Self-compacting white fair-faced concrete
By adjusting the ratio of white cement, gravel, sand and titanium dioxide in white clean water concrete, combined with high-efficiency water reducing agent, the problems of vibration strength and self-concentration effect during construction are solved, and high-quality self-concentration white clean water is achieved Concrete, suitable for complex special-shaped curved surface projects.
Patent Information
- Application Number
- CN202410995243.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, white clean water concrete has poor appearance quality due to complex structures and high vibration strength during construction, and it is difficult to achieve self-condensing effect, which affects construction efficiency and surface quality.
A specific ratio of white cement, gravel, sand and titanium dioxide is used, combined with a polycarboxylic acid-based high-efficiency water reducing agent, control the water cement ratio and the specifications of gravel, and combine the clean water effect and self-condensing effect through moderate vibration.
It realizes that the vibration strength is reduced without separating the water, ensuring that there is no bubble enrichment on the surface, and the concrete reaches C40 self-finishing grade, and the strengths of 7d and 28d reach 34MPa and 45MPa respectively, with good appearance quality and suitable for complex and special shapes. Surface engineering.
Smart Images

Figure BDA0004959973890000051 
Figure BDA0004959973890000052 
Figure BDA0004959973890000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete preparation, and in particular to a self-compacting white plain concrete. Background Art
[0002] Fair-faced concrete is formed in one step without any decoration, and directly uses the natural color of cast-in-place concrete as the finish. It is the product of the combination of human beings' increasing environmental awareness and new construction design concepts. In recent years, with the rapid development of construction projects, colored fair-faced concrete structures produced by adding some colorants have become more and more popular and are increasingly being promoted.
[0003] White fair-faced concrete is popular due to its beautiful appearance and space-saving properties. However, the current fair-faced concrete has a complex structure, dense reinforcement, and a large number of special-shaped structures, which makes it impossible to work during the pouring process. When performing fair-faced concrete construction, workers often adopt "blind vibration", which results in poor vibration effect, affecting the appearance quality after demoulding and the expression of the "fair-faced" effect.
[0004] Fair-faced concrete uses coarse aggregate of ordinary particle size and pays more attention to the expression of fair-faced effect, such as requiring no obvious bubbles on the surface. Self-compacting concrete emphasizes the workability of concrete. It has high fluidity, no segregation, and better uniformity and stability than fair-faced concrete. It can effectively reduce the vibration strength and improve the construction efficiency of concrete pouring. White fair-faced concrete uses white cement and titanium dioxide on the basis of ordinary fair-faced concrete. On the one hand, it increases the hydration heat of concrete. On the other hand, due to the increase in the specific surface area of the material and the increase in water absorption, the workability, cohesion and other working properties of white fair-faced concrete decrease. If the three are combined to form self-compacting white fair-faced concrete, it is expected to effectively combine the performance advantages of the three special concretes, make up for the performance defects among the three, and thus be more suitable for complex special-shaped curved surface fair-faced concrete projects.
[0005] "Self-compacting concrete", "plain concrete" and "white plain concrete" are inherently contradictory. For example, "self-compacting concrete" requires high fluidity because of the large amount of cementitious materials (450-550 kg / m3). At the same time, the high air content (2.5%-4.5%) will reduce the shear force and increase the flow rate; in order to prevent segregation and bleeding, the slurry viscosity is required to be high and the sand ratio is high (47%-55%). However, the above factors easily make bubbles accumulate on the surface of concrete and difficult to discharge, which contradicts the requirement of "plain concrete" to have no holes on the surface. "Bare concrete" should be vibrated to improve the filling property of concrete and discharge bubbles in concrete to reduce the surface pore content. Self-compacting concrete uses vibration to discharge bubbles, which will increase the possibility of segregation and bleeding, affecting the mechanical properties of concrete. Due to the different performance requirements of "self-compacting concrete", "plain concrete" and "white plain concrete", the raw material formula requirements are different, and even the specifications and dosages of some components are opposite. It is very difficult to design the material formula to form self-compacting white plain concrete. Summary of the invention
[0006] In order to overcome the defects of the prior art, a self-compacting white plain concrete is provided to solve the problem that the appearance quality after demoulding is affected by the use of traditional plain concrete and blind vibration in plain concrete projects with special-shaped curved surfaces.
