Preparation method and application of PBA-coated NiCo-LDH-CQDs composite material
Through the preparation of PBA@NiCo-LDH-CQDs composite material, the combination of in-situ growth MOF and carbon quantum dots has been used to solve the problem of poor conductivity of existing electrode materials, and high specific capacitance and good cycle stability are achieved. It is suitable for supercapacitors Positive electrode material.
Patent Information
- Application Number
- CN202411157004.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing supercapacitor electrode materials have low energy density and poor conductivity, which limits their application in the energy storage field, especially the electronic conductivity and ions of Prussian blue analogs and layered double hydroxide materials during charging and discharging. Inadequate diffusion performance.
Using the preparation method of PBA@NiCo-LDH-CQDs composite material, by growing MOFs in situ and combining them with carbon quantum dots, electron-rich regions are built, the conductivity and cyclic properties of the material are improved, the self-aggregation effect of LDH nanoparticles is reduced, and the self-aggregation effect of LDH nanoparticles is shortened. The transmission pathways of ions and electrons.
It achieves high specific capacitance, good rate performance and cycle stability, and is suitable for supercapacitor positive electrode materials, improving the electrochemical performance of the material.
Smart Images

Figure CN118942924A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of supercapacitor electrode positive electrode materials, and specifically relates to a preparation method and application of a PBA@NiCo-LDH-CQDs composite material. Background Art
[0002] Supercapacitors are a new type of energy storage element between ordinary capacitors and secondary batteries. They have become a rapidly rising star under the new energy policy due to their advantages such as high power density, fast charging speed, and long service life. However, the low energy density greatly limits the large-scale use of supercapacitors, and the electrode material plays a decisive role in the performance of supercapacitors. Designing and manufacturing electrode materials with special structures can improve the energy density of supercapacitors while maintaining other properties, thereby preparing supercapacitors with higher performance, which will have great strategic significance in the field of energy storage.
[0003] Prussian blue analogs (PBA) are a class of compounds with a similar crystal structure to Prussian blue (PB). They belong to the category of metal organic framework compounds, which are three-dimensional network structures formed by iron ions and ligands (usually cyanide) connected by coordination bonds. The material has a cubic microscopic morphology and good stability, but has the disadvantage of poor conductivity. Therefore, it is rarely used directly as an electrode material for supercapacitors in the research process. Instead, it is used as a template or metal source to derive the corresponding metal compounds to obtain electrode materials with high specific capacitance and long-term stability.
[0004] Layered double hydroxide (LDH) is considered to be a potential electrode material. As a pseudocapacitive electrode material, FeCoNo-LDH has the advantages of low resource cost, relatively high theoretical capacity and high specific surface area, but poor electronic conductivity and slow ion diffusion limit its application in supercapacitors.
[0005] Carbon quantum dots (CQDs) are a type of zero-dimensional carbon material with a size below 10 nm. As a highly promising candidate material, they have attracted increasing attention in the field of energy storage. As a size regulator and conductive agent, CQDs can not only increase the specific surface area by regulating the size of the material, provide more active sites for redox reactions and thus improve charge storage performance, but also effectively improve the kinetic performance and cycle stability of the material by improving its conductivity. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a PBA@NiCo-LDH-CQDs composite material and its application in view of the deficiencies of the above-mentioned prior art. The PBA@NiCo-LDH-CQDs composite material prepared by the method has excellent electrochemical performance, and the structure retains the unique morphology of the core PBA material. By in-situ growing MOF, assembling LDH nanoparticles after composite CQDs, the prepared electrode material has high specific capacitance, good rate performance, and stable cycle performance, which has practical guiding significance for the preparation of positive electrode materials for supercapacitors.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a PBA@NiCo-LDH-CQDs composite material, the method comprising:
