Preparation method of low-carboxyl-terminated polyester
By adding heat stabilizers and antioxidants to the esterification and polycondensation reaction of polyester, and using epoxy groups glyceryl ethers as carboxyl end capping agents, the stability of the middle and low-end carboxyl polyesters in the prior art is solved and The problem of insufficient end carboxyl group content achieves higher polymer performance and stability, avoiding moisture-induced degradation and photodepolymerization.
Patent Information
- Application Number
- CN202411227961.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-12
AI Technical Summary
The preparation method of the middle and low-end carboxylic polyester in the prior art has problems such as insufficient end carboxylic content and poor stability, and the conventional methods have complicated steps, large equipment transformation, easy degradation of products, and unstable color.
By combining esterification reaction and polycondensation reaction, the polycondensation reaction is performed by adding heat stabilizers and antioxidants before or before the esterification reaction begins or ends, and then performing polycondensation reaction under high vacuum conditions, and adding carboxylated capping agents in the later stage of polycondensation. Anti-hydrolyzing agents and light stabilizers, epoxy glycerol ether compounds are used as carboxyl end capping agents, to control the end carboxyl content and increase the average molecular weight of the polymer.
It achieves a lower end carboxylic content and improved polymer performance, avoids degradation caused by moisture, ensures the stability and long-term storage effect of the product, and reduces the risk of depolymerization of the product under light.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester synthesis, in particular to a preparation method of a low-end carboxyl polyester. Background Art
[0002] Polyester (PET) is a compound obtained by polycondensation of polyacids and polyols. It usually refers to a semi-crystalline polymer formed by the condensation polymerization of terephthalic acid and ethylene glycol. Since its launch, its products have been widely used in clothing, packaging and other industries due to their excellent performance. It is the largest variety of synthetic fibers. Due to its excellent comprehensive performance, it maintains excellent physical properties in a wide temperature range, high impact strength, friction resistance, good rigidity, high hardness, low hygroscopicity, good dimensional stability, excellent electrical properties, and stability to most organic solvents and inorganic acids. Therefore, it has also been widely used as a non-fiber polymer material, and has further expanded to various containers, packaging materials, films, films, engineering plastics and other fields.
[0003] Polyester materials are used in different applications through modification and synthesis. In the process of processing, storage and use, they need to adapt to different use and processing environments, and therefore require different properties. Different environments are affected by the combined effects of internal and external factors (including light, heat, humidity, mechanical pressure), etc., and polyester ages, resulting in a gradual decline in material properties and loss of use function. Therefore, by taking appropriate measures to prevent or delay aging, the aging resistance of the material can be improved, the aging rate of the material can be slowed down, thereby broadening the scope of application and extending the service life.
[0004] The terminal carboxyl content is an important indicator of the quality of polyester materials. The terminal carboxyl content of conventional polyester is generally 30mmol / kg (only numbers are used in the following text, and the units are the same as in the previous text). The terminal carboxyl group is one of the main factors affecting the thermal / oxygen stability and hydrolysis stability of polyester chips. Since the acid is an esterification catalyst, the terminal carboxyl group can also catalyze the depolymerization reaction of the PET molecular chain. When the polyester molecules with high terminal carboxyl groups are affected by the external environment, such as temperature, humidity, and light, they will accelerate aging and degradation during processing, storage and use. Therefore, controlling the low terminal carboxyl content is beneficial to the storage, processing and use of polyester materials.
[0005] The Chinese invention patent with the patent number ZL95102732 discloses a method for reducing the terminal carboxyl group, by adding methanol (ethanol) alkali metal salt and alkali metal alcoholate in the later stage of polymerization, polymerizing to obtain a polymer with a viscosity of about 0.68, and after viscosity enhancement, a low-terminal carboxyl polyester can be obtained. This method has two disadvantages: 1. To reach more than 20 terminal carboxyl groups, it is necessary to increase the viscosity and condensation to about 10 in the later stage, the number of terminal carboxyl groups is still high, and the steps are cumbersome; 2. Alkylates of alkali metals are strong bases, which will cause serious degradation of polyester in the later stage, darkening of color, and increase of b value.
