Method for step-by-step extraction of copper, selenium, gold and silver from copper anode slime by full-wet method

By using a two-stage selective leaching process, the treatment of copper anode mud is optimized with persulfate and hydrogen peroxide, which solves the problems of low copper leaching efficiency and incomplete selenium leaching in copper anode mud. This achieves efficient separation and recovery of copper, selenium, gold and silver, simplifies the process and reduces energy consumption.

CN118932176APending Publication Date: 2024-11-12KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410940942.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing copper anode mud treatment processes suffer from problems such as large equipment investment, lengthy processes, high energy consumption, low precious metal recovery rate, and environmental pollution. In particular, the leaching efficiency of copper is low and the leaching effect of selenium is not good, and commonly used oxidants can introduce impurities.

Method used

A two-stage selective leaching process was adopted. First, copper was selectively leached with persulfate, then selenium was leached with hydrogen peroxide, and finally gold and silver were recovered with thiourea solution. The reaction effect of each step was optimized by controlling reaction conditions such as temperature, time and liquid-solid ratio.

Benefits of technology

It achieves efficient and selective separation and recovery of copper, selenium, gold and silver, reduces the loss of precious metals, simplifies the process, avoids the discharge of heavy metal wastewater, improves copper leaching efficiency and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004944081640000031
    Figure BDA0004944081640000031
Patent Text Reader

Abstract

The invention discloses a method for extracting copper, selenium, gold and silver step by step from copper anode slime through a full-wet method, and aims to solve the problems of low selectivity and long flow in comprehensive utilization of anode slime, and the method comprises the following steps: (1) leaching the copper anode slime by using a potassium persulfate solution, and filtering to obtain copper removal slag and copper-containing leachate; (2) treating the copper-removed slag with reagents such as hydrogen peroxide, sulfuric acid and sodium chloride to extract selenium, and filtering to obtain selenium-containing leachate and selenium-removed slag; and (3) leaching the selenium-removed slag by using thiourea, sulfuric acid and an oxidizing agent, and filtering to obtain a leaching solution containing gold and silver. According to the method, the copper anode slime full-wet process is adopted, so that loss of precious metal in the roasting process is avoided, and pollution caused by emission of harmful metal oxides is reduced; selective leaching of copper and selenium is achieved in the pretreatment stage, and reference can be provided for the problem that copper and selenium ions are difficult to separate in a wet environment; in the post-treatment stage, gold and silver are recovered at the same time, precious metal is concentrated, loss is avoided, and follow-up step-by-step extraction is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrometallurgy, and in particular relates to a method for extracting copper, selenium, gold and silver from copper anode mud in a fully wet step-by-step manner. Background Art

[0002] Copper anode mud is an important "secondary resource" in the non-ferrous metal metallurgical process. It is an important raw material for refining valuable metals because it contains a large amount of valuable metals. The composition of copper anode mud is mainly affected by the composition of the copper anode plate, casting quality and electrolytic refining conditions, resulting in a very complex chemical composition and a large fluctuation in the content of various components. It usually contains valuable elements such as Cu, Pb, Se, Te, As, Sb, Bi, and precious metal elements such as Au and Ag. Among them, selenium is not only a trace element necessary for all organisms, but also an important industrial raw material, widely used in Metallurgy, glass, electronics, chemical industry, agriculture, medicine, biology and other fields; At present, 90% of selenium raw materials come from anode mud. The selenium grade in copper anode mud is about 4%-12%, mainly in the form of Cu2Se, Ag2Se, PbSe and elemental Se. The copper in copper anode mud mainly exists in the form of indefinite compounds composed of Cu2S, Cu2O, Cu2Se and Cu2Te. Silver mainly exists in the form of Ag, Ag2Se, Ag2Te, CuAgSe and AgCl. Gold is in the form of (Ag, AuTe) or free state.

