the material, thereby reducing the absorption of water and carbon dioxide in the air by the residual alkali, which is beneficial to improving air stability. The low residual alkali can also prevent alkaline substances from attacking the fluorine in the polyvinylidene fluoride (PVDF) binder, thereby improving the stability of the positive electrode material slurry; the fast ion conductor sodium titanate formed can also promote sodium ion transmission, which is beneficial to improving the capacity and cycle stability of the positive electrode material; if the titanium content is too small, the capacity of the material will be affected; if the content is too large, the air stability and cycle performance of the positive electrode material will deteriorate; the calcium element is coated on the outer surface of the base material to form a protective coating, which hinders the intrusion of water and carbon dioxide in the air and improves the air stability and cycle performance of the positive electrode material; if the calcium content is too small, it cannot completely block the water and carbon dioxide in the air, and the air stability improvement effect is not obvious, while the calcium content is too large, resulting in a too thick coating layer, which hinders the sodium ion transmission and increases the impedance. Although the air stability is significantly improved, the capacity of the material will be greatly reduced. The present invention simultaneously dopes titanium and calcium on the outer surface of the base material, and the combination of the two can greatly improve the cycle performance and stability of the material.
[0028] 2. The preparation method of the positive electrode material of the sodium ion battery provided by the present invention limits the secondary sintering temperature to 750°C-900°C, so that the titanium element penetrates deeply into the interior of the particles, stabilizes the lattice structure, forms a titanium gradient doping structure, and greatly improves the material cycle performance; at the same time, the titanium element reacts with the residual alkali on the surface of the particles to form a sodium titanate fast ion conductor, promotes the diffusion of sodium ions, and improves air stability; in addition, the calcium element forms a smooth coating on the surface of the particles, reduces the side reaction between the material surface and the electrolyte, and improves the cycle performance.
[0029] The present invention co-dopes titanium and calcium in the coating layer and performs secondary sintering at 750° C.-900° C., which can significantly reduce surface residual alkali, alleviate the occurrence of side reactions, and improve the air stability and cycle performance of the positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 It is a scanning electron microscope image of the positive electrode material prepared in Example 1 of the present invention.
[0032] Figure 2It is a comparison chart of the moisture content of the positive electrode materials prepared in Example 1 of the present invention and Comparative Examples 1 to 3.
[0033] Figure 3 It is a comparison chart of the viscosity values of the positive electrode materials of Example 1 of the present invention and Comparative Examples 1 to 3 after being made into slurries.
[0034] Figure 4 It is a comparison chart of the capacity retention values of button-type batteries made of the positive electrode materials of Example 1 of the present invention and Comparative Examples 1 to 3. DETAILED DESCRIPTION
[0035] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0036] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0037] In order to solve the problems existing in the above-mentioned related art, according to the first aspect of the present invention, the present invention provides a sodium ion battery positive electrode material, comprising a base material and a coating layer coated on the outer surface of the base material, wherein the coating layer contains calcium and titanium elements, and the content of the titanium element is higher than the content of the calcium element by the mass of the base material, and the content of the calcium element is 0.1wt%-0.5wt%, and the content of the titanium element is 0.2wt%-1.0wt%; preferably, the content of the calcium element is 0.1wt%-0.3wt%, and the content of the titanium element is 0.3wt%-0.7wt% by the mass of the base material; the chemical formula of the base material is Na 1+a Ni b Fe c Mn 1-b-c O2, where 0.02≤a≤0.10, 0.2≤b≤0.4, 0.3≤c≤0.5.
