Aluminum alloy plate and preparation method thereof
By performing multiple steps on aluminum alloy sheets, including homogenization, hot rolling, cold rolling, solid solution and quenching, the problems of low mechanical properties and intergranular corrosion resistance of aluminum alloy sheets are solved, and the mechanical properties of the sheets are improved And corrosion resistance, suitable for automotive exterior covering parts.
Patent Information
- Application Number
- CN202411244003.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-12
AI Technical Summary
Existing aluminum alloy sheets have problems with low mechanical properties and intergranular corrosion resistance, which are difficult to meet the needs of automobile body styling and performance stability.
The aluminum alloy ingots are sequentially homogenized, hot rolled, first cold rolled, intermediate annealing, second cold rolled, solid solution treatment, quenching, straightening and pre-aging treatment, and control the solid solution treatment. The temperature and time are to ensure uniform dissolution of alloy solute elements and control the size of the grain boundary precipitation phase, thereby improving the tensile strength and intergranular corrosion resistance of aluminum alloy sheets.
The paint strength, tensile strength and intergranular corrosion resistance of aluminum alloy sheets are improved, stamping forming performance and production efficiency are enhanced, and production costs are reduced.
Smart Images

Figure BDA0005030089580000091 
Figure BDA0005030089580000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloys, and in particular to an aluminum alloy plate and a preparation method thereof. Background Art
[0002] 6111 aluminum alloy belongs to the 6xxx series Al-Mg-Si alloy. It has excellent properties such as good formability, high baking strength and high surface quality. Therefore, it is widely used in automobile engine hoods, doors, tailgates, side panels and other body exterior coverings. Based on the consideration of green recycling, 6xxx series alloys are gradually used in body structural parts, doors and hood inner panels and other structural parts. The Cu content in 6111 aluminum alloy is higher than that of 6xxx series alloys such as 6016 and 6014. While achieving higher strength, it also has a more serious tendency to intergranular corrosion.
[0003] 6xxx aluminum alloys use heat treatment methods such as solution treatment, quenching, and aging to regulate the precipitation of a large number of nano-scale strengthening phases in the matrix, thereby achieving significant precipitation strengthening effects. At the same time, the grain boundary area forms typical non-uniform organizational characteristics: grain boundary precipitation phases and non-precipitation areas. The microstructural inhomogeneity makes 6xxx aluminum alloys prone to local corrosion such as intergranular corrosion.
[0004] In order to meet the requirements of automobile body styling, 6xxx series aluminum alloy automobile sheets should have a suitable initial yield strength to ensure excellent stamping formability while taking into account the anti-dent performance of the body exterior covering. 6xxx series aluminum alloy automobile sheets should also have a high baking strength. As an aluminum alloy for automobiles, the performance stability of the material during service is the focus of industry attention, and in particular, it is required to have good resistance to intergranular corrosion.
[0005] In recent years, some domestic universities and research institutes have carried out a lot of work on the mechanical properties and intergranular corrosion performance of 6xxx series aluminum alloy body panels. At present, in order to improve the strength and intergranular corrosion resistance of the panels, most researchers mainly focus on the research of homogenization and aging processes, and relatively less on the solution process. The Chinese patent application with patent application number 201910141343.2 discloses that the problem of precipitation of dispersed phases in Al-Cu-Mg series aluminum alloys is overcome by homogenization heat treatment. In a short homogenization time, fine, uniform and dispersed AlCuMn phases can be precipitated in the matrix; after low-temperature short-time treatment, while eliminating the dendrite structure in the microstructure, the small amount of coarse phase remaining in the microstructure is controlled, so that the aluminum matrix is in an undersaturated state during solid solution, reducing the quenching sensitivity of the material, and inhibiting the precipitation of nano-scale second phases at the grain boundaries of the material after solid solution, thereby achieving the effect of improving production efficiency and improving the intergranular corrosion resistance of the product, but the mechanical properties of the material are not mentioned. The Chinese patent application with patent application number 201010134389.0 discloses that by adding trace scandium (Sc) to 6013 alloy, recrystallization and grain growth are hindered, and trace zirconium (Zr) is added on the basis of adding trace scandium to form a ternary coherent composite phase Al3 (Sc) with a smaller size than Al3Sc and better coherence with the matrix. 1-x , Zrx), which doubles the microalloying effect of Sc. The addition of trace strontium (Sr) has the functions of effectively purifying the melt, removing impurities, and refining the structure. It also protects the burning of Sc and Zr, and improves the intergranular corrosion resistance of 6013 alloy. However, the addition of trace rare earth elements such as Sc, Zr, and Sr increases the alloy cost, which is not suitable for promotion in the field of automotive aluminum alloy plates. The Chinese patent application with patent application number 202011025607.7 discloses that the precipitation of coarse phases during hot extrusion is suppressed by online quenching, so that the intergranular corrosion performance of Al-Mg-Mn-Er alloy extrusion products is improved, but the extrusion profile process is not suitable for the production of automotive aluminum alloy sheets. Summary of the invention
[0006] The main purpose of the present invention is to provide an aluminum alloy plate and a preparation method thereof, so as to solve the problem that the aluminum alloy plate in the prior art has low mechanical properties and low intergranular corrosion resistance.