[0006] The Chinese invention patent with publication number CN115286777A provides a method for producing a low-end carboxyl biodegradable polyester copolymer. The main product is PBAT / PEST. It is necessary to use a late chain extender to carry out a chain extension reaction at 180°C-220°C, and then mix it with a modifier in a three-stage dynamic mixer to obtain the low-end carboxyl biodegradable polyester special material, and the stirring speed of the three-stage dynamic mixer. However, this method has a long preparation process and the polyester is severely degraded. The viscosity cannot be stabilized by late chain extension.
[0007] The Chinese invention patent with publication number CN103665788A prepares high viscosity modified PET copolyester by adding oxazoline compounds and hydroxy chain extenders. The low viscosity polyester is used to increase viscosity to achieve the purpose of reducing the terminal carboxyl group. The terminal carboxyl group can be controlled to about 6. This method also requires a two-step method to obtain, first produce low viscosity slices, and then modify them later. Because the viscosity cannot be controlled by the later viscosity increase method, the product stability is not good. At the same time, screw processing has a great influence on product stability.
[0008] The Chinese invention patent with the authorization announcement number CN106220835B discloses an organic amine-terminated low-end carboxyl polyester and its preparation method. The method is said to obtain a low-end carboxyl polyester. It is divided into two steps:
[0009] In step (1), part of the organic amines are added to the esterification reaction product, and a polycondensation reaction is carried out under high vacuum; after the reaction time is 2 hours, a carboxyl end-capping agent, an anti-hydrolysis agent, and a light stabilizer are added, and stirring and vacuuming are continued until the reaction end point; in step (2), at the end of the polycondensation reaction, the remaining organic amines are added for end-capping to obtain a polyester with a low end carboxyl content. This method has the following problems: 1. Organic amines are highly volatile and the formula cannot be stable; 2. Organic amines are alkaline, which will affect the color of the product and cause partial degradation; 3. When the organic amines are added at the later stage of the polymerization, they are not added under vacuum, but are added at normal pressure or high pressure, which brings in gas during stirring. When pelletizing is produced, bubbles are generated in the pellets, which has a great impact on the later drying and use.
[0010] Chinese invention patent with authorization announcement number CN109575254B. Low-end carboxyl polyester is obtained by adding carboxyl end-capping agent titanate before or after the esterification reaction for cross-linking and coupling end-capping. The end-capping agent titanate is alcoholamine titanate, phosphoric acid type monoalkoxy titanate or composite monoalkoxy titanate. Problems: 1. Polyester is easily cross-linked by the end-capping agent to produce gel, the kinematic viscosity of the polymer rises sharply and the degree of polymerization is difficult to increase; 2. Phthalate has catalytic and degradation catalytic properties, which affects the color of the product; 3. The terminal carboxyl group is basically above 10meq / kg, and it is difficult to reduce it to below 10meq / kg.
[0011] The Chinese invention patent with publication number CN109081929A proposes a method for preparing a hydrolysis-resistant polyester film, claiming to have invented a low-end carboxyl polyester. The purpose of reducing the end carboxyl group is achieved by using a phthalate catalyst. The same problems exist as the patent with authorization announcement number CN109575254B. In addition, after repeated experiments, the following problems were found: 1. The reduction of the end carboxyl group is unstable; 2. The product color is unstable, easy to degrade, and the b value increases.