[0007] To achieve the above object, a self-compacting white plain concrete is provided, comprising:
[0008] Each cubic meter of self-compacting white plain concrete is composed of the following components: 390-410 kg of white cement, 780-850 kg of sand, 880-920 kg of gravel, 5-10 kg of titanium dioxide, 8-9 kg of water reducer and water, and the water-binder ratio of the self-compacting white plain concrete is 0.38-0.45;
[0009] The fineness modulus of the sand is 2.8, the mud content of the sand is <2%, and the chloride ion content of the sand is <0.06%;
[0010] The stone is a graded stone with a particle size of 5 to 15 mm, and the bulk density of the stone is >1350 kg / m 3 The crushing value of the stone is ≤18%, the water absorption rate of the stone is ≤2%, the mud content of the stone is ≤0.5%, and the needle-shaped and flaky particle content of the stone is <8%.
[0011] Furthermore, the cement is PW 42.5 white cement.
[0012] Furthermore, the water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.
[0013] Furthermore, each cubic meter of self-compacting white plain concrete is composed of the following components: 400 kg of white cement, 840 kg of sand, 910 kg of gravel, 5 kg of titanium dioxide, 8 kg of water reducing agent and water, and the water-cement ratio of the self-compacting white plain concrete is 0.41.
[0014] Furthermore, the titanium dioxide is a rutile titanium dioxide pigment with a whiteness of ≥92% and a mesh size of ≥325 meshes.
[0015] Furthermore, the bulk density of the stone is 1510 kg / m 3 .
[0016] The beneficial effect of the present invention is that the self-compacting white clear water concrete of the present invention uses white cement as a cementitious material, stone as a coarse aggregate, sand as a fine aggregate, and titanium dioxide as a colorant. By controlling each component to the above-mentioned specific ratio and certain specifications, the concrete can achieve a clear water effect, and achieve a self-compacting effect without separating bleeding water. Specifically, the formula is adjusted to achieve high fluidity to reduce the vibration intensity during the construction process. At the same time, moderate vibration is used during the pouring of clear water concrete to achieve the purpose of "defoaming" and achieve a clear water effect. At the same time, under the premise of ensuring that bleeding water is not separated, the viscosity of the freshly mixed concrete is reduced to achieve a self-compacting effect.
[0017] The self-compacting white plain concrete of the present invention has good appearance quality, no obvious bubble enrichment on the surface, no segregation and bleeding phenomenon during the vibration process, and the concrete test block reaches the C40 self-compacting grade, and the 7d and 28d strengths reach 34MPa and 45MPa or more, respectively. DETAILED DESCRIPTION
[0018] The present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention.
[0019] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below in conjunction with the embodiments.
[0020] The invention provides a self-compacting white plain concrete. Each cubic meter of the self-compacting white plain concrete is composed of the following components: 390-410 kg of white cement, 780-850 kg of sand, 880-920 kg of gravel, 5-10 kg of titanium dioxide, 8-9 kg of water reducing agent and water. The water-cement ratio of the self-compacting white plain concrete is 0.38-0.45.
[0021] As a preferred embodiment, each cubic meter of self-compacting white plain concrete is composed of the following components: 400 kg of white cement, 840 kg of sand, 910 kg of gravel, 5 kg of titanium dioxide, 8 kg of water reducer and water, and the water-cement ratio of the self-compacting white plain concrete is 0.41.
[0022] In this embodiment, the cement is PW 42.5 white cement.
[0023] The present invention preferably uses the above-mentioned 425 grade cement of the same origin, the same brand and the same color, and is provided with an independent storage tank for storage, so as to avoid the different physical and chemical properties of cements from different manufacturers and different batches, which may cause the concrete cast by cements of different varieties and different manufacturers to have different colors or properties.
[0024] In the embodiments of the present invention, P.W42.5 cement produced in Jiangxi and provided by Yinshan Cement Plant is preferably used.
[0025] In this embodiment, the fineness modulus of the sand is 2.8, the mud content of the sand is less than 2%, and the chloride ion content of the sand is less than 0.06%. Only by using the sand with the above specific fineness modulus can it be well matched with other components, meet the requirements of appearance quality and other physical and mechanical properties, and achieve the self-compacting water-clearing effect.