[0038] The coating layer of the present invention contains calcium and titanium elements, which are combined with the residual alkali on the surface of the base material to form a coating layer, which greatly reduces the residual alkali content, improves the side reaction between the material surface and the electrolyte, effectively alleviates the flatulence problem caused by the side reaction, and has excellent air stability and cycle performance. The positive electrode slurry prepared by using the positive electrode material has good stability when the ambient humidity is below 20%, reduces the amount of moisture and other substances adsorbed by the positive electrode material in the air, and can greatly reduce the cost of using drying and dehumidification equipment; specifically:
[0039] The titanium element is coated on the outer surface of the base material and can combine with the residual alkali on the surface of the base material to form fast ion conductor sodium titanate, which greatly reduces the residual alkali on the surface of the material, thereby reducing the absorption of water and carbon dioxide in the air by the residual alkali, which is beneficial to improving air stability. The low residual alkali can also prevent alkaline substances from attacking the fluorine in the polyvinylidene fluoride (PVDF) binder, thereby improving the stability of the positive electrode material slurry; the fast ion conductor sodium titanate formed also promotes sodium ion transmission, which is beneficial to improving the capacity and cycle stability of the positive electrode material; if the titanium content is too small, it will affect the capacity of the material; if the content is too large, it will cause the air stability and cycle performance of the positive electrode material to deteriorate; the calcium element is coated on the outer surface of the base material to form a protective coating, which hinders the intrusion of water and carbon dioxide in the air and improves the air stability and cycle performance of the positive electrode material; if the calcium content is too small, it cannot completely block the water and carbon dioxide in the air, and the air stability improvement effect is not obvious, while the calcium content is too large, resulting in a too thick coating layer, which hinders the sodium ion transmission and increases the impedance. Although the air stability is significantly improved, the capacity of the material will be greatly reduced. The present invention simultaneously dopes titanium and calcium on the outer surface of the base material, and the combination of the two can greatly improve the cycle performance and stability of the material.
[0040] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps:
[0041] (1) mixing a sodium source, a nickel source, an iron source and a manganese source, heating the mixture to 900°C-1050°C at a heating rate of 1°C / min-5°C / min in an air atmosphere, sintering the mixture for 10h-24h, and then cooling the mixture to room temperature at a cooling rate of 0.5°C / min-1.5°C / min to obtain a matrix material; the molar ratio of the sodium element in the sodium source, the nickel element in the nickel source, the iron element in the iron source and the manganese element in the manganese source is 1.02-1.10:0.2-0.4:0.3-0.5:0.3-0.5; the sodium source comprises at least one of sodium carbonate, sodium hydroxide, sodium bicarbonate and sodium acetate; the nickel source comprises at least one of nickel oxide, nickel hydroxide, nickel oxyhydroxide and nickel acetate; the iron source comprises at least one of ferric oxide, ferric oxide and ferric acetate; the manganese source comprises at least one of manganese dioxide, manganese trioxide, manganese tetraoxide and manganese acetate;
[0042] (2) After mixing the matrix material, titanium source and calcium source, the temperature is first increased to 750°C-900°C at a heating rate of 1°C / min-5°C / min in an air atmosphere for secondary sintering for 5h-10h, and then cooled to room temperature at a cooling rate of 0.5°C / min-1.5°C / min to obtain; the mass ratio of the matrix material, the titanium element in the titanium source, and the calcium element in the calcium source is 100:0.2-1.0:0.1-0.5; the titanium source includes at least one of titanium dioxide, titanium monoxide, titanium trioxide, and titanium oxalate; the calcium source includes at least one of calcium carbonate, calcium oxide, calcium hydroxide, and calcium oxalate.
[0043] The secondary sintering temperature is limited to 750℃-900℃, so that the titanium element can penetrate into the interior of the particles, stabilize the lattice structure, form a titanium gradient doping structure, and greatly improve the material's cycle performance; at the same time, the titanium element reacts with the residual alkali on the surface of the particles to form a sodium titanate fast ion conductor, which promotes the diffusion of sodium ions and improves air stability; in addition, the calcium element forms a smooth coating on the surface of the particles, reducing the side reactions between the material surface and the electrolyte and improving the cycle performance.
[0044] The present invention co-dopes titanium and calcium in the coating layer and performs secondary sintering at 750°C-900°C, which can greatly reduce the residual alkali on the surface while improving the air stability and cycle performance of the positive electrode material, effectively alleviating the occurrence of side reactions, and thus reducing battery gas production.