[0012] The Chinese invention patent with the patent number ZL 200720038513.7 discloses a production device that can effectively control the terminal carboxyl group. The utility model adds a pipeline reactor between esterification and pre-polycondensation, and controls the terminal carboxyl group by injecting unequal amounts of ethylene glycol before and after the pipeline reactor and setting the temperature of the reactor. Compared with the existing technology, this method requires a lot of equipment modification and a large investment. At the same time, the pipeline reactor may undergo alcoholysis reaction instead of just esterification reaction, and reducing the terminal carboxyl group will also change the DEG content of the product. In addition, the water generated by esterification cannot be discharged smoothly in the pipeline, so it may hydrolyze and produce terminal carboxyl groups. Summary of the invention
[0013] In view of the deficiencies in the prior art, the present invention provides a method for preparing a low-terminal carboxyl polyester, which solves various problems in the prior art such as insufficient terminal carboxyl content and poor stability.
[0014] According to an embodiment of the present invention, a method for preparing a low-end carboxyl polyester comprises the following steps:
[0015] Esterification reaction: using dibasic acid and diol as raw materials, first prepare slurry, then add catalyst, stir evenly and add into reactor for esterification reaction, the esterification temperature is 220-270°C; wherein the molar ratio of dibasic acid to diol is 1:1.05-1:1.25; before or after the esterification reaction, add heat stabilizer and antioxidant, after the reaction is completed, obtain oligomer;
[0016] Polycondensation reaction: the oligomer prepared in the previous step is used as a raw material and put into a polycondensation kettle for polycondensation reaction. After reacting for at least 2 hours at a temperature of 270-285°C and a pressure of 50-120 Pa, a carboxyl end-capping agent is added and stirring and vacuuming are continued until the end of the reaction to obtain a polymer melt. Then, a carboxyl end-capping agent, an anti-hydrolysis agent and a light stabilizer are added, and after stirring evenly, the polyester chips are obtained by cooling, pelletizing and drying. The carboxyl end-capping agent is an epoxy group glycerol ether compound.
[0017] Preferably, the dibasic acid includes terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, diphenyl dicarboxylic acid and their derivatives, as well as oxalic acid, succinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, cyclohexanedicarboxylic acid and their derivatives; the derivatives refer to lower alkyl esters and acid anhydrides, and the dibasic acid is a mixture of one or more of the above substances.
[0018] Preferably, the diol includes a mixture of one or more of ethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, heptanediol, octanediol, diethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, and the like.
[0019] Preferably, the catalyst is added in an amount such that the antimony ion concentration is 200-250 ppm, and the catalyst includes one of ethylene glycol antimony, antimony acetate or antimony trioxide.
[0020] Preferably, the amount of the heat stabilizer added is 200-500 ppm, and the heat stabilizer includes a mixture of one or more of phosphoric acid, triethyl phosphate, trimethyl phosphate, triphenyl phosphite, and triethyl phosphate.
[0021] Preferably, the antioxidant is added in an amount of 500-700 ppm, and the antioxidant is a hindered phenol antioxidant, including one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
[0022] Preferably, the added amount of the carboxyl end-capping agent is 0.1 to 0.5% of the weight of the finished product, and the carboxyl end-capping agent includes one or more of ethylene glycol diglycidyl ether, terephthalic acid diglycidyl ester, epoxy resin active diluent 669, epoxy diluent 622, epoxy diluent 669, epoxy diluent X-652 or epoxy diluent D-678.
[0023] Preferably, the anti-hydrolysis agent is added in an amount of 0.3%-0.5% of the weight of the finished product, and the anti-hydrolysis agent is a (poly)carbodiimide compound.
[0024] Preferably, the light stabilizer is added in an amount of 500-1000 ppm, and the light stabilizer is a hindered amine compound, including one of light stabilizer 622, light stabilizer 944, and light stabilizer 770.