[0003] The treatment process of copper anode mud can be divided into three types: traditional pyrometallurgical process, semi-wet process, and wet process. The traditional pyrometallurgical process has the disadvantages of large equipment investment, lengthy process, large amount of returned materials and low direct recovery rate of precious metals, and the exhaust dust contains toxic metal oxides such as As, Sb and Pb, which is easy to cause environmental pollution. The semi-wet process combines roasting and wet treatment. This method has problems such as high production cost, poor raw material adaptability, high energy consumption, and large amount of wastewater treatment. Due to its environmental, economic and technical advantages, the wet process has been widely used to extract valuable metals from low-grade ores or "secondary resources". In the wet smelting process, atmospheric pressure oxidation acid leaching has the advantages of simple equipment, simple operation process, small amount of sulfuric acid, and no silver loss in anode mud. Its disadvantage is that the oxidation of Cu2S and Cu2Se in anode mud is incomplete, and the copper leaching efficiency is low, generally between 80% and 85%. The copper leaching efficiency of high-pressure oxidation acid leaching is a common method, but it has problems such as high energy consumption and complex equipment. Summary of the invention

[0004] The present invention adopts persulfate to selectively leach copper in copper anode mud, avoids high leaching energy consumption and complex equipment problems, has almost no leaching effect on selenium, adopts H2O2 as a selenium oxidant, has a fast reaction speed, and does not discharge heavy metal wastewater. Therefore, a two-stage selective leaching of copper and selenium is adopted in the pretreatment stage, which avoids secondary separation of substances to a certain extent and reduces losses.

[0005] A two-stage leaching process was used to study the leaching rates of copper and selenium. Potassium persulfate was used to remove copper from copper anode mud, and then hydrogen peroxide was used to leach selenium. In the post-treatment stage, thiourea was used with ferric nitrate (ferric sulfate) and sulfuric acid as auxiliary agents to recover gold and silver from the leached residue, so that the precious metals were concentrated and loss was avoided. The subsequent extraction could also be carried out in steps.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions:

[0007] (1) Grinding the anode mud to a particle size of 75 μm, adding the ground anode mud to a persulfate solution with a concentration range of 2-20 g / L at a liquid-to-solid ratio of (10-20):1, the unit of the liquid-to-solid ratio is mL:g, stirring, leaching, filtering, and washing to obtain copper-removed slag and copper leaching solution.

[0008] (2) drying the copper removal slag, adding the copper removal slag to a leaching solution I at a liquid-solid ratio of (10-20):1, wherein the unit of the liquid-solid ratio is mL:g, stirring, leaching, filtering, and washing to obtain a deselenium removal slag and a selenium leaching solution; the leaching solution I is prepared from hydrogen peroxide, a soluble chloride salt, and sulfuric acid, wherein the concentration of hydrogen peroxide in the leaching solution I is 3-15%, the concentration of the soluble chloride salt is 2-12 g / L, and the concentration of the sulfuric acid is 0.2-0.8 mol / L.

[0009] (3) drying the deselenium residue, adding the dried deselenium residue to leaching solution II at a liquid-solid ratio of (10-20):1, where the unit of the liquid-solid ratio is mL:g; stirring, leaching, filtering, washing, and solid-liquid separation to obtain a filtrate containing gold and silver, wherein the leaching solution II is prepared from thiourea, ferric nitrate, and sulfuric acid, wherein the concentration of perthiourea in the leaching solution II is 5-30 g / L, the concentration of ferric nitrate is 1-8 g / L, and the concentration of sulfuric acid is 0.2-1 mol / L.

[0010] Preferably, the stirring leaching conditions in step (1) of the present invention are stirring leaching at 30-80° C. for 0.5-6 h.

[0011] Preferably, the stirring leaching conditions in step (2) of the present invention are: stirring leaching at a temperature of 30-80° C. for 0.5-4 h.

[0012] Preferably, the stirring leaching conditions in step (3) of the present invention are: stirring leaching at a temperature of 20-50° C. for 2-4 hours.

[0013] Preferably, the persulfate in step (1) of the present invention includes potassium persulfate, ammonium persulfate, and sodium persulfate.