[0045] Example 1
[0046] This embodiment provides a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0047] (1) Sodium carbonate, nickel oxide, ferric oxide, and manganese dioxide are weighed and mixed according to a molar ratio of Na:Ni:Fe:Mn of 1.02:0.3:0.4:0.3 to obtain a solid mixture; the solid mixture is placed in a box furnace, heated to 980°C at a heating rate of 2°C / min in an air atmosphere, calcined for 12 hours, then cooled to room temperature at a cooling rate of 1°C / min, and crushed to obtain a matrix material Na 1.02 Ni 0.3 Fe 0.4 Mn 0.3 O2;
[0048] (2) The above-mentioned base material, titanium dioxide and calcium carbonate were weighed according to the mass ratio of base material: Ti: Ca being 100:0.4:0.2, mixed and placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined for 8 hours, then cooled to room temperature at a cooling rate of 1°C / min, and sieved to obtain a positive electrode material for a sodium ion battery; wherein, based on the mass of the base material, the content of titanium element is 0.4wt%, the content of calcium element is 0.2wt%, and the scanning electron microscope image of the positive electrode material is as follows: Figure 1 As shown in the figure, it can be seen that a smooth coating is formed on the surface of the single crystal particles after coating.
[0049] Example 2
[0050] This embodiment provides a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0051] (1) Sodium carbonate, nickel oxide, ferric oxide, and manganese dioxide are weighed and mixed according to a molar ratio of Na:Ni:Fe:Mn of 1.02:0.3:0.4:0.3 to obtain a solid mixture; the solid mixture is placed in a box furnace, heated to 980°C at a heating rate of 2°C / min in an air atmosphere, calcined for 12 hours, then cooled to room temperature at a cooling rate of 1°C / min, and crushed to obtain a matrix material Na 1.02 Ni 0.3 Fe 0.4 Mn 0.3 O2;
[0052] (2) The above-mentioned matrix material, titanium dioxide and calcium carbonate were weighed according to a mass ratio of matrix material: Ti: Ca of 100:0.3:0.1, mixed and placed in a box furnace, heated to 800°C at a heating rate of 2°C / min in an air atmosphere, calcined for 8 hours, then cooled to room temperature at a cooling rate of 1°C / min, and sieved to obtain a sodium ion battery positive electrode material; wherein, based on the mass of the matrix material, the content of titanium element is 0.3wt%, and the content of calcium element is 0.1wt%.
[0053] Example 3
[0054] This embodiment provides a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0055] (1) Sodium carbonate, nickel oxide, ferric oxide, and manganese dioxide are weighed and mixed according to a molar ratio of Na:Ni:Fe:Mn of 1.02:0.3:0.4:0.3 to obtain a solid mixture; the solid mixture is placed in a box furnace, heated to 980°C at a heating rate of 2°C / min in an air atmosphere, calcined for 12 hours, then cooled to room temperature at a cooling rate of 1°C / min, and crushed to obtain a matrix material Na 1.02 Ni0.3 Fe 0.4 Mn 0.3 O2;
[0056] (2) The above-mentioned base material, titanium dioxide and calcium carbonate were weighed according to the mass ratio of base material: Ti: Ca being 100:0.8:0.3, mixed and placed in a box furnace, heated to 800° C. at a heating rate of 2° C. / min in an air atmosphere, calcined for 8 h, then cooled to room temperature at a cooling rate of 1° C. / min, and sieved to obtain a sodium ion battery positive electrode material; wherein, based on the mass of the base material, the content of titanium element is 0.8wt%, and the content of calcium element is 0.3wt%.