[0025] Preferably, the stabilizer, catalyst and antioxidant are prepared as ethylene glycol solutions and added; the catalyst is prepared as butanediol solution and added; the anti-hydrolysis agent and light stabilizer are prepared as master batches and then added; the carboxyl end-capping agent is a liquid and is added directly; the carboxyl end-capping agent, anti-hydrolysis agent and light stabilizer added in the later stage of polycondensation are all added using a sealed can with a nitrogen filling port.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The carboxyl end-capping agent used in the present invention is a linear molecule containing epoxy functional groups at both ends. While blocking the terminal carboxyl groups, the chain growth is achieved, thereby improving the average molecular weight of the polymer and the product performance. In addition, when the epoxy functional group is used as the carboxyl end-capping agent, the end-capping efficiency is high, no moisture is generated, and other end-capping agents are prevented from generating moisture and causing degradation, and new terminal carboxyl groups are generated;
[0028] 2. In the present invention, a carboxyl end-capping agent is added in the late stage of polymerization to perform carboxyl end-capping. In the late stage of the polycondensation stage, after entering high vacuum for a period of time, the system is substantially free of moisture. At this time, a carboxyl end-capping agent that is sensitive to moisture is added to avoid the side reaction caused by adding epoxy groups to end-cap the carboxyl groups when moisture still exists in the early reaction system, thereby ensuring the end-capping effect and avoiding degradation caused by excessive water content to produce new terminal carboxyl groups;
[0029] 3. The present invention also adds an anti-hydrolysis agent, which can produce a synergistic effect with the epoxy group and further reduce the terminal carboxyl content. At the same time, the addition of the anti-hydrolysis agent and the light stabilizer can prevent the product from depolymerizing and accumulating terminal carboxyl groups during storage, transportation and use. The anti-hydrolysis agent is added after the polymerization is completed to ensure that it will not be consumed in the early polycondensation process. The present invention also adds a light stabilizer, which can reduce the depolymerization of the product under light environment and the accumulation of carboxyl groups, which is beneficial to the polyester product to still have a good effect after long-term storage;
[0030] 4. The present invention adopts a higher molar ratio and a longer time for esterification, thereby ensuring a higher esterification rate. A higher esterification rate can control the terminal carboxyl group of the final product. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below in conjunction with embodiments.
[0032] In this embodiment, the stabilizer, catalyst, and antioxidant are prepared as ethylene glycol solutions and added; the anti-hydrolysis agent and light stabilizer are prepared as master batches and added; the carboxyl end-capping agent is a liquid and added directly; the carboxyl end-capping agent, anti-hydrolysis agent, and light stabilizer added in the later stage of polycondensation are all added using a sealed can with a nitrogen filling port.
[0033] Embodiment 1:
[0034] Weigh 2000g of terephthalic acid and 900g of ethylene glycol, add them to the reactor and stir evenly, then carry out esterification reaction at a reaction temperature of 256-262°C; after the esterification is completed, add catalyst, stabilizer, antioxidant, turn on the vacuum system, gradually establish vacuum, slowly reduce the reaction pressure to 50Pa, set the reaction temperature to 274-280°C, and carry out polycondensation reaction. After 2 hours of polycondensation reaction, add carboxyl end-capping agent, continue stirring and vacuuming until the reaction reaches the end point. Add anti-hydrolysis and light stabilizer, stir evenly, cool, pelletize, and dry to obtain low-end carboxyl polyester chips.
[0035] Embodiment 2:
[0036] Weigh 1650g of terephthalic acid, 350g of isophthalic acid, and 900g of ethylene glycol, add them into a reactor for esterification reaction, and the reaction temperature is 250-255°C; after the esterification is completed, add a catalyst, a stabilizer, and an antioxidant, turn on the vacuum system, gradually establish a vacuum, slowly reduce the reaction pressure to 50Pa, set the reaction temperature to 274-280°C, and carry out a polycondensation reaction; after 2 hours of reaction time, add a carboxyl end-capping agent, continue stirring and vacuuming until the reaction reaches the end point. Add anti-hydrolysis and light stabilizers, stir evenly, cool, pelletize, and dry to obtain high shrinkage film-grade polyester chips.