[0026] In this embodiment, the stone is a graded stone with a particle size of 5 to 15 mm, and the bulk density of the stone is >1350 kg / m 3 The crushing value of the stone is ≤18%, the water absorption rate of the stone is ≤2%, the mud content of the stone is ≤0.5%, and the needle-shaped and flaky particle content of the stone is <8%.
[0027] As a preferred embodiment, the packing density of the stones is 1510kg / m 3 .
[0028] The graded stones of 5 to 15 mm can be well matched with other materials in the self-compacting white plain concrete of the present invention to produce excellent physical and mechanical properties.
[0029] In this embodiment, the water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.
[0030] In this embodiment,
[0031] Titanium dioxide is a rutile titanium dioxide pigment with a whiteness ≥92% and a mesh size ≥325.
[0032] In the self-compacting white plain concrete of the present invention, the amount of water is expressed as a water-cement ratio, which refers to the mass ratio of water used per cubic meter of concrete to all cementitious materials (i.e. cement). In the present invention, the water-cement ratio is 0.38 to 0.45, preferably 0.40.
[0033] The present invention has no special restrictions on the preparation method of the self-compacting plain concrete. The components are mixed into concrete slurry in a conventional manner known to those skilled in the art, and then poured. Specifically, the concrete slurry can be mixed in the following manner: gravel, sand, titanium dioxide, cement, water and admixtures are mixed and stirred to obtain a concrete mixture.
[0034] In the existing technology, white fair-faced concrete is favored due to its beautiful appearance and space-saving function. However, the current fair-faced concrete has a complex structure, dense reinforcement, and many special-shaped structures, which makes it impossible to work during the pouring process. When performing fair-faced concrete construction, workers often adopt "blind vibration", which results in poor vibration effect, affecting the appearance quality after demoulding and the expression of the "fair-faced" effect.
[0035] The self-compacting white plain concrete of the present invention can achieve the clear water effect of concrete through the above-mentioned specific component specifications and proportions, and achieve the self-compacting effect without separating bleeding water, and can be used for special working conditions where ordinary concrete cannot be used for pouring, such as complex and densely reinforced concrete engineering structures of level 2 or above, and difficult vibration. The test results show that the concrete provided by the present invention has good appearance quality, no obvious bubble enrichment on the surface, and no separation of bleeding water during the vibration process. The obtained material reaches the C40 self-compacting grade, and the 7d and 28d strengths reach 35MPa and 45MPa or more, respectively.
[0036] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0037] In the following examples, PW 42.5 cement was produced by Yinshan Cement Plant in Jiangxi Province.
[0038] The sand specifications are fineness modulus 2.8, mud content <2%, and chloride ion content <0.06%.
[0039] The specifications of the gravel are bulk density of 1510kg / m3, crushing value = 12.8%, water absorption rate = 0.90%, mud content ≤ 0.5%, and needle-shaped and flaky particle content < 8%.
[0040] The specification of titanium dioxide is a specific surface area of 30m 2 / g.
[0041] The polycarboxylic acid water reducer model is HQPC808-IV and is provided by Quzhou Dingsheng.
[0042] Example 1
[0043] 1.1 Raw material formula:
[0044]
[0045] 1.2 Preparation
[0046] Weigh gravel and sand, then weigh titanium dioxide and cement, and finally add water and water reducing agent. Start the mixer and stir for 120 seconds to obtain a concrete mixture.
[0047] 1.3 Performance Testing
[0048] The obtained concrete slurry was poured into a 150mm×150mm×150mm standard test block, rammed, and then cured (cured in a standard curing room with a temperature of 20±2°C and a relative humidity of>95%).
[0049] During the vibration process, no water segregation or bleeding occurred in the test block, and no bubbles were accumulated on the surface. After vibration and curing, various properties of the concrete test blocks were tested, see Table 1.
[0050] Table 1. Performance of concrete in Example 1
[0051]
[0052] It can be seen from the test results in Table 1 that the concrete test block has good self-compactness and mechanical properties. Among them, good working performance means that the concrete does not separate and bleed, the slurry wraps the stones and flows evenly during flow, and there is no stone accumulation phenomenon. The holes left after the bubbles are discharged are quickly closed within 5 seconds, and there is no phenomenon of bubbles not breaking or holes not closing after initial setting.