[0057] Example 4
[0058] This embodiment provides a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0059] (1) Sodium hydroxide, nickel hydroxide, ferroferric oxide, and manganese trioxide were weighed and mixed according to a molar ratio of Na:Ni:Fe:Mn of 1.1:0.3:0.35:0.35 to obtain a solid mixture; the solid mixture was placed in a box furnace, heated to 900°C at a heating rate of 5°C / min in an air atmosphere, calcined for 24 hours, then cooled to room temperature at a cooling rate of 1.5°C / min, and crushed to obtain a matrix material Na 1.1 Ni 0.3 Fe 0.35 Mn 0.35 O2;
[0060] (2) The above-mentioned matrix material, titanium monoxide and calcium oxide were weighed according to a mass ratio of matrix material: Ti: Ca of 100:0.6:0.4, mixed and placed in a box furnace, heated to 900° C. at a heating rate of 5° C. / min in an air atmosphere, calcined for 5 h, then cooled to room temperature at a cooling rate of 1.5° C. / min, and sieved to obtain a sodium ion battery positive electrode material; wherein, based on the mass of the matrix material, the content of titanium element is 0.6wt%, and the content of calcium element is 0.4wt%.
[0061] Example 5
[0062] This embodiment provides a method for preparing a positive electrode material for a sodium ion battery, comprising the following steps:
[0063] (1) Sodium bicarbonate, nickel acetate, iron acetate, and manganese acetate were weighed and mixed according to a molar ratio of Na:Ni:Fe:Mn of 1.05:0.2:0.5:0.3 to obtain a solid mixture; the solid mixture was placed in a box furnace, heated to 1050°C at a heating rate of 1°C / min in an air atmosphere, calcined for 10 h, cooled to room temperature at a cooling rate of 0.5°C / min, and crushed to obtain a matrix material Na 1.05 Ni 0.2 Fe 0.5 Mn 0.3 O2;
[0064] (2) The above-mentioned base material, titanium oxalate and calcium oxalate are weighed according to the mass ratio of base material: Ti: Ca being 100:1.0:0.5, mixed and placed in a box furnace, heated to 750°C at a heating rate of 1°C / min in an air atmosphere, calcined in the box furnace for 10 hours, then cooled to room temperature at a cooling rate of 0.5°C / min, sieved, and a sodium ion battery positive electrode material is obtained; wherein, based on the mass of the base material, the content of titanium element is 1wt%, and the content of calcium element is 0.5wt%.
[0065] Comparative Example 1
[0066] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is substantially the same as the steps in Example 1, except that step (2) is omitted.
[0067] Comparative Example 2
[0068] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is substantially the same as the steps of Example 1, except that in step (2), calcium carbonate is replaced by titanium dioxide.
[0069] Comparative Example 3
[0070] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is substantially the same as the steps of Example 1, except that in step (2), titanium dioxide is replaced by calcium carbonate.
[0071] Comparative Example 4
[0072] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is substantially the same as the steps of Example 1, except that the mass ratio of matrix material: Ti: Ca is 100:1.4:0.6.
[0073] Comparative Example 5
[0074] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is substantially the same as the steps of Example 1, except that the mass ratio of matrix material: Ti: Ca is 100:0.2:0.2.
[0075] Comparative Example 6
[0076] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is substantially the same as the steps in Example 1, except that titanium dioxide is replaced by tungsten oxide.
[0077] Comparative Example 7
[0078] This comparative example provides a method for preparing a positive electrode material for a sodium ion battery, which is basically the same as the steps of Example 1, except that in step (2), the secondary sintering temperature is 650°C.