[0037] Embodiment 3:
[0038] Weigh 1850g of terephthalic acid and 1250g of 1,3-butanediol, add them to the reactor, then add 0.3g of tetrabutyl titanate, and carry out esterification reaction, the reaction temperature is 230-235℃, and the pressure is 40kpa; after the esterification is completed, add anti-hydrolysis agent, stabilizer, antioxidant, and the reaction pressure is slowly reduced to 30Pa, the reaction temperature is 258-265℃, and polycondensation reaction is carried out; after 2 hours, add 10g of carboxyl end-capping agent, continue stirring and vacuum until the reaction end; after the reaction is completed, add 8g of anti-hydrolysis agent and 2.5g of light stabilizer, stir evenly, cool, pelletize, and dry to obtain low-end carboxyl PBT slices. The slices are used for optical fiber coating materials and have anti-hydrolysis and anti-ultraviolet effects.
[0039] Embodiment 4:
[0040] Weigh 1840g of terephthalic acid, 160g of isophthalic acid, 770g of ethylene glycol, 150g of neopentyl glycol and 1g of germanium dioxide into a reactor for esterification reaction at a reaction temperature of 256-262°C. After the esterification is completed, add a catalyst, a stabilizer and an antioxidant, turn on the vacuum system, gradually establish a vacuum, slowly reduce the reaction pressure to 50Pa, set the reaction temperature to 274-280°C, and carry out a polycondensation reaction; after 2 hours of reaction time, add a carboxyl end-capping agent, continue stirring and evacuate until the reaction reaches the end point. Add an anti-hydrolysis and light stabilizer, stir evenly, cool, pelletize and dry to obtain a high-shrinkage film-grade polyester chip containing low-end carboxyl groups.
[0041] Embodiment 5:
[0042] Weigh 2000g of terephthalic acid, 650g of ethylene glycol, 350g of neopentyl glycol and 1g of germanium dioxide, add them into a reactor for esterification reaction, and the reaction temperature is 256-262°C. After the esterification is completed, add a catalyst, a stabilizer, and an antioxidant, turn on the vacuum system, gradually establish a vacuum, slowly reduce the reaction pressure to 50Pa, set the reaction temperature to 274-280°C, and carry out a polycondensation reaction; after 2 hours of reaction time, add a carboxyl end-capping agent, continue stirring and vacuuming until the reaction reaches the end point. Add an anti-hydrolysis and light stabilizer, stir evenly, cool, pelletize, and dry to obtain a high-shrinkage film-grade polyester chip containing low-end carboxyl groups.
[0043] Comparative Example 1:
[0044] Weigh 2000g of terephthalic acid and 900g of ethylene glycol, add them into a reactor for esterification reaction, and the reaction temperature is 256-262°C; after the esterification is completed, add a catalyst, a stabilizer, and an antioxidant, turn on the vacuum, slowly reduce the reaction pressure to 60Pa, set the reaction temperature to 274-280°C, and carry out a condensation reaction; after the reaction time is 2 hours, add a carboxyl end-capping agent, continue stirring and evacuate, and after reaching the reaction end point, cool, pelletize, and dry to obtain polyester chips.
[0045] Comparative Example 2:
[0046] Weigh 2000g of terephthalic acid and 900g of ethylene glycol, mix them evenly and add them into a reactor for esterification reaction at a reaction temperature of 256-262°C; after the esterification is completed, add a catalyst, a stabilizer and an antioxidant, turn on the vacuum, slowly reduce the reaction pressure to 40Pa, set the reaction temperature to 274-280°C, carry out a condensation reaction, and after reaching the reaction end point, cool, pelletize and dry to obtain polyester chips.
[0047] The test results of the above examples 1-5 and comparative examples 1-2 are shown in Table 1:
[0048]
[0049]
[0050] Table 1
[0051] It can be seen from Table 1 that the examples of the present invention have a significantly lower terminal carboxyl content than the comparative example.