[0008] S1. Anhydrous citric acid and deionized water were mixed and magnetically stirred to obtain solution A, and then a hydrothermal reaction was performed. After the reaction was completed, the solution was naturally cooled to room temperature, filtered and dialyzed for 8h to 12h, and freeze-dried at a temperature of -30°C for 24h to obtain a carbon quantum dot material;
[0009] S2, nickel nitrate, cobalt nitrate, sodium citrate and deionized water are mixed, ultrasonicated and magnetically stirred to obtain solution B, potassium ferrocyanide is dispersed in deionized water, ultrasonicated and magnetically stirred until uniform, to obtain solution C, the solution C is transferred to the solution B, magnetically stirred to obtain solution D;
[0010] S3, aging the solution D obtained in S2, separating the solid matter by centrifugation after aging, washing and drying to obtain a gray powder, named PBA;
[0011] S4, dispersing the PBA obtained in S3 in deionized water, and stirring magnetically until uniform, to obtain solution E;
[0012] Then, nickel nitrate, cobalt nitrate and the carbon quantum dots obtained in S1 are dissolved in ethanol and magnetically stirred until uniform, to obtain solution F;
[0013] Transferring the solution F to the solution E, and stirring by magnetic force until uniform, to obtain a solution G;
[0014] Then, sodium dodecyl sulfate and trimesic acid are dissolved in N,N-dimethylformamide and stirred magnetically until uniform to obtain solution H;
[0015] The solution H is transferred into the solution G, and after magnetic stirring, a solution I is obtained;
[0016] S5, subjecting the solution I obtained in S4 to a hydrothermal reaction, cooling the solution to room temperature naturally after the reaction is completed, centrifuging, washing and drying the solid matter, and obtaining PBA@NiCo-MOF-CQDs;
[0017] S6, dispersing the PBA@NiCo-MOF-CQDs obtained in S5 in deionized water, and stirring evenly with a magnetic stirrer to obtain a solution J;
[0018] Dissolve sodium carbonate and sodium hydroxide in deionized water and stir evenly with a magnetic stirrer to obtain solution K;
[0019] Then, the solution K is transferred into the solution J and stirred evenly by magnetic force to obtain a solution L;
[0020] S7. After centrifuging the solution L obtained in S6, the solid matter is washed and dried to obtain a PBA@NiCo-LDH-CQDs composite material.
[0021] Preferably, the dosage ratio of citric acid to deionized water in S1 is 500 mg:50 mL; the hydrothermal reaction temperature is 160° C. to 200° C., and the reaction time is 4 h to 8 h.
[0022] Preferably, the usage ratio of nickel nitrate, cobalt nitrate, sodium citrate and potassium ferrocyanide in S2 is 145.5 mg: 436.5 mg: 650.0 mg: 483.9 mg; and the ultrasonic time is 20 min to 40 min.
[0023] Preferably, the aging time in S3 is 24h to 36h, the centrifugal speed is 5000r / min to 8000r / min, and the centrifugal time is 2min to 5min; the washing method is: washing with deionized water for 3 to 4 times, and then washing with anhydrous ethanol for 3 to 4 times; the drying temperature is 60℃ to 70℃, and the drying time is 12h to 24h.
[0024] Preferably, the usage ratio of PBA, nickel nitrate, cobalt nitrate, carbon quantum dots, sodium dodecyl sulfate and trimesic acid in S4 is 100 mg: 872.4 mg: 225.1 mg: 5 mg: (3-10) mg: 632.4 mg.
[0025] Preferably, the hydrothermal reaction temperature in S5 is 100°C to 160°C, and the hydrothermal reaction time is 8h to 16h; the centrifugal speed is 5000r / min to 8000r / min, and the centrifugal time is 2min to 5min; the washing method is: first washing with deionized water for 3 to 4 times, and then washing with methanol for 3 to 4 times; the drying temperature is 60°C to 70°C, and the drying time is 12h to 24h.
[0026] Preferably, the mass ratio of PBA@NiCo-MOF-CQDs, sodium carbonate and sodium hydroxide in S6 is 100 mg:530 mg:2000 mg.