[0007] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a method for preparing an aluminum alloy plate is provided, the preparation method comprising: subjecting an aluminum alloy ingot to a homogenization treatment, a hot rolling treatment, a first cold rolling treatment, an intermediate annealing treatment, a second cold rolling treatment, a solution treatment, a quenching treatment, a straightening treatment and a pre-aging treatment in sequence to obtain an aluminum alloy plate; wherein the temperature of the solution treatment is 540°C to 570°C, and the holding time of the solution treatment is 5 to 60s.
[0008] Furthermore, the temperature of the above-mentioned solution treatment is 540°C to 560°C; and / or the holding time of the solution treatment is 5 to 30s; and / or the heating rate of the solution treatment is 10 to 100°C / s, preferably 15 to 60°C / s.
[0009] Furthermore, the time interval between the completion of the insulation treatment of the above-mentioned solution treatment and the start of the quenching treatment is no more than 3s; and / or, the cooling rate of the quenching treatment is 8-100°C / s, preferably 27-60°C / s; and / or, the temperature of the material after quenching treatment is 10-35°C.
[0010] Furthermore, the time interval between the completion of the straightening treatment and the start of the pre-aging treatment is no more than 3 minutes; and / or the temperature of the pre-aging treatment is 70-120° C.; and / or the holding time of the pre-aging treatment is 4-10 hours.
[0011] Furthermore, the time interval between the completion of the quenching treatment and the start of the straightening treatment is no more than 1 minute; and / or the deformation amount of the straightening treatment is 0.2% to 0.5%; and / or the thickness of the material after the second cold rolling treatment is 0.7mm to 3mm.
[0012] Furthermore, the temperature of the above-mentioned homogenization treatment is 560°C; and / or, the holding time of the homogenization treatment is 8h; and / or, after the homogenization treatment is completed, the temperature is lowered to 510°C and then the hot rolling treatment is started; and / or, the temperature at the end of the hot rolling treatment is 270°C; and / or, the thickness of the material at the end of the hot rolling treatment is 6mm; and / or, the thickness of the material after the first cold rolling treatment is 1.4mm; and / or, the reduction rate of the first cold rolling treatment is 77%; and / or, the temperature of the intermediate annealing treatment is 475°C; and / or, the holding time of the intermediate annealing treatment is 30s; and / or, the reduction rate of the second cold rolling treatment is 29%.
[0013] Furthermore, the aluminum alloy ingot comprises the following elements, in percentage by mass: Si content is 0.50-1.50wt%, Fe content is ≤0.50wt%, Cu content is 0.50-1.0wt%, Mn content is 0.10-0.45wt%, Mg content is 0.25-1.20wt%, Cr content is ≤0.10wt%, Zn content is ≤0.15wt%, Ti content is ≤0.10wt%, the total content of unavoidable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
[0014] Furthermore, the above-mentioned aluminum alloy ingot includes the following elements: Si element content is 0.72~1.50wt%, Fe element content is 0.18~0.50wt%, Cu element content is 0.75~1.0wt%, Mn element content is 0.18~0.45wt%, Mg element content is 0.80~1.20wt%, Cr element content is 0.015~0.10wt%, Zn element content is 0.015~0.15wt%, Ti element content is 0.02~0.10wt%, the total content of inevitable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
[0015] According to another aspect of the present invention, an aluminum alloy plate is provided. The aluminum alloy plate is prepared by the aforementioned preparation method.
[0016] Furthermore, the yield strength of the above-mentioned aluminum alloy plate after being placed at 25°C for 7 days is 120-140MPa; and / or, the tensile strength of the aluminum alloy plate after being placed at 25°C for 7 days is not less than 270MPa; and / or, the elongation of the aluminum alloy plate after being placed at 25°C for 7 days is not less than 27%; and / or, the aluminum alloy plate after being placed at 25°C for 7 days is sequentially subjected to a 2% pre-stretching treatment and a baking treatment at 185°C for 20 minutes to obtain a treated aluminum alloy plate, and the yield strength of the treated aluminum alloy plate is not less than 230MPa; the tensile strength of the treated aluminum alloy plate is not less than 315MPa; the average intergranular corrosion depth of the treated aluminum alloy plate does not exceed 100μm.