[0079] Experimental example
[0080] The positive electrode materials prepared in the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 7 were tested for residual alkali content, air stability, slurry stability, and electrical properties. The results are shown in Tables 1 and Figure 2-Figure 4 As shown:
[0081] Air stability test: 100 g of the positive electrode materials prepared in the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 7 were weighed and placed in a culture dish, flattened to a thickness of 5 mm, and then placed in an environment at room temperature of 25° C. and air humidity of 45% for 0 days, 1 day, 3 days, 5 days, and 7 days, and then the moisture content was tested using a Karl Fischer titrator;
[0082] Slurry stability test: The positive electrode materials, polyvinylidene fluoride (PVDF), and Super P (conductive carbon black SP) prepared in the above Examples 1 to 5 and Comparative Examples 1 to 7 were uniformly mixed in N-methylpyrrolidone at a mass ratio of 90:5:5 to prepare a slurry; 100 mL of the above slurry was measured and placed in a beaker, and placed in an environment with a room temperature of 25°C and an air humidity of 20% for 0 h, 0.5 h, 1 h, 2 h, 4 h, 8 h, 12 h, 18 h, and 24 h, and then the viscosity of the slurry was tested using a viscometer (speed of 1 rpm);
[0083] Electrical performance test: The positive electrode materials, polyvinylidene fluoride (PVDF), and Super P (conductive carbon black SP) prepared in the above-mentioned Examples 1-5 and Comparative Examples 1-7 were uniformly mixed in N-methylpyrrolidone at a mass ratio of 90:5:5, and the positive electrode plates were made by homogenization, coating, drying, and cutting. The metal Na plate was used as the counter electrode, the glass fiber was used as the diaphragm, and 1 mol / L NaPF6 was mixed in ethylene carbonate (EC) / dimethyl carbonate (DMC) / ethyl methyl carbonate (EMC) (volume ratio 1:1:0.5) solution as the electrolyte. The CR2032 button battery assembled with the positive electrode plate, glass fiber diaphragm, Na plate, gasket and shrapnel was placed in the blue electric test system for cycle performance test; the cycle performance test conditions were: voltage range 2.0V-4.0V, and 1C / 1C charge and discharge cycle 50 times for cycle performance test.
[0084] Table 1 Test results of residual alkali content of positive electrode materials prepared in various embodiments and comparative examples
[0085]
[0086]
[0087] Table 2 Moisture test results of positive electrode materials prepared in various embodiments and comparative examples
[0088]
[0089] Table 3 Viscosity test results of slurries prepared from positive electrode materials of various embodiments and comparative examples
[0090]
[0091]
[0092] Table 4 Cycle test results of button cells made from positive electrode materials prepared in various embodiments and comparative examples
[0093] Capacity retention rate (%) Example 1 96.64 Example 2 97.30 Example 3 95.46 Example 4 95.80 Example 5 94.67 Comparative Example 1 81.03 Comparative Example 2 89.22 Comparative Example 3 91.03 Comparative Example 4 87.65 Comparative Example 5 89.75 Comparative Example 6 88.31 Comparative Example 7 90.04
[0094] From the above table and Figure 2-Figure 4It can be seen that the positive electrode material prepared in the embodiment has a low residual alkali content and has excellent air stability, slurry stability and cycle performance; Comparative Example 1 has not been coated, and the material has a large degree of contact with the air, resulting in the highest residual alkali content, and the worst air stability, slurry stability and cycle performance; Comparative Example 2 and Comparative Example 3 are Ti-coated and Ca-coated, respectively. Compared with Comparative Document 1, the residual alkali content is less, and the air stability, slurry stability and cycle performance are not significantly improved; In Comparative Example 4, the Ti and Ca coating content is too much. After the residual alkali is consumed during the high-temperature sintering process, the remaining Ti and Ca elements exist in the form of oxides, which are easily absorbed by water when exposed to the air, resulting in poor air stability and slurry stability. In addition, the coating layer is too thick, which affects the sodium ion transmission and makes the cycle performance poor; in Comparative Example 5, the Ti and Ca coating contents are the same, which is not conducive to improving the air stability and slurry stability, and the cycle performance is poor. It also shows that the control of the titanium content to be higher than the calcium content in the present invention is helpful to reduce the residual alkali, which is beneficial to improve the air stability and slurry stability; in Comparative Example 6, W element is used for coating, and its ability to consume residual alkali is worse than that of Ti element, and the effect of improving the air stability and slurry stability is limited; in addition, the conductivity of the formed sodium tungstate ions is worse than that of sodium titanate, resulting in poor cycle performance; in Comparative Example 7, the secondary sintering temperature is low, and the residual alkali cannot be effectively consumed, resulting in poor air stability, slurry stability and cycle performance.