[0027] Preferably, the centrifugal speed in S7 is 5000r / min~8000r / min, and the centrifugal time is 2min~5min; the washing method is: washing with deionized water for 3~4 times, and then washing with anhydrous ethanol for 3~4 times; the drying temperature is 60℃~70℃, and the drying time is 12h~24h.
[0028] The present invention also provides an application of the PBA@NiCo-LDH-CQDs composite material prepared by the above method, and the PBA@NiCo-LDH-CQDs composite material is applied in a supercapacitor positive electrode.
[0029] Preferably, when the PBA@NiCo-LDH-CQDs composite material is used in the positive electrode of a supercapacitor, the -1 The specific capacitance is 1309.2F·g at a current density of -1 ~1331.2F·g -1 , and at 10A·g -1 The capacitance retention rate is 86.0% to 86.5% when the cycle is repeated, and the capacitance retention rate is 82.5% to 83.8% after 5000 cycles.
[0030] The present invention uses PBA as a template to derive MOF and then convert it into LDH to reduce the stacking of LDH sheets during the charge and discharge process, and composites it with CQDs materials with good conductivity, thereby effectively improving the conductivity and cycle performance of the material.
[0031] Compared with the prior art, the present invention has the following advantages:
[0032] The present invention uses PBA as a precursor, modifies the surface of PBA by using a surfactant, sodium dodecyl sulfate, anchors nickel and cobalt ions on the surface of PBA without damaging the inner core cubic PBA, and then combines with organic ligands to grow NiCo-MOF in situ on the surface of PBA. 2 The hybrid zero-dimensional carbon material and carbon quantum dots are combined to construct electron-rich regions to change part of the electronic environment, thereby improving the electronic conductivity of the electrode. Through a mild alkalization method, the outermost layer is precisely processed into a layered double hydroxide, thereby achieving controllable preparation of PBA@NiCo-LDH-CQDs composite materials.
[0033] At the same time, the LDH nanoparticles are assembled, which not only reduces the self-aggregation effect of LDH nanoparticles, increases more exposed electroactive sites, but also shortens the transmission pathways of ions and electrons. Its special hierarchical core-shell structure is not easy to collapse or agglomerate during the charge and discharge cycle, and is more stable. In addition, the carbon quantum dot material, which is very novel in the field of supercapacitors, is introduced to construct electron-rich regions to change part of the electronic environment, thereby improving the electronic conductivity of the electrode. Therefore, the prepared PBA@NiCo-LDH-CQDs has excellent electrochemical properties such as high specific capacitance, good rate performance and cycle stability, and can be widely used in supercapacitor positive electrode materials.
[0034] The present invention is further described in detail below with reference to the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the XRD pattern of PBA@NiCo-LDH-CQDs prepared in Example 1 of the present invention and the corresponding standard card.
[0036] Figure 2 This is the SEM image of PBA@NiCo-LDH-CQDs prepared in Example 1 of the present invention.
[0037] Figure 3 Cyclic voltammograms of PBA@NiCo-LDH-CQDs prepared in Example 1 of the present invention at different scan rates.
[0038] Figure 4 This is the constant current charge and discharge diagram of PBA@NiCo-LDH-CQDs prepared in Example 1 of the present invention at different current densities.