[0017] By applying the technical solution of the present application, the aluminum alloy ingot is subjected to a homogenization treatment, which helps to improve the uniformity of element distribution in the aluminum alloy plate, thereby helping to improve the ductility and strength of the aluminum alloy plate; the hot rolling treatment helps to promote the diffusion of alloy elements and make the alloy structure more uniform, thereby helping to improve the plasticity and toughness of the aluminum alloy plate; the first cold rolling treatment helps to refine the grains, thereby helping to improve the strength and hardness of the aluminum alloy plate; the intermediate annealing treatment helps to promote the rearrangement of the microstructure inside the alloy and reduce the dislocation density, thereby reducing the hardening effect; the second cold rolling treatment helps to further refine the grains, thereby helping to further improve the tensile strength and toughness of the aluminum alloy plate; the solid solution treatment helps to dissolve the solute elements in the alloy more evenly in the aluminum matrix. If the temperature of the solution treatment is too low and the time is too short, it is not conducive to the full solution of the aluminum alloy, and thus it is not conducive to improving the strength of the aluminum alloy plate; if the temperature of the solution treatment is too high and the time is too long, the solubility of the solute atoms is too high, and the size of the grain boundary precipitation phase is large, which is not conducive to improving the uniformity of the microstructure, and thus it is not conducive to reducing the corrosion potential difference, and thus it is not conducive to improving the intergranular corrosion resistance. The average intergranular corrosion depth is too high, and the intergranular corrosion performance of the plate is unqualified. The present application controls the temperature and holding time of the solution treatment within the above range, which helps to fully dissolve the alloy solute atoms and accurately control the solubility of the solute atoms, thereby helping to control the size of the grain boundary precipitation phase, improve the uniformity of the microstructure, thereby helping to improve the tensile strength of the aluminum alloy plate, reduce the yield strength of the aluminum alloy plate, and reduce the corrosion potential difference of the aluminum alloy plate, thereby helping to improve the stamping forming performance and intergranular corrosion resistance of the aluminum alloy plate. Therefore, the preparation method of the present application can help improve the mechanical properties such as paint strength and intergranular corrosion resistance of the aluminum alloy plate on the one hand, and help improve the production efficiency and yield of the aluminum alloy plate on the other hand, thereby helping to save the production cost of the aluminum alloy plate. DETAILED DESCRIPTION
[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0019] As analyzed in the background technology of the present application, the aluminum alloy plates in the prior art have the problem of low mechanical properties and intergranular corrosion resistance. In order to solve this problem, the present application provides an aluminum alloy plate and a preparation method thereof.
[0020] It should be noted that the paint yield strength and paint tensile strength refer to the aluminum alloy sheet that has been parked for 7 days and then pre-stretched by 2% and then painted. The paint baking temperature is 185°C and the insulation time is 20 minutes to obtain the aluminum alloy sheet after paint treatment. The aluminum alloy sheet after paint treatment is subjected to yield strength and tensile strength tests to obtain the paint yield strength and paint tensile strength of the aluminum alloy sheet.
[0021] In a typical embodiment of the present application, a method for preparing an aluminum alloy plate is provided, the preparation method comprising: subjecting an aluminum alloy ingot to a homogenization treatment, a hot rolling treatment, a first cold rolling treatment, an intermediate annealing treatment, a second cold rolling treatment, a solution treatment, a quenching treatment, a straightening treatment and a pre-aging treatment in sequence to obtain an aluminum alloy plate; wherein the temperature of the solution treatment is 540°C to 570°C, and the holding time of the solution treatment is 5 to 60s.
[0022] Homogenizing the aluminum alloy ingot helps to improve the uniformity of element distribution in the aluminum alloy sheet, thereby helping to improve the ductility and strength of the aluminum alloy sheet; hot rolling treatment helps to promote the diffusion of alloy elements and make the alloy structure more uniform, thereby helping to improve the plasticity and toughness of the aluminum alloy sheet; the first cold rolling treatment helps to refine the grains, thereby helping to improve the strength and hardness of the aluminum alloy sheet; the intermediate annealing treatment helps to promote the rearrangement of the microstructure inside the alloy, reduce the dislocation density, and thus reduce the hardening effect; the second cold rolling treatment helps to further refine the grains, thereby helping to further improve the tensile strength and toughness of the aluminum alloy sheet; the solution treatment helps to make the solute elements in the alloy more uniformly dissolved in the aluminum matrix. It should be particularly emphasized that the temperature of the solution treatment used in this application is 540℃~570℃, and the holding time of the solution treatment is 5~60s. If the temperature and time of the solution treatment are too low and too short, it is not conducive to the full solid solution of the aluminum alloy, and thus it is not conducive to improving the strength of the aluminum alloy sheet; if the temperature and time of the solution treatment are too high, the solubility of the solute atoms is too high, and the size of the grain boundary precipitation phase is large, which is not conducive to improving the uniformity of the microstructure, and thus it is not conducive to reducing the corrosion potential difference, and thus it is not conducive to improving the intergranular corrosion resistance. The average intergranular corrosion depth is too high, and the intergranular corrosion performance of the sheet is unqualified. For example, the holding time of the solution treatment in the prior art is usually greater than 10 minutes, resulting in a high solubility of the solute atoms, so that the aluminum alloy sheet has a lower intergranular corrosion resistance. The present application controls the temperature and holding time of the solution treatment within the above range, which helps to fully dissolve the alloy solute atoms and accurately control the solubility of the solute atoms, thereby helping to control the size of the grain boundary precipitation phase, improve the uniformity of the microstructure, thereby helping to improve the tensile strength of the aluminum alloy sheet, reduce the yield strength of the aluminum alloy sheet, and reduce the corrosion potential difference of the aluminum alloy sheet, thereby helping to improve the stamping forming performance and intergranular corrosion resistance of the aluminum alloy sheet. Therefore, the preparation method of the present application can help improve the mechanical properties such as paint strength and intergranular corrosion resistance of the aluminum alloy plate on the one hand, and help improve the production efficiency and yield of the aluminum alloy plate on the other hand, thereby helping to save the production cost of the aluminum alloy plate.