[0053] Example 2
[0054] 1.1 Raw material formula:
[0055]
[0056] 1.2 Preparation
[0057] Weigh gravel and sand, then weigh titanium dioxide and cement, and finally add water and water reducing agent. Start the mixer and stir for 120 seconds to obtain a concrete mixture.
[0058] 1.3 Performance Testing
[0059] The obtained concrete slurry was poured into a 150mm×150mm×150mm standard test block, rammed, and then cured (cured in a standard curing room with a temperature of 20±2°C and a relative humidity of>95%).
[0060] During the vibration process, no water segregation or bleeding occurred in the test block, and no bubbles were accumulated on the surface. After vibration and curing, various properties of the concrete test blocks were tested, see Table 2.
[0061] Table 2. Performance of concrete in Example 2
[0062]
[0063] It can be seen from the test results in Table 2 that the concrete test block has good self-compactness, mechanical properties and working performance. At the same time, the appearance quality of the test block is observed, and the results show that the surface of the test block is smooth, without defects such as honeycombs, and achieves a good clear water expression effect.
[0064] Example 3
[0065] 1.1 Raw material formula:
[0066]
[0067] 1.2 Preparation
[0068] Weigh gravel and sand, then weigh titanium dioxide and cement, and finally add water and water reducing agent. Start the mixer and stir for 120 seconds to obtain a concrete mixture.
[0069] 1.3 Performance Testing
[0070] The obtained concrete slurry is poured into a 150mm×150mm×150mm standard test block, rammed and then cured (cured in a standard curing room with a temperature of 20±2°C and a relative humidity of>95%).
[0071] During the vibration process, no water segregation or bleeding occurred in the test block, and no bubbles were accumulated on the surface. After vibration and curing, various properties of the concrete test blocks were tested, see Table 3.
[0072] Table 3. Performance of concrete in Example 3
[0073]
[0074] It can be seen from the test results in Table 3 that the concrete test block has good self-compactness, mechanical properties and working performance. At the same time, the appearance quality of the test block is observed, and the results show that the surface of the test block is smooth, without defects such as honeycombs, and achieves a good clear water expression effect.
[0075] Comparative Example 1
[0076] 1.1 Raw material formula:
[0077]
[0078] Weigh gravel and sand, then weigh titanium dioxide and cement, and finally add water and water reducing agent. Start the mixer and stir for 120 seconds to obtain a concrete mixture.
[0079] 1.2 Preparation
[0080] 1.3 Performance Testing
[0081] The obtained concrete slurry was poured into a 150mmx150mmx150mm standard test block, rammed, and then cured (cured in a standard curing room with a temperature of 20±2°C and a relative humidity of>95%).
[0082] The fluidity decreases during the vibration process. After vibration and curing, the various properties of the concrete specimens are tested, see Table 4.
[0083] Table 4. Performance of concrete of comparative example 1
[0084]
[0085] It can be seen from the test results in Table 4 that the various properties of the concrete test block have declined. At the same time, the appearance quality of the test block was observed, and the results showed that the diameter and number of bubbles on the surface of the test block increased, proving that the clear water expression effect of the concrete is not good. It is proved that good self-compacting performance and clear water expression effect can only be obtained within the ratio range of the present invention.
[0086] Comparative Example 2
[0087] On the basis of Example 2, all the small stones are replaced by large stones, as follows:
[0088] 1.1 Raw material formula:
[0089]
[0090] 1.2 Preparation
[0091] Weigh gravel and sand, then weigh titanium dioxide and cement, and finally add water and water reducing agent. Start the mixer and stir for 120 seconds to obtain a concrete mixture.
[0092] 1.3 Performance Testing
[0093] The obtained concrete slurry was poured into a 150mmx150mmx150mm standard test block, rammed, and then cured (cured in a standard curing room with a temperature of 20±2°C and a relative humidity of>95%).
[0094] The fluidity is poor during the vibration process and it is not easy to vibrate. After vibration and curing, the various properties of the concrete test blocks are tested and see Table 5.