[0039] Figure 5 This is the cycle performance diagram of PBA@NiCo-LDH-CQDs prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0040] Example 1
[0041] The preparation method of the PBA@NiCo-LDH-CQDs composite material of this embodiment is characterized in that the method comprises:
[0042] S1. Mix 500 mg of anhydrous citric acid with 50 mL of deionized water, stir magnetically to obtain solution A, transfer to a 100 mL polytetrafluoroethylene-lined autoclave, and then perform hydrothermal reaction at 200 ° C for 4 h. After the reaction is completed, naturally cool to room temperature, filter and dialyze for 12 h, and freeze-dry at -30 ° C for 24 h to obtain carbon quantum dot material (CQDs);
[0043] S2, 145.5 mg nickel nitrate, 436.5 mg cobalt nitrate, 650.0 mg sodium citrate and 50 mL deionized water were mixed, ultrasonicated for 20 min and magnetically stirred at a speed of 400 r / min for 30 min to obtain solution B, 483.9 mg potassium ferrocyanide was dispersed in 50 mL deionized water, ultrasonicated and magnetically stirred until uniform, to obtain solution C, the solution C was transferred to the solution B, and magnetically stirred at a speed of 400 r / min for 30 min to obtain solution D;
[0044] S3, aging the solution D obtained in S2 for 24 hours, and after aging, centrifuging at a speed of 8000r / min for 2 minutes to separate the solid matter, and then washing it with deionized water for 3 to 4 times, and then washing it with anhydrous ethanol for 3 times, and finally drying it in a vacuum oven at a temperature of 60°C for 24 hours to obtain a gray powder, named PBA;
[0045] S4, dispersing 100 mg of the PBA obtained in S3 in 20 mL of deionized water, and stirring magnetically at a speed of 500 r / min for 20 min until the mixture is uniform, to obtain a solution E;
[0046] Then, 872.4 mg of nickel nitrate, 225.1 mg of cobalt nitrate and 5 mg of the carbon quantum dots obtained in S1 were dissolved in 20 mL of ethanol and magnetically stirred until uniform to obtain solution F;
[0047] The solution F was transferred into the solution E, and magnetically stirred at a rotation speed of 500 r / min for 20 min until the mixture was uniform, to obtain a solution G;
[0048] Then, 10 mg of sodium dodecyl sulfate and 632.4 mg of trimesic acid were dissolved in 20 mL of N,N-dimethylformamide, and magnetically stirred at a speed of 500 r / min for 20 min until the mixture was homogeneous, to obtain solution H;
[0049] The solution H was transferred into the solution G, and magnetically stirred at a rotation speed of 500 r / min for 20 min until the mixture was uniform, to obtain a solution I;
[0050] S5. The solution I obtained in S4 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and a hydrothermal reaction was carried out at a temperature of 100° C. for 16 h. After the reaction was completed, the solution was naturally cooled to room temperature, and the solution was centrifuged at a speed of 8000 r / min for 2 min. The solid matter was washed, first with deionized water for 3 times, then with methanol for 3 times, and finally dried at a temperature of 60° C. to 70° C. for 24 h to obtain PBA@NiCo-MOF-CQDs.
[0051] S6, 100 mg of PBA@NiCo-MOF-CQDs obtained in S5 was dispersed in 40 mL of deionized water, and magnetically stirred at a speed of 600 r / min for 30 min until uniform, to obtain solution J;
[0052] 530 mg of sodium carbonate and 2000 mg of sodium hydroxide were dissolved in 50 mL of deionized water, and magnetically stirred at a speed of 500 r / min for 30 min until the mixture was uniform, to obtain solution K;
[0053] Then, the solution K was transferred into the solution J, and magnetically stirred for 240 min at a rotation speed of 800 r / min until the solution was uniform, to obtain a solution L;
[0054] S7. After the solution L obtained in S6 was centrifuged at a speed of 8000 r / min for 2 min, the solid matter was washed, first with deionized water for 3 times, then with anhydrous ethanol for 3 times, and finally dried at a temperature of 60°C for 24 h to obtain a dark green powder, which is the PBA@NiCo-LDH-CQDs composite material.
[0055] This embodiment also provides an application of the PBA@NiCo-LDH-CQDs composite material prepared by the above method, wherein the PBA@NiCo-LDH-CQDs composite material is applied in a positive electrode of a supercapacitor.
[0056] Figure 1 : This is the XRD pattern of PBA@NiCo-LDH-CQDs prepared in this embodiment and the corresponding standard card. As shown in the figure, the diffraction peak of PBA@NiCo-LDH-CQDs at 2θ=21.2° can be attributed to the diffraction peak of the (002) crystal plane, which is the characteristic diffraction peak of the carbon quantum dot material; the diffraction peaks at 2θ=23.4°, 34.5°, 60.0°, 61.3°, etc. can be attributed to (0012), (204), (1 The characteristic diffraction peaks of the (110), (113), (202) and other crystal planes are all attributable to the characteristic diffraction peaks of the (202), (110), (202 ...)