[0023] In one embodiment of the present application, the temperature of the above-mentioned solution treatment is 540℃~560℃; and / or the holding time of the solution treatment is 5~30s; and / or the heating rate of the solution treatment is 10~100℃ / s, preferably 15~60℃ / s.
[0024] It is preferred to control the temperature and time of the solution treatment within the above range, which helps to further accurately control the solubility of the solute atoms, thereby helping to control the size of the precipitated phase at the grain boundary, improve the uniformity of the microstructure, reduce the corrosion potential difference, and thus help to improve the intergranular corrosion resistance of the aluminum alloy sheet. It is preferred to control the heating rate of the solution treatment within the above range, which helps to make the solid solution behavior of the alloy solute atoms occur in the solution insulation section, thereby helping to improve the stability of process parameters such as the solution temperature and insulation time, and thus help to improve the tensile strength and intergranular corrosion resistance of the aluminum alloy sheet. In addition, the heating rate of the above-mentioned solution treatment is based on the heating capacity of the continuous annealing furnace of the industrial production equipment for automotive aluminum alloy sheets, which meets the actual situation of large-scale industrial production sites and does not require additional equipment investment.
[0025] In one embodiment of the present application, the time interval between the completion of the insulation treatment of the above-mentioned solid solution treatment and the start of the quenching treatment is no more than 3s; and / or, the cooling rate of the quenching treatment is 8 to 100°C / s, preferably 27 to 60°C / s; and / or, the temperature of the material after quenching treatment is 10 to 35°C.
[0026] It is preferred to control the cooling rate of the quenching treatment within the above range, which helps to reduce the precipitation behavior of solute atoms during the cooling process of the aluminum alloy, thereby helping to improve the tensile strength of the aluminum alloy sheet. It is preferred to control the temperature of the cooling medium of the quenching treatment within the above range, which helps to control the cooling rate of the quenching treatment. In addition, the temperature of the cooling medium of the quenching treatment is 10 to 35°C, and the cooling medium is preferably water. It should be noted that the start of cooling is the time node for the start of the quenching treatment.
[0027] In one embodiment of the present application, the time interval between the completion of the straightening treatment and the start of the pre-aging treatment is no more than 3 minutes; and / or the temperature of the pre-aging treatment is 70-120° C.; and / or the holding time of the pre-aging treatment is 4-10 hours.
[0028] It is preferred to control the temperature and time of the pre-aging treatment within the above ranges, which helps control the formation and distribution of the precipitated phase, thereby helping to improve the tensile strength, hardness and plasticity of the aluminum alloy.
[0029] In one embodiment of the present application, the time interval between the completion of the quenching treatment and the start of the straightening treatment is no more than 1 minute; and / or the deformation amount of the straightening treatment is 0.2% to 0.5%; and / or the thickness of the material after the second cold rolling treatment is 0.7mm to 3mm.
[0030] Preferably, the deformation amount of the straightening treatment is controlled within the above range, which helps to reduce various defects generated in the production and processing of the aluminum alloy sheet, thereby helping to make the geometric dimensions of the aluminum alloy sheet meet the requirements of technical standards. Controlling the thickness of the material after the second cold rolling treatment within the above range helps to make the aluminum alloy sheet more suitable for automotive exterior panel sheets.
[0031] In order to further improve the mechanical properties and intergranular corrosion resistance of the aluminum alloy plate, in one embodiment of the present application, the temperature of the above-mentioned homogenization treatment is preferably 560°C; and / or, the holding time of the homogenization treatment is 8h; and / or, after the homogenization treatment is completed and the holding time is reduced to 510°C, the hot rolling treatment is started; and / or, the temperature at the end of the hot rolling treatment is 270°C; and / or, the thickness of the material at the end of the hot rolling treatment is 6mm; and / or, the thickness of the material after the first cold rolling treatment is 1.4mm; and / or, the reduction rate of the first cold rolling treatment is 77%; and / or, the temperature of the intermediate annealing treatment is 475°C; and / or, the holding time of the intermediate annealing treatment is 30s; and / or, the reduction rate of the second cold rolling treatment is 29%.
[0032] In one embodiment of the present application, the aluminum alloy ingot includes the following elements, measured in mass percentage: Si element content is 0.50-1.50wt%, Fe element content is ≤0.50wt%, Cu element content is 0.50-1.0wt%, Mn element content is 0.10-0.45wt%, Mg element content is 0.25-1.20wt%, Cr element content is ≤0.10wt%, Zn element content is ≤0.15wt%, Ti element content is ≤0.10wt%, the total content of unavoidable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
[0033] It is preferred to control the types and contents of elements in the aluminum alloy ingot within the above ranges, which helps to further improve the formability, paint strength, surface quality and other properties of the aluminum alloy sheet.