[0014] Preferably, the soluble chloride salt in step (2) of the present invention includes sodium chloride, potassium chloride, and ammonium chloride.

[0015] The principle of the present invention is that the copper in the copper anode mud exists in complex forms, mainly in the form of compounds of Cu2S, Cu2O, Cu2Se, and Cu2Te, which react with potassium persulfate to produce CuSO4. The chemical reactions involved in this process are as follows:

[0016]

[0017] Cu2S+2K2S2O8=2CuSO4+2K2SO4+S

[0018] Cu2Se+2K2S2O8=2CuSO4+2K2SO4+Se

[0019] Cu2Te+2K2S2O8=2CuSO4+2K2SO4+Te

[0020] In step (2), selenium will enter the solution in the form of selenite in the hydrogen peroxide oxidation system, and the leached Ag + Reacts with NaCl to generate AgCl which enters the deselenization slag. The chemical reactions involved in this process are as follows:

[0021] Se+2H2O2=H2SeO3+H2O

[0022] Cu2Se+4H2O2+H2SO4=CuSO4+CuSeO3+5H2O

[0023] Ag2Se+3H2O2=Ag2SeO3+3H2O

[0024] Ag2SeO3+2NaCl=2AgCl+Na2SeO3

[0025] In step (3), the deselenized residue is leached in a thiourea acid solution, and Au and Ag enter the solution in the form of a complex, thereby achieving separation and recovery of Au and Ag; the chemical equation that may be involved in this process is as follows:

[0026]

[0027] The method for recovering copper, selenium, gold and silver by fully wet separation of copper anode mud of the present invention can use activated carbon as an adsorbent to extract and recover gold and silver in the leaching solution.

[0028] Beneficial effects of the present invention:

[0029] In the method for recovering copper, selenium, gold and silver by fully wet separation of copper anode mud of the present invention, potassium persulfate, hydrogen peroxide and thiourea are all prone to decomposition during the reaction process through the synergistic effect of various process steps and process parameters. It is necessary to optimize the reagent concentration, time, temperature and liquid-solid ratio to achieve the best selective separation and recovery effect of copper, selenium, gold and silver. When an oxidant containing metal ions such as manganese dioxide is used as a leaching agent, foreign metal ions (Mn 2+ ), which is not conducive to the subsequent recovery of copper and selenium; when potassium persulfate and hydrogen peroxide are used as leaching oxidants, the reaction speed is fast, no heavy metal wastewater is discharged, and new impurities generated by the decomposition of the oxidant during the leaching process are avoided while achieving selective separation of copper and selenium; in addition, there is no obvious extraction effect on gold and silver during the leaching process of copper and selenium, so that gold and silver are enriched in the reaction process, which not only shortens the gold and silver recovery process, but also reduces the loss of gold and silver. DETAILED DESCRIPTION

[0030] In order to gain a deeper understanding and effectively implement the invention, and verify the significant effect of the process optimization proposed in the invention on the copper anode mud treatment process, the invention is described in detail in combination with specific implementation cases. It should be noted that the invention is not limited to the examples listed below.

[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased on the market or prepared by existing methods.

[0032] The contents of various elements in the copper anode mud treated in the following examples and comparative examples are shown in Table 1 below.

[0033] Table 1: Chemical composition of copper anode mud (%)

[0034] element Pb S Cu Ag Se As Au content 23.03 8.91 8.08 7.59 6.32 2.13 0.09

[0035] Example 1

[0036] (1) The anode mud was ground to a particle size of 75 μm, and the ground anode mud was added to a persulfate solution with a concentration of 6 g / L at a liquid-to-solid ratio of 12:1. The unit of the liquid-to-solid ratio was mL:g. The solution was stirred and leached at 80°C for 1 h. After filtering and washing, the copper-removing slag and copper-containing leaching solution were obtained after solid-liquid separation. The copper content was determined by atomic absorption spectrometry, and the copper leaching rate was measured to be 87.23%.