[0095] The results of Examples 1-5 indicate that the titanium content of the present invention is preferably 0.3wt%-0.7wt%, and the calcium content is preferably 0.1wt%-0.3wt%, which can further improve air stability and slurry stability, thereby improving cycle performance.
[0096] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A sodium ion battery positive electrode material, comprising a base material and a coating layer coated on the outer surface of the base material, characterized in that: The coating layer contains calcium and titanium. Based on the mass of the base material, the titanium content is higher than the calcium content, and the calcium content is 0.1wt%-0.5wt%, and the titanium content is 0.2wt%-1.0wt%.
2. The sodium ion battery positive electrode material according to claim 1, characterized in that Based on the mass of the base material, the calcium content is 0.1wt%-0.3wt%, and the titanium content is 0.3wt%-0.7wt%.
3. The sodium ion battery positive electrode material according to claim 1, characterized in that The chemical formula of the matrix material is Na 1+a Ni b Fe c Mn 1-b-c O2, where 0.02≤a≤0.10, 0.2≤b≤0.4, 0.3≤c≤0.
5.
4. A method for preparing a positive electrode material for a sodium ion battery according to any one of claims 1 to 3, characterized in that: The steps include: (1) mixing a sodium source, a nickel source, an iron source, and a manganese source and sintering them once to obtain a matrix material; (2) mixing the matrix material, titanium source and calcium source and performing secondary sintering to obtain; The secondary sintering temperature is 750°C-900°C.
5. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The molar ratio of the sodium element in the sodium source, the nickel element in the nickel source, the iron element in the iron source, and the manganese element in the manganese source is 1.02-1.10: 0.2-0.4: 0.3-0.5: 0.3-0.
5.
6. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The mass ratio of the matrix material, the titanium element in the titanium source, and the calcium element in the calcium source is 100: 0.2-1.0: 0.1-0.
5.
7. The method for preparing a positive electrode material for a sodium ion battery according to claim 4 or 5, characterized in that: The sodium source includes at least one of sodium carbonate, sodium hydroxide, sodium bicarbonate, and sodium acetate; And / or, the nickel source includes at least one of nickel oxide, nickel hydroxide, nickel oxyhydroxide, and nickel acetate; And / or, the iron source includes at least one of ferric oxide, ferrosoferric oxide, and ferric acetate; And / or, the manganese source includes at least one of manganese dioxide, manganese trioxide, manganese tetraoxide, and manganese acetate.
8. The method for preparing a positive electrode material for a sodium ion battery according to claim 4 or 6, characterized in that: The titanium source includes at least one of titanium dioxide, titanium monoxide, titanium trioxide, and titanium oxalate; And / or, the calcium source includes at least one of calcium carbonate, calcium oxide, calcium hydroxide and calcium oxalate.
9. The method for preparing a positive electrode material for a sodium ion battery according to claim 4, characterized in that: The primary sintering step comprises: firstly heating the temperature to 900°C-1050°C at a heating rate of 1°C / min-5°C / min and sintering for 10h-24h, then cooling the temperature to room temperature at a cooling rate of 0.5°C / min-1.5°C / min, and the sintering atmosphere is air; And / or, the secondary sintering step includes: first heating to 750°C-900°C at a heating rate of 1°C / min-5°C / min and sintering for 5h-10h, then cooling to room temperature at a cooling rate of 0.5°C / min-1.5°C / min, and the sintering atmosphere is air.
10. Use of the sodium ion battery positive electrode material according to any one of claims 1 to 3 or the sodium ion battery positive electrode material prepared by the preparation method according to any one of claims 4 to 9 in a sodium ion battery.
Citation Information
Cited By
Sodium-ion battery oxide single-crystal positive electrode material as well as preparation method and application thereof
CN120099640A
Sodium-ion battery positive electrode material, preparation method thereof and sodium-ion battery
CN120511277A
Layered oxide material and preparation method thereof, positive electrode material, positive electrode plate and sodium ion battery