[0034] The method for preparing the aluminum alloy ingot comprises: melting, refining and casting various raw materials including metals in accordance with a proportion to obtain the aluminum alloy ingot.
[0035] In order to further improve the formability, paint strength and surface quality of the aluminum alloy sheet, in one embodiment of the present application, the above-mentioned aluminum alloy ingot preferably includes the following elements: the content of Si element is 0.72~1.50wt%, the content of Fe element is 0.18~0.50wt%, the content of Cu element is 0.75~1.0wt%, the content of Mn element is 0.18~0.45wt%, the content of Mg element is 0.80~1.20wt%, the content of Cr element is 0.015~0.10wt%, the content of Zn element is 0.015~0.15wt%, the content of Ti element is 0.02~0.10wt%, the total content of unavoidable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
[0036] In another typical embodiment of the present application, an aluminum alloy sheet is provided. The aluminum alloy sheet is prepared by the aforementioned preparation method.
[0037] The aluminum alloy sheet prepared by the preparation method of the present application, especially the aluminum alloy sheet prepared by using 6111 alloy, has high mechanical properties such as baking varnish strength and intergranular corrosion resistance.
[0038] In one embodiment of the present application, the yield strength of the above-mentioned aluminum alloy plate after being placed at 25°C for 7 days is 120-140MPa; and / or, the tensile strength of the aluminum alloy plate after being placed at 25°C for 7 days is not less than 270MPa; and / or, the elongation of the aluminum alloy plate after being placed at 25°C for 7 days is not less than 27%; and / or, the aluminum alloy plate after being placed at 25°C for 7 days is sequentially subjected to a 2% pre-stretching treatment and a baking treatment at 185°C for 20 minutes to obtain a treated aluminum alloy plate, and the yield strength of the treated aluminum alloy plate is not less than 230MPa; the tensile strength of the treated aluminum alloy plate is not less than 315MPa; the average intergranular corrosion depth of the treated aluminum alloy plate does not exceed 100μm.
[0039] The aluminum alloy sheet having the above-mentioned yield strength, tensile strength, paint yield strength, paint tensile strength and average intergranular corrosion depth range has more excellent stamping forming performance, intergranular corrosion resistance and stability, making the aluminum alloy sheet more suitable for use as an automobile exterior cover sheet.
[0040] The beneficial effects of the present application will be further illustrated below in conjunction with embodiments.
[0041] Example 1
[0042] The aluminum alloy components are, by mass percentage, Si: 0.72wt%, Fe: 0.18wt%, Cu: 0.75wt%, Mn: 0.18wt%, Mg: 0.80wt%, Cr: 0.015wt%, Zn: 0.015wt%, Ti: 0.02wt%, and the remainder is Al and impurities with a content of less than 0.05wt%.
[0043] The alloy was melted according to the above ratio, and the melt was refined (filtered with a 50ppi filter, degassed with argon online, and the hydrogen content was controlled to 0.13ml / 100g Al) and then cast an ingot using a semi-continuous casting device; the ingot is subjected to homogenization treatment after head cutting and milling, the homogenization treatment temperature is 560°C, and the homogenization treatment holding time is 8h; after the holding is completed, the temperature is lowered to 510°C and hot rolling is started, rolled to 6mm, and the final rolling temperature is 270°C; the first cold rolling is to 1.4mm, the first cold rolling reduction rate is 77%, the intermediate annealing temperature is 475°C, the annealing time is 30s, the second cold rolling is to 1.0mm, the cold rolling reduction rate is 29%, and then a solid solution treatment is performed, the temperature is increased to the solid solution treatment temperature of 560°C at a heating rate of 15°C / s, the holding time is 9s, quenched within 3s, cooled to 25°C at a cooling rate of 27°C / s, and straightened within 1min after cooling with a deformation of 0.3%, and the straightened plate is transferred to 80°C within 3min and kept at 80°C for 8h to finally obtain an aluminum alloy plate.
[0044] Example 2
[0045] The difference from Example 1 is that the heating rate of the solution treatment is 60° C. / s, and an aluminum alloy plate is finally obtained.
[0046] Example 3
[0047] The difference from Example 1 is that the heating rate of the solution treatment is 10°C / s, and an aluminum alloy plate is finally obtained.
[0048] Example 4
[0049] The difference from Example 1 is that the heating rate of the solution treatment is 100° C. / s, and an aluminum alloy plate is finally obtained.
[0050] Example 5
[0051] The difference from Example 1 is that the heating rate of the solution treatment is 9° C. / s, and an aluminum alloy plate is finally obtained.
[0052] Example 6
[0053] The difference from Example 1 is that the temperature of the solution treatment is 550° C., the holding time is 30 s, and finally an aluminum alloy plate is obtained.
[0054] Example 7
[0055] The difference from Example 1 is that the temperature of the solution treatment is 540° C., the holding time is 5 s, and finally an aluminum alloy plate is obtained.
[0056] Example 8
[0057] The difference from Example 1 is that the temperature of the solution treatment is 570° C., the holding time is 60 s, and finally an aluminum alloy plate is obtained.