[0037] (2) The copper removal slag is dried and added to the leaching solution I at a liquid-to-solid ratio of 12:1. The unit of the liquid-to-solid ratio is mL:g. The reaction temperature is controlled to be 50°C and stirred in an oil bath. After reacting for 1 hour, the deselenized slag and selenium leaching solution are obtained after solid-liquid separation. The leaching solution I is prepared from hydrogen peroxide, soluble chloride salt and sulfuric acid. The concentration of hydrogen peroxide in the leaching solution I is 3%, the concentration of soluble chloride salt is 4 g / L, and the concentration of sulfuric acid is 0.2 mol / L. At this time, the selenium leaching rate is measured to be 89.23%.

[0038] (3) drying the deselenium residue, adding the dried deselenium residue to leaching solution II at a liquid-to-solid ratio of 12:1, where the unit of the liquid-to-solid ratio is mL:g; stirring and leaching for 4 hours at a reaction temperature of 30°C, filtering, washing, and solid-liquid separation to obtain a filtrate containing gold and silver, wherein leaching solution II is prepared from thiourea, ferric nitrate, and sulfuric acid, wherein the concentration of perthiourea in leaching solution II is 5 g / L, the concentration of ferric nitrate is 1 g / L, and the concentration of sulfuric acid is 0.2 mol / L, and the leaching rates of gold and silver are 88.74% and 86.34%, respectively.

[0039] Example 2

[0040] (1) The anode mud was ground to a particle size of 75 μm, and the ground anode mud was added to a persulfate solution with a concentration of 20 g / L at a liquid-to-solid ratio of 20:1. The unit of the liquid-to-solid ratio was mL:g. The solution was stirred and leached at 40°C for 6 h. After filtering and washing, the copper-removed slag and copper-containing leaching solution were obtained after solid-liquid separation. The copper content was determined by atomic absorption spectrometry, and the copper leaching rate was measured to be 89.31%.

[0041] (2) The copper removal slag is dried and added to the leaching solution I at a liquid-solid ratio of 20:1, the unit of the liquid-solid ratio is mL:g, the reaction temperature is controlled to 80°C, and the mixture is stirred in an oil bath. After reacting for 4 hours, the deselenized slag and selenium leaching solution are obtained after solid-liquid separation; the leaching solution I is prepared from hydrogen peroxide, soluble chloride salt and sulfuric acid. The concentration of hydrogen peroxide in the leaching solution I is 15%, the concentration of soluble chloride salt is 12 g / L, and the concentration of sulfuric acid is 0.8 mol / L. At this time, the selenium leaching rate is measured to be 95.35%.

[0042] (3) drying the deselenium residue, adding the dried deselenium residue to leaching solution II at a liquid-to-solid ratio of 20:1, where the unit of the liquid-to-solid ratio is mL:g; stirring and leaching for 2 h at a reaction temperature of 60°C, filtering, washing, and then separating the solid and liquid to obtain a filtrate containing gold and silver. Leaching solution II is prepared from thiourea, ferric nitrate, and sulfuric acid. In the leaching solution II, the concentration of perthiourea is 30 g / L, the concentration of ferric nitrate is 6 g / L, and the concentration of sulfuric acid is 1 mol / L. At this time, the leaching rates of gold and silver are 89.81% and 94.72%, respectively.

[0043] Example 3

[0044] (1) The anode mud was ground to a particle size of 75 μm, and the ground anode mud was added to a persulfate solution with a concentration of 10 g / L at a liquid-to-solid ratio of 14:1. The unit of the liquid-to-solid ratio was mL:g. The solution was stirred and leached at 60°C for 2 h. After filtering and washing, the copper-removed slag and copper-containing leaching solution were obtained after solid-liquid separation. The copper content was determined by atomic absorption spectrometry, and the copper leaching rate was measured to be 98.72%.