[0057] Figure 2 This is a scanning electron microscope image of PBA@NiCo-LDH-CQDs prepared in this example. From the scanning electron microscope image, it can be seen that the material retains the cubic morphology while assembling LDH nanoparticles to form a unique core-shell structure, thereby improving the electrochemical performance of the material.
[0058] Figure 3 The cyclic voltammetry curves (CV curves) of PBA@NiCo-LDH-CQDs prepared in this embodiment at different scan rates. It can be seen from the CV curve that there are obvious redox peaks, which can prove that the material is a typical pseudocapacitive material. In addition, as the scan rate increases, the peak current of the redox peak increases significantly, indicating that the redox rate on the electrode is accelerated; at the same time, the overall shape of the curve does not change much, and the corresponding redox peak remains well, indicating that the polarization phenomenon of the electrode is not obvious.
[0059] Figure 4 The constant current charge and discharge diagram of PBA@NiCo-LDH-CQDs prepared in this example at different current densities. -1 The specific capacitances at different current densities are 1331.2, 1299.2, 1276.8, 1232, and 1152 F·g -1 , indicating that the material has a high specific capacitance. And the current density is 10A·g -1 The specific capacitance can still maintain 1A·g -1 The 86.5% initial specific capacitance at the current density also indicates that the material has excellent rate performance.
[0060] Figure 5 This is the cycle performance diagram of PBA@NiCo-LDH-CQDs prepared in this example. After 5000 cycles, the specific capacitance of PBA@NiCo-LDH-CQDs can still maintain 83.8% of the initial value, indicating that the material has good cycle stability.
[0061] The PBA@NiCo-LDH-CQDs structure prepared in this embodiment retains the unique morphology of the core PBA material. By in-situ growing MOF, assembling LDH nanoparticles after composite CQDs, the prepared electrode material has high specific capacitance, good rate performance, and stable cycle performance, which has practical guiding significance for the preparation of positive electrode materials for supercapacitors.
[0062] Example 2
[0063] The preparation method of the PBA@NiCo-LDH-CQDs composite material of this embodiment is characterized in that the method comprises:
[0064] S1. Mix 500 mg of anhydrous citric acid with 50 mL of deionized water, stir magnetically to obtain solution A, transfer to a 100 mL polytetrafluoroethylene-lined autoclave, and then perform a hydrothermal reaction at 160 ° C for 8 h. After the reaction is completed, naturally cool to room temperature, filter and dialyze for 8 h, and freeze-dry at -30 ° C for 24 h to obtain a carbon quantum dot material;
[0065] S2, 145.5 mg nickel nitrate, 436.5 mg cobalt nitrate, 650.0 mg sodium citrate and 50 mL deionized water were mixed, ultrasonicated for 40 min and magnetically stirred at a speed of 400 r / min for 30 min to obtain solution B, 483.9 mg potassium ferrocyanide was dispersed in 50 mL deionized water, ultrasonicated and magnetically stirred until uniform, to obtain solution C, the solution C was transferred to the solution B, and magnetically stirred at a speed of 400 r / min for 30 min to obtain solution D;
[0066] S3, aging the solution D obtained in S2 for 36 hours. After aging, centrifuging at a speed of 5000 r / min for 5 minutes to separate the solid matter, then washing it with deionized water for 4 times, and then washing it with anhydrous ethanol for 4 times, and finally drying it in a vacuum oven at a temperature of 70°C for 12 hours to obtain a gray powder, named PBA;
[0067] S4, dispersing 100 mg of the PBA obtained in S3 in 20 mL of deionized water, and stirring magnetically at a speed of 500 r / min for 20 min until the mixture is uniform, to obtain a solution E;
[0068] Then, 872.4 mg of nickel nitrate, 225.1 mg of cobalt nitrate and 5 mg of the carbon quantum dots obtained in S1 were dissolved in 20 mL of ethanol and magnetically stirred until uniform to obtain solution F;
[0069] The solution F was transferred into the solution E, and magnetically stirred at a rotation speed of 500 r / min for 20 min until the mixture was uniform, to obtain a solution G;
[0070] Then, 3 mg of sodium dodecyl sulfate and 632.4 mg of trimesic acid were dissolved in 20 mL of N,N-dimethylformamide, and magnetically stirred at a speed of 500 r / min for 20 min until the mixture was homogeneous, to obtain solution H;
[0071] The solution H was transferred into the solution G, and magnetically stirred at a rotation speed of 500 r / min for 20 min until the mixture was uniform, to obtain a solution I;