[0058] Example 9
[0059] The difference from Example 1 is that the cooling rate of the quenching treatment is 60° C. / s, and an aluminum alloy plate is finally obtained.
[0060] Example 10
[0061] The difference from Example 1 is that the cooling rate of the quenching treatment is 8° C. / s, and an aluminum alloy plate is finally obtained.
[0062] Embodiment 11
[0063] The difference from Example 1 is that the cooling rate of the quenching treatment is 100° C. / s, and an aluminum alloy plate is finally obtained.
[0064] Example 12
[0065] The difference from Example 1 is that the cooling rate of the quenching treatment is 7° C. / s, and an aluminum alloy plate is finally obtained.
[0066] Example 13
[0067] The difference from Example 1 is that the temperature of the pre-aging treatment is 70° C., the holding time of the pre-aging treatment is 10 h, the deformation amount of the straightening treatment is 0.2%, and finally an aluminum alloy plate is obtained.
[0068] Embodiment 14
[0069] The difference from Example 1 is that the temperature of the pre-aging treatment is 120° C., the holding time of the pre-aging treatment is 4 h, the deformation amount of the straightening treatment is 0.5%, and finally an aluminum alloy plate is obtained.
[0070] Embodiment 15
[0071] The difference from Example 1 is that the temperature of the pre-aging treatment is 130° C., the holding time of the pre-aging treatment is 3 h, the deformation amount of the straightening treatment is 0.6%, and finally an aluminum alloy plate is obtained.
[0072] Example 16
[0073] The difference from Example 1 is that the aluminum alloy components, in mass percentage, are: Si: 1.50wt%, Fe: 0.50wt%, Cu: 1.0wt%, Mn: 0.45wt%, Mg: 1.20wt%, Cr: 0.10wt%, Zn: 0.15wt%, Ti: 0.10wt%, and finally an aluminum alloy sheet is obtained.
[0074] Embodiment 17
[0075] The difference from Example 1 is that the time interval between the completion of the solution treatment and the start of the quenching treatment is 4s, the time interval between the completion of the straightening treatment and the start of the pre-aging treatment is 4min, and the time interval between the completion of the quenching treatment and the start of the straightening treatment is 2min, and finally an aluminum alloy plate is obtained.
[0076] Comparative Example 1
[0077] The difference from Example 1 is that the temperature of the solution treatment is 535° C., the holding time is 4 s, and finally an aluminum alloy plate is obtained.
[0078] Comparative Example 2
[0079] The difference from Example 1 is that the temperature of the solution treatment is 580° C., the holding time is 65 s, and finally an aluminum alloy plate is obtained.
[0080] Comparative Example 3
[0081] The aluminum alloy sheet is prepared by the method in Example 1 disclosed in the Chinese patent application with patent application publication number CN108251712A. Specifically, a 6111 aluminum alloy ingot is prepared by semi-continuous casting; pretreatment and hot rolling: the 6111 aluminum alloy ingot is heated to 200°C and kept warm for 4 hours; then the temperature is raised to 460°C, kept warm for 3 hours, and then hot-rolled to obtain a hot-rolled plate with a thickness of 4 mm; intermediate annealing: the hot-rolled plate is heated to 480°C in a circulating cyclone furnace and kept warm for 6 hours, and then cooled to room temperature by air cooling to obtain an annealed rolled plate; Cold rolling: cold rolling the annealed plate to obtain a cold-rolled plate; the final rolling thickness of the cold-rolled plate is 0.9 mm; solution treatment: solution treatment is performed on the cold-rolled plate to obtain a solution-treated plate; wherein the heating temperature of the solution treatment is 550°C, the holding time is 12 minutes, and the cooling method is water quenching to room temperature; room temperature placement: after the solution treatment, the cold-rolled plate is placed at room temperature for 7 minutes; pre-aging treatment: pre-aging treatment is performed on the plate after being placed at room temperature to form a pre-aged rolled plate; wherein the pre-aging temperature is 170°C, and the pre-aging treatment time is 8 minutes.
[0082] Performance Testing
[0083] 1. Mechanical properties test:
[0084] The yield strength (Rp 0.2 ), tensile strength (R m ), elongation (A 50 ) test; after the aluminum alloy sheet was parked for 7 days, it was pre-stretched by 2%, and then the paint was simulated in an oil bath furnace at a paint temperature of 185°C for 20 minutes, and then the paint yield strength (Rp 0.2 / BH), paint tensile strength (R m / BH). All mechanical properties test samples were sampled along the vertical rolling direction, and the sample size adopted the A50 tensile sample recommended by GB / T228.
[0085] 2. Evaluation of plate type:
[0086] For the obtained aluminum alloy plate, take a sample with a length of 1000mm and a width of the whole width of the plate along the rolling direction for plate shape test. Measure the warping height of the plate end, the maximum horizontal or vertical unevenness of the plate surface outside the end, and record the number of waves per meter. According to the above measurement results, the plate shape grade is evaluated (the warping height of the end is ≤5mm, the maximum horizontal or vertical unevenness of the plate surface outside the end is ≤2.5mm, and the number of waves per meter is ≤3, which is defined as excellent; the warping height of the end is ≤10mm, the maximum horizontal or vertical unevenness of the plate surface outside the end is ≤5mm, and the number of waves per meter is ≤7, which is defined as good; the rest are unqualified).