[0045] (2) The copper removal slag is dried and added to the leaching solution I at a liquid-solid ratio of 12:1. The unit of the liquid-solid ratio is mL:g. The reaction temperature is controlled to 60°C and stirred in an oil bath. After reacting for 3 hours, the deselenized slag and selenium leaching solution are obtained after solid-liquid separation. The leaching solution I is prepared from hydrogen peroxide, soluble chloride salt and sulfuric acid. The concentration of hydrogen peroxide in the leaching solution I is 12%, the concentration of soluble chloride salt is 10 g / L, and the concentration of sulfuric acid is 0.4 mol / L. At this time, the selenium leaching rate is measured to be 95.84%.

[0046] (3) drying the deselenium residue, adding the dried deselenium residue to leaching solution II at a liquid-to-solid ratio of 12:1, where the unit of the liquid-to-solid ratio is mL:g; stirring and leaching for 4 hours at a reaction temperature of 40°C, filtering, washing, and solid-liquid separation to obtain a filtrate containing gold and silver, wherein leaching solution II is prepared from thiourea, ferric nitrate, and sulfuric acid, wherein the concentration of perthiourea in leaching solution II is 20 g / L, the concentration of ferric nitrate is 3 g / L, and the concentration of sulfuric acid is 0.5 mol / L. At this time, the leaching rates of gold and silver are 91.23% and 89.24%, respectively.

[0047] Comparative Example 1

[0048] Compared with the embodiment, other conditions remain unchanged, potassium persulfate is replaced with manganese dioxide and sulfuric acid, and copper and selenium can be leached simultaneously. The anode mud is ground to a particle size of 75 μm, and the ground anode mud is added to the leaching solution I at a liquid-solid ratio of 14:1. The unit of the liquid-solid ratio is mL:g. The leaching solution I is prepared from manganese dioxide and sodium sulfate, with a manganese dioxide concentration of 10 g / L and a sulfuric acid concentration of 0.5 mol / L. The leaching is stirred at 60°C for 2 hours, filtered, washed, and solid-liquid separated to obtain leaching residue and copper- and selenium-containing leaching solutions. The copper and selenium contents are measured respectively, and the copper and selenium leaching rates are measured to be 69.23% and 55.78%, respectively.

[0049] The leaching residue is dried and added to the leaching solution II at a liquid-to-solid ratio of 14:1, and the unit of the liquid-to-solid ratio is mL:g; the leaching is stirred for 4 hours at a reaction temperature of 40°C, and the filtrate containing gold and silver is obtained by solid-liquid separation after filtering and washing. The leaching solution II is prepared from potassium chlorate and sulfuric acid, the concentration of potassium perchlorate is 5g / L, and the concentration of sulfuric acid is 0.2mol / L. At this time, the leaching rates of gold and silver are 89.74% and 4.32%, respectively.

[0050] At this time, the leaching rates of copper and selenium are very low, and foreign metal ions (Mn 2+ ), resulting in complicated subsequent separation; when potassium chlorate is used to leach gold and silver, gold has a better leaching effect, while silver is converted into silver chloride precipitation, which requires a step of extraction. In addition, potassium chlorate is corrosive and toxic, and has certain hazards and damages to the human body.

[0051] Comparative Example 2

[0052] Compared with the embodiment, the anode mud is ground to a particle size of 75 μm, and the ground anode mud is added to the leaching solution I at a liquid-solid ratio of 14:1. The unit of the liquid-solid ratio is mL:g. The leaching solution I is prepared from hydrogen peroxide, sulfuric acid and sodium chloride. The hydrogen peroxide concentration is 24%, the sulfuric acid concentration is 0.5 mol / L, and the sodium chloride concentration is 10 g / L. The leaching is stirred at 60° C. for 2 h, filtered, washed, and solid-liquid separated to obtain a leaching residue and a copper- and selenium-containing leaching solution. The copper and selenium contents are determined respectively, and the copper and selenium leaching rates are measured to be 61.78% and 89.78%, respectively.