[0095] Table 5. Performance of Concrete in Comparative Example 2
[0096]
[0097] It can be seen from the test results in Table 5 that the various properties of the concrete test block have significantly decreased. At the same time, the appearance quality of the test block was observed, and the results showed that the bubble area on the surface of the test block was significantly increased, and the bubble diameter and depth also increased, proving that the self-compacting white plain concrete has a poor clear water expression effect. It is proved that good self-compacting performance and clear water expression effect can only be obtained under the self-compacting white plain concrete ratio range of the present invention and the combination of the stone particle size.
[0098] It can be seen from Examples 1 to 3 and Comparative Examples 1 to 2 that, compared with Comparative Examples 1 to 2, the various properties of the self-compacting white plain concrete of Examples 1 to 3 of the present invention are significantly improved, proving that within the specific mix ratio range of the self-compacting white plain concrete of the present invention, the self-compacting white plain concrete can obtain good self-compacting performance and clear water expression effect.
[0099] The self-compacting white clear water concrete of the present invention uses white cement as a cementitious material, stone as a coarse aggregate, sand as a fine aggregate, and titanium dioxide as a colorant. By controlling each component to the above-mentioned specific ratio and certain specifications, the concrete can achieve a clear water effect, and achieve a self-compacting effect without separating bleeding water. Specifically, the formula is adjusted to achieve high fluidity to reduce the vibration intensity during the construction process. At the same time, moderate vibration is used during the pouring of clear water concrete to achieve the purpose of "defoaming" and achieve a clear water effect. At the same time, under the premise of ensuring that bleeding water is not separated, the viscosity of the freshly mixed concrete is reduced to achieve a self-compacting effect.
[0100] The self-compacting white plain concrete of the present invention has good appearance quality, no obvious bubble enrichment on the surface, no segregation and bleeding phenomenon during the vibration process, and the concrete test block reaches the C40 self-compacting grade, and the 7d and 28d strengths reach 34MPa and 45MPa or more, respectively.
[0101] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.
Claims
1. A self-compacting white plain concrete, It is characterized in that Each cubic meter of self-compacting white plain concrete is composed of the following components: 390-410 kg of white cement, 780-850 kg of sand, 880-920 kg of gravel, 5-10 kg of titanium dioxide, 8-9 kg of water reducer and water, and the water-binder ratio of the self-compacting white plain concrete is 0.38-0.45; The fineness modulus of the sand is 2.8, the mud content of the sand is <2%, and the chloride ion content of the sand is <0.06%; The stone is a graded stone with a particle size of 5 to 15 mm, and the bulk density of the stone is >1350 kg / m 3 The crushing value of the stone is ≤18%, the water absorption rate of the stone is ≤2%, the mud content of the stone is ≤0.5%, and the needle-shaped and flaky particle content of the stone is <8%.
2. The self-compacting white plain concrete according to claim 1, It is characterized in that The cement is PW 42.5 white cement.
3. The self-compacting white plain concrete according to claim 1, It is characterized in that The water reducing agent is a polycarboxylic acid-based high-efficiency water reducing agent.
4. The self-compacting white plain concrete according to claim 1, It is characterized in that Each cubic meter of self-compacting white plain concrete is composed of the following components: 400 kg of white cement, 840 kg of sand, 910 kg of gravel, 5 kg of titanium dioxide, 8 kg of water reducing agent and water, and the water-cement ratio of the self-compacting white plain concrete is 0.
41.
5. The self-compacting white plain concrete according to claim 1, It is characterized in that The titanium dioxide is a rutile titanium dioxide pigment with a whiteness of ≥92% and a mesh size of ≥325.
6. The self-compacting white plain concrete according to claim 1, It is characterized in that The bulk density of the stone is 1510kg / m 3 .
Citation Information
Patent Citations
Machine-made sand fair-faced concrete mixer
CN101353241A
Formula for preparing white faced as-cast finish concrete composition
CN101955342A
Self-compaction fair-faced concrete with strength grade of C50
CN102690089A
White self-compacting C40-pumping fair-faced concrete
CN108996969A
Large-expansion self-compacting bare concrete material and preparation method thereof
CN110467403A