[0087] 3. Evaluation of intergranular performance:
[0088] Take a sample of 50mm in length and 30mm in width along the rolling direction of the plate after baking varnish treatment, clean the sample with acetone or alcohol to remove oil stains, soak in 5% NaOH solution for 60±5s at 60±2℃, the sample needs to be suspended and cannot touch the bottom of the container, and rinse with tap water for 3~5min after soaking. Soak in 70% nitric acid at room temperature for 60±5s, the sample needs to be suspended and cannot touch the bottom of the container, and rinse with tap water for 3~5min after soaking, and clean the sample with acetone or alcohol again, air dry at room temperature, and there are no spots after the sample is cleaned. Add 30±0.1g sodium chloride and 10±0.1ml 37% hydrochloric acid to each liter of water, and mix them thoroughly to make a corrosion solution. The corrosion solution is placed in a constant temperature device at 30±0.2℃, and the sample is completely immersed in the solution. The sample is suspended in the solution and the soaking time is 24h±15min. Rinse with tap water immediately after taking out the sample, remove the surface reaction products under the flowing water, rinse with anhydrous alcohol and air dry. Use a stereo microscope to find 2 to 3 severely corroded areas on the surface and take photos and record them at a magnification of 10 to 20X. Make cross-sectional specimens in these areas with the observation direction perpendicular to the strain direction. Grind and polish the specimens according to the metallographic specimen preparation method without erosion. Use a metallographic microscope at a magnification of 100 to 500X to record the corrosion depth and calculate the average corrosion depth.
[0089] The yield strength (R p0.2 ), tensile strength (R m ), elongation (A 50 ), paint yield strength (R p0.2 / BH), paint tensile strength (R m / BH), plate type and average intergranular corrosion depth test, the test results are shown in Table 1
[0090] Table 1
[0091]
[0092]
[0093] It can be seen from Table 1 that the yield strength of the plate in the embodiment is maintained at 120-140 MPa after being parked for 7 days, and the elongation is ≥27%, which meets the plate punching requirements; after the plate is pre-stretched by 2% + 185℃×20min simulated baking paint, the yield strength is greater than 230 MPa, and can be used as a high-strength automotive exterior cover.
[0094] In Comparative Example 1, due to the too low solid solution temperature, the solid solubility of the solute atoms is too low. In the subsequent aging process, the amount of strengthening phase precipitation is insufficient, resulting in insufficient strength and failure to meet the performance requirements.
[0095] In Comparative Example 2, due to the high solid solution temperature, the solute atom has a high solid solubility, the size of the precipitated phase at the grain boundary is large, the uniformity of the microstructure deteriorates, and the corrosion potential difference increases, resulting in poor intergranular corrosion performance, the average intergranular corrosion depth is greater than 100 μm, and the intergranular corrosion performance of the plate is unqualified;
[0096] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:
[0097] Homogenizing the aluminum alloy ingot helps to improve the uniformity of element distribution in the aluminum alloy sheet, thereby helping to improve the ductility and strength of the aluminum alloy sheet; hot rolling treatment helps to promote the diffusion of alloy elements and make the alloy structure more uniform, thereby helping to improve the plasticity and toughness of the aluminum alloy sheet; the first cold rolling treatment helps to refine the grains, thereby helping to improve the strength and hardness of the aluminum alloy sheet; the intermediate annealing treatment helps to promote the rearrangement of the microstructure inside the alloy and reduce the dislocation density, thereby reducing the hardening effect; the second cold rolling treatment helps to further refine the grains, thereby helping to further improve the tensile strength and toughness of the aluminum alloy sheet; the solid solution treatment helps to dissolve the solute elements in the alloy more evenly in the aluminum matrix. If the temperature of the solution treatment is too low and the time is too short, it is not conducive to the full solution of the aluminum alloy, and thus it is not conducive to improving the strength of the aluminum alloy plate; if the temperature of the solution treatment is too high and the time is too long, the solubility of the solute atoms is too high, and the size of the grain boundary precipitation phase is large, which is not conducive to improving the uniformity of the microstructure, and thus it is not conducive to reducing the corrosion potential difference, and thus it is not conducive to improving the intergranular corrosion resistance. The average intergranular corrosion depth is too high, and the intergranular corrosion performance of the plate is unqualified. The present application controls the temperature and holding time of the solution treatment within the above range, which helps to fully dissolve the alloy solute atoms and accurately control the solubility of the solute atoms, thereby helping to control the size of the grain boundary precipitation phase, improve the uniformity of the microstructure, thereby helping to improve the tensile strength of the aluminum alloy plate, reduce the yield strength of the aluminum alloy plate, and reduce the corrosion potential difference of the aluminum alloy plate, thereby helping to improve the stamping forming performance and intergranular corrosion resistance of the aluminum alloy plate. Therefore, the preparation method of the present application can help improve the mechanical properties such as paint strength and intergranular corrosion resistance of the aluminum alloy plate on the one hand, and help improve the production efficiency and yield of the aluminum alloy plate on the other hand, thereby helping to save the production cost of the aluminum alloy plate.