[0053] The leaching residue is dried and added to the leaching solution II at a liquid-to-solid ratio of 14:1, and the unit of the liquid-to-solid ratio is mL:g; the leaching is stirred for 4 hours at a reaction temperature of 40°C, and the filtrate containing gold and silver is obtained by solid-liquid separation after filtering and washing. The leaching solution II is prepared from potassium chlorate and sulfuric acid, the concentration of potassium perchlorate is 5g / L, and the concentration of sulfuric acid is 0.2mol / L. At this time, the leaching rates of gold and silver are 89.74% and 4.32%, respectively.

[0054] At this time, hydrogen peroxide has a good leaching rate for selenium, but it will also extract a portion of copper, causing the copper to be dispersed and difficult to recover in a centralized manner, resulting in complicated subsequent separation. When potassium chlorate is used to leach gold and silver, it has a good leaching effect on gold, while silver is converted into silver chloride precipitate, which requires a one-step extraction. In addition, potassium chlorate is corrosive and toxic, and poses certain hazards and damages to the human body.

Claims

1. A method for extracting copper, selenium, gold and silver from copper anode mud by a fully wet method, characterized in that: The specific steps include: (1) grinding the anode mud to a particle size of 75 μm, adding the ground anode mud to a persulfate solution with a concentration range of 2-20 g / L at a liquid-to-solid ratio of (10-20):1, the unit of the liquid-to-solid ratio being mL:g, stirring, leaching, filtering, and washing to obtain a copper-removed slag and a copper leaching solution; (2) drying the copper removal slag, adding the copper removal slag to the leaching solution I at a liquid-solid ratio of (10-20):1, the unit of the liquid-solid ratio is mL:g, stirring, leaching, filtering, and washing to obtain the deselenium removal slag and selenium leaching solution; the leaching solution I is prepared from hydrogen peroxide, soluble chloride salt, and sulfuric acid, wherein the concentration of hydrogen peroxide in the leaching solution I is 3-15%, the concentration of soluble chloride salt is 2-12 g / L, and the concentration of sulfuric acid is 0.2-0.8 mol / L; (3) drying the deselenium residue, adding the dried deselenium residue to leaching solution II at a liquid-to-solid ratio of (10-20):1, where the unit of the liquid-to-solid ratio is mL:g; stirring, leaching, filtering, washing, and solid-liquid separation to obtain a filtrate containing gold and silver, wherein the leaching solution II is prepared from thiourea, ferric nitrate, and sulfuric acid, wherein the concentration of thiourea in the leaching solution II is 5-30 g / L, the concentration of ferric nitrate is 1-8 g / L, and the concentration of sulfuric acid is 0.2-1 mol / L.

2. The method for extracting copper, selenium, gold and silver from copper anode mud by fully wet stepwise method according to claim 1, characterized in that: The stirring and leaching conditions in step (1) are: stirring and leaching at 30-80° C. for 0.5-6 h.

3. The method for extracting copper, selenium, gold and silver from copper anode mud by fully wet stepwise method according to claim 1, characterized in that: The stirring and leaching conditions in step (2) are: stirring and leaching at a temperature of 30-80° C. for 0.5-4 h.

4. The method for extracting copper, selenium, gold and silver from copper anode mud by fully wet stepwise method according to claim 1, characterized in that: The stirring and leaching conditions in step (3) are: stirring and leaching at a temperature of 20-50° C. for 2-4 hours.

5. The method for extracting copper, selenium, gold and silver from copper anode mud by fully wet stepwise method according to claim 1, characterized in that: The persulfate in step (1) includes potassium persulfate, ammonium persulfate and sodium persulfate.

6. The method for extracting copper, selenium, gold and silver from copper anode mud by fully wet stepwise method according to claim 1, characterized in that: The soluble chloride salt in step (2) includes sodium chloride, potassium chloride and ammonium chloride.

Citation Information

Cited By

  • Method for extracting copper and selenium step by step through low-temperature sulfating roasting of copper anode slime

    CN120249666A