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a low-end carboxyl polyester, It is characterized in that The steps include: Esterification reaction: using dibasic acid and diol as raw materials, first prepare slurry, then add catalyst, stir evenly and add into reactor for esterification reaction, the esterification temperature is 220-270°C; wherein the molar ratio of dibasic acid to diol is 1:1.05-1:1.25; before or after the esterification reaction, add heat stabilizer and antioxidant, after the reaction is completed, obtain oligomer; Polycondensation reaction: the oligomer prepared in the previous step is used as a raw material and put into a polycondensation kettle for polycondensation reaction. After reacting for at least 2 hours at a temperature of 270-285°C and a pressure of 50-120 Pa, a carboxyl end-capping agent is added and stirring and vacuuming are continued until the end of the reaction to obtain a polymer melt. Then, a carboxyl end-capping agent, an anti-hydrolysis agent and a light stabilizer are added, and after stirring evenly, the polyester chips are obtained by cooling, pelletizing and drying. The carboxyl end-capping agent is an epoxy group glycerol ether compound.
2. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The dibasic acids include terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, biphenyl dicarboxylic acid and their derivatives, as well as oxalic acid, succinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, cyclohexane dicarboxylic acid and their derivatives; the derivatives refer to lower alkyl esters and acid anhydrides, and the dibasic acid is a mixture of one or more of the above substances.
3. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The diol includes a mixture of one or more of ethylene glycol, propylene glycol, butylene glycol, pentanediol, hexanediol, heptanediol, octanediol, diethylene glycol, polyethylene glycol, polypropylene glycol, polybutylene glycol, and the like.
4. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The catalyst is added in an amount of 200-250 ppm of antimony ion concentration, and the catalyst includes one of ethylene glycol antimony, antimony acetate or antimony trioxide.
5. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The amount of the heat stabilizer added is 200-500 ppm, and the heat stabilizer includes a mixture of one or more of phosphoric acid, triethyl phosphate, trimethyl phosphate, triphenyl phosphite, and triethyl phosphate.
6. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The antioxidant is added in an amount of 500-700 ppm, and the antioxidant is a hindered phenol antioxidant, including one of antioxidant 1010, antioxidant 1076, and antioxidant 168.
7. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The added amount of the carboxyl end-capping agent is 0.1-0.5% of the weight of the finished product, and the carboxyl end-capping agent includes one or more of ethylene glycol diglycidyl ether, terephthalic acid diglycidyl ester, epoxy resin active diluent 669, epoxy diluent 622, epoxy diluent 669, epoxy diluent X-652 or epoxy diluent D-678.
8. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The amount of the anti-hydrolysis agent added is 0.3%-0.5% of the weight of the finished product, and the anti-hydrolysis agent is a (poly)carbodiimide compound.
9. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The light stabilizer is added in an amount of 500-1000 ppm. The light stabilizer is a hindered amine compound, including one of light stabilizer 622, light stabilizer 944 and light stabilizer 770.
10. A method for preparing a low-end carboxyl polyester as claimed in claim 1, Features: The stabilizer, catalyst and antioxidant are prepared as ethylene glycol solution and added; the catalyst is prepared as butanediol solution and added; the anti-hydrolysis agent and light stabilizer are prepared as master batches and added; the carboxyl end-capping agent is a liquid and added directly; the carboxyl end-capping agent, anti-hydrolysis agent and light stabilizer added in the later stage of polycondensation are all added using a sealed can with a nitrogen filling port.
Citation Information
Patent Citations
Modified PET copolyester and preparation method and application thereof
CN103665788A
Organic amine-terminated polyester with low-end carboxyl content and preparation method thereof
CN106220835B
Method for preparing hydrolysis resistant polyester film
CN109081929A
Preparation method of low-end carboxyl polyester
CN109575254B
Low-carboxyl-terminated biodegradable polyester and preparation method of special material thereof
CN115286777A
Cited By
Hydrolysis-resistant copolyester composition and preparation method thereof
CN121006033A