[0072] S5, the solution I obtained in S4 was transferred to a 100 mL polytetrafluoroethylene-lined autoclave, and a hydrothermal reaction was carried out at a temperature of 160° C. for 8 h. After the reaction was completed, it was naturally cooled to room temperature, and centrifuged at a speed of 5000 r / min for 5 min. The solid matter was washed, first with deionized water for 4 times, then with methanol for 4 times, and finally dried at a temperature of 70° C. for 12 h to obtain PBA@NiCo-MOF-CQDs;
[0073] S6, 100 mg of PBA@NiCo-MOF-CQDs obtained in S5 was dispersed in 40 mL of deionized water, and magnetically stirred at a speed of 600 r / min for 30 min until uniform, to obtain solution J;
[0074] 530 mg of sodium carbonate and 2000 mg of sodium hydroxide were dissolved in 50 mL of deionized water, and magnetically stirred at a speed of 500 r / min for 30 min until the mixture was uniform, to obtain solution K;
[0075] Then, the solution K was transferred into the solution J, and magnetically stirred for 240 min at a rotation speed of 800 r / min until the solution was uniform, to obtain a solution L;
[0076] S7. After centrifuging the solution L obtained in S6 at a rotation speed of 5000 r / min for 5 minutes, the solid matter was washed, first with deionized water for 4 times, then with anhydrous ethanol for 4 times, and finally dried at a temperature of 70°C for 12 hours to obtain a dark green powder, which is the PBA@NiCo-LDH-CQDs composite material.
[0077] This embodiment also provides an application of the PBA@NiCo-LDH-CQDs composite material prepared by the above method, wherein the PBA@NiCo-LDH-CQDs composite material is applied in a positive electrode of a supercapacitor.
[0078] PBA@NiCo-LDH-CQDs composites at 1A·g -1 The best performance is 1309.2F·g -1 Excellent specific capacitance, and at 10A·g -1 The capacitance retention rate is 86.0%, showing excellent rate performance, and the capacitance retention rate is still 82.5% after 5000 cycles. The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the essence of the invention technology still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a PBA@NiCo-LDH-CQDs composite material, It is characterized in that The method is: S1. Anhydrous citric acid and deionized water were mixed and magnetically stirred to obtain solution A, and then a hydrothermal reaction was performed. After the reaction was completed, the solution was naturally cooled to room temperature, filtered and dialyzed for 8h to 12h, and freeze-dried at a temperature of -30°C for 24h to obtain a carbon quantum dot material; S2, nickel nitrate, cobalt nitrate, sodium citrate and deionized water are mixed, ultrasonicated and magnetically stirred to obtain solution B, potassium ferrocyanide is dispersed in deionized water, ultrasonicated and magnetically stirred until uniform, to obtain solution C, the solution C is transferred to the solution B, magnetically stirred to obtain solution D; S3, aging the solution D obtained in S2, separating the solid matter by centrifugation after aging, washing and drying to obtain a gray powder, named PBA; S4, dispersing the PBA obtained in S3 in deionized water, and stirring magnetically until uniform, to obtain solution E; Then, nickel nitrate, cobalt nitrate and the carbon quantum dots obtained in S1 are dissolved in ethanol and magnetically stirred until uniform, to obtain solution F; Transferring the solution F to the solution E, and stirring by magnetic force until uniform, to obtain a solution G; Then, sodium dodecyl sulfate and trimesic acid are dissolved in N,N-dimethylformamide and stirred magnetically until uniform to obtain solution H; The solution H is transferred into the solution G, and after magnetic stirring, a solution I is obtained; S5, subjecting the solution I obtained in S4 to a hydrothermal reaction, cooling the solution to room temperature naturally after the reaction is completed, centrifuging, washing and drying the solid matter, and obtaining PBA@NiCo-MOF-CQDs; S6, dispersing the PBA@NiCo-MOF-CQDs obtained in S5 in deionized water, and stirring evenly with a magnetic stirrer to obtain a solution J; Dissolve sodium carbonate and sodium hydroxide in deionized water and stir evenly with a magnetic stirrer to obtain solution K; Then, the solution K is transferred into the solution J and stirred evenly by magnetic force to obtain a solution L; S7. After centrifuging the solution L obtained in S6, the solid matter is washed and dried to obtain a PBA@NiCo-LDH-CQDs composite material.
2. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The dosage ratio of citric acid and deionized water in S1 is 500 mg:50 mL; the hydrothermal reaction temperature is 160° C. to 200° C., and the reaction time is 4 h to 8 h.
3. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The usage ratio of nickel nitrate, cobalt nitrate, sodium citrate and potassium ferrocyanide in S2 is 145.5 mg: 436.5 mg: 650.0 mg: 483.9 mg; and the ultrasonic time is 20 min to 40 min.
4. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The aging time in S3 is 24h~36h, the centrifugal speed is 5000r / min~8000r / min, and the centrifugal time is 2min~5min; the washing method is: washing with deionized water for 3~4 times, and then washing with anhydrous ethanol for 3~4 times; the drying temperature is 60℃~70℃, and the drying time is 12h~24h.
5. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The usage ratio of PBA, nickel nitrate, cobalt nitrate, carbon quantum dots, sodium dodecyl sulfate and trimesic acid described in S4 is 100 mg: 872.4 mg: 225.1 mg: 5 mg: (3-10) mg: 632.4 mg.
6. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The hydrothermal reaction temperature in S5 is 100°C to 160°C, and the hydrothermal reaction time is 8h to 16h; the centrifugal speed is 5000r / min to 8000r / min, and the centrifugal time is 2min to 5min; the washing method is: first washing with deionized water for 3 to 4 times, and then washing with methanol for 3 to 4 times; the drying temperature is 60°C to 70°C, and the drying time is 12h to 24h.
7. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The mass ratio of PBA@NiCo-MOF-CQDs, sodium carbonate and sodium hydroxide described in S6 is 100 mg:530 mg:2000 mg.
8. A method for preparing a PBA@NiCo-LDH-CQDs composite material according to claim 1, It is characterized in that The centrifugal speed in S7 is 5000r / min~8000r / min, and the centrifugal time is 2min~5min; the washing method is: washing with deionized water for 3~4 times, and then washing with anhydrous ethanol for 3~4 times; the drying temperature is 60℃~70℃, and the drying time is 12h~24h.
9. An application of a PBA@NiCo-LDH-CQDs composite material prepared by the method according to any one of claims 1 to 8, It is characterized in that The PBA@NiCo-LDH-CQDs composite material is used in the positive electrode of a supercapacitor.
10. The use according to claim 9, It is characterized in that When the PBA@NiCo-LDH-CQDs composite material is used as the positive electrode of supercapacitor, the -1 The specific capacitance is 1309.2F·g at a current density of -1 ~1331.2F·g -1 , and at 10A·g -1 The capacitance retention rate is 86.0% to 86.5% when the cycle is repeated, and the capacitance retention rate is 82.5% to 83.8% after 5000 cycles.
Citation Information
Cited By
NiCoPBA (at) rGO electrode material and preparation method and application thereof
CN119964998A
Quantum dot doped NiCo-LDH composite material and preparation method and application thereof
CN121662620A
Ferronickel Prussian blue supercapacitor electrode material, preparation method thereof and supercapacitor
CN121905728A