[0098] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an aluminum alloy sheet, characterized in that: The preparation method comprises: The aluminum alloy ingot is sequentially subjected to homogenization treatment, hot rolling treatment, first cold rolling treatment, intermediate annealing treatment, second cold rolling treatment, solution treatment, quenching treatment, straightening treatment and pre-aging treatment to obtain the aluminum alloy sheet; wherein, The temperature of the solution treatment is 540° C. to 570° C., and the holding time of the solution treatment is 5 to 60 seconds.
2. The preparation method according to claim 1, characterized in that: The temperature of the solution treatment is 540°C to 560°C; and / or the holding time of the solution treatment is 5 to 30s; and / or the heating rate of the solution treatment is 10 to 100°C / s, preferably 15 to 60°C / s.
3. The preparation method according to claim 1 or 2, characterized in that: The time interval between the completion of the solution treatment and the start of the quenching treatment is no more than 3s; and / or the cooling rate of the quenching treatment is 8-100°C / s, preferably 27-60°C / s; and / or the temperature of the material after the quenching treatment is 10-35°C.
4. The preparation method according to any one of claims 1 to 3, characterized in that The time interval between the completion of the straightening treatment and the start of the pre-aging treatment is no more than 3 minutes; and / or, the temperature of the pre-aging treatment is 70-120° C.; and / or, the holding time of the pre-aging treatment is 4-10 hours.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The time interval between the completion of the quenching treatment and the start of the straightening treatment is no more than 1 minute; and / or, the deformation amount of the straightening treatment is 0.2% to 0.5%; and / or, the thickness of the material after the second cold rolling treatment is 0.7mm to 3mm.
6. The preparation method according to any one of claims 1 to 5, characterized in that The temperature of the homogenization treatment is 560°C; and / or, the holding time of the homogenization treatment is 8h; and / or, after the homogenization treatment is completed, the temperature is lowered to 510°C and then the hot rolling treatment is started; and / or, the temperature at the end of the hot rolling treatment is 270°C; and / or, the thickness of the material at the end of the hot rolling treatment is 6mm; and / or, the thickness of the material after the first cold rolling treatment is 1.4mm; And / or, the reduction ratio of the first cold rolling treatment is 77%; and / or, the temperature of the intermediate annealing treatment is 475°C; and / or, the holding time of the intermediate annealing treatment is 30s; and / or, the reduction ratio of the second cold rolling treatment is 29%.
7. The preparation method according to any one of claims 1 to 6, characterized in that The aluminum alloy ingot comprises the following elements in percentage by mass: Si element content is 0.50-1.50wt%, Fe element content is ≤0.50wt%, Cu element content is 0.50-1.0wt%, Mn element content is 0.10-0.45wt%, Mg element content is 0.25-1.20wt%, Cr element content is ≤0.10wt%, Zn element content is ≤0.15wt%, Ti element content is ≤0.10wt%, the total content of unavoidable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
8. The preparation method according to claim 7, characterized in that: The aluminum alloy ingot comprises the following elements: Si element content is 0.72-1.50wt%, Fe element content is 0.18-0.50wt%, Cu element content is 0.75-1.0wt%, Mn element content is 0.18-0.45wt%, Mg element content is 0.80-1.20wt%, Cr element content is 0.015-0.10wt%, Zn element content is 0.015-0.15wt%, Ti element content is 0.02-0.10wt%, the total content of inevitable impurities is ≤0.15wt%, the content of a single impurity does not exceed 0.05wt%, and the balance is Al element.
9. An aluminum alloy plate, characterized in that: The aluminum alloy sheet is prepared by the preparation method described in any one of claims 1 to 8.
10. The aluminum alloy sheet according to claim 9, characterized in that: The yield strength of the aluminum alloy plate after being placed at 25°C for 7 days is 120-140 MPa; and / or the tensile strength of the aluminum alloy plate after being placed at 25°C for 7 days is not less than 270 MPa; and / or the elongation of the aluminum alloy plate after being placed at 25°C for 7 days is not less than 27%; And / or, the aluminum alloy plate after being placed at 25°C for 7 days is subjected to a 2% pre-stretching treatment and a baking treatment at 185°C for 20 minutes in sequence to obtain a treated aluminum alloy plate, wherein the yield strength of the treated aluminum alloy plate is not less than 230MPa; the tensile strength of the treated aluminum alloy plate is not less than 315MPa; and the average intergranular corrosion depth of the treated aluminum alloy plate does not exceed 100μm.
Citation Information
Cited By
6451 aluminum alloy plate based on dynamic diffusion field regulation and control
CN120796787A
Aluminum alloy plate based on dynamic diffusion field regulation
CN120796787B
Aluminum alloy plate and preparation method thereof
CN121087308A
Aluminum alloy sheet and method for manufacturing the same
CN121087308B
Al-Mg-Si aluminum alloy plate and preparation method thereof
CN121204476A