Cobalt phthalocyanine catalytic electrode and preparation method and application thereof
Through the combination of cobalt phthalocyanine catalytic electrode and acetylene black, the problem of poor reversibility of the positive electrode of lithium/thionyl chloride batteries is solved, the cycle life and reversible capacity of the battery is improved, the storage risk of chlorine is reduced, and more efficient battery cycles are achieved Stability and safety.
Patent Information
- Application Number
- CN202410987817.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
The existing lithium/thionyl chloride batteries have poor positive electrode reversibility, resulting in short cycle life and low reversible capacity. The shuttle effect of chlorine increases the explosion hazards of the battery and electrode corrosion, limiting the cyclic application of the battery.
The catalytic electrode of phthalocyanine is prepared by solid-phase sintering method to combine with acetylene black, and is loaded on nickel foam. The positive electrode of rechargeable Li/SOCl2 battery is prepared by rolling method to promote the conversion of Cl2 to SOCl2 and reduce the Internal resistance and improve cycle stability.
Improves the cycle life and reversible capacity of lithium/thionyl chloride batteries, reduces the storage risk of chlorine, improves the charging and discharging performance and safety of the battery, and increases the average Coulomb efficiency by about 15%, under the cycling capacity of 800mAhg-1 It can cycle stably for 100 times.
Smart Images

Figure CN118943299A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rechargeable lithium / thionyl chloride batteries, and in particular is a cobalt phthalocyanine catalytic electrode and a preparation method and application thereof. Background Art
[0002] In recent years, with the emergence of various new electronic products, the demand for rechargeable batteries has increased. Lithium / thionyl chloride battery (Li / SOCl2) is one of the batteries with the highest specific energy, with a specific energy of up to 590Wh kg -1 , and the open circuit voltage reaches about 3.6V, with a storage life of 5 to 10 years. However, the original lithium / thionyl chloride battery has poor reversibility and is non-rechargeable, resulting in extremely high cost of use. Therefore, the research on rechargeable lithium / thionyl chloride batteries has received widespread attention.
[0003] In existing rechargeable lithium / thionyl chloride batteries based on thionyl chloride (SOCl2) electrolyte, the positive electrode usually adopts a porous carbon electrode. The oxidation of lithium chloride on the surface of the first discharge provides the reversibility of the positive electrode. Porous carbon stores chlorine (Cl2) generated during charging for cyclic discharge (Zhu G, et al. Nature. 2021, 596 (7873), 525-530). Chlorine is in gaseous state at room temperature, which increases the explosion risk of increased voltage inside the battery, and has low safety performance. In addition, the shuttle effect of chlorine corrodes the anode and reduces the battery capacity. In addition, due to the adsorption of Cl2 by porous carbon, the conversion of Cl2 to SOCl2 is severely reduced (Cl2+S→SCl2, Cl2+SO2→SO2Cl2, SCl2+SO2Cl2→SOCl2) (Chen G, et al. J. Am. Chem. Soc. 2023, 145 (40), 22158-22167), which makes the rechargeable lithium / thionyl chloride battery reversible and limits the cyclic application of the battery. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a cobalt phthalocyanine catalytic electrode and a preparation method and application thereof, so as to improve the cycle life and reversible capacity of a rechargeable Li / SOCl2 battery.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A method for preparing a cobalt phthalocyanine catalytic electrode comprises the following steps:
[0007] Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of (0.58-0.86):(1.12-1.73):(0.51-0.78):(0.11-0.36) to obtain a mixture A;
[0008] Step 2, placing mixture A into a muffle furnace, heating from room temperature to 140-160° C. at a heating rate of 10-20° C. / min in an air atmosphere and keeping the temperature for 0.5-2 h, then heating to 270-290° C. at a heating rate of 5-10° C. / min, keeping the temperature for 2-3 h, cooling naturally to room temperature, grinding, soaking, washing and drying in sequence to obtain a phthalocyanine cobalt catalyst material powder;
[0009] Step 3, mixing acetylene black and cobalt phthalocyanine catalyst material powders in a mass ratio of (5.2-7.6):(0.8-2.2) and stirring evenly to obtain a mixed positive electrode powder B;
[0010] Step 4, mixing the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% in a mass ratio of 100:(7-12), stirring evenly to obtain a mixture C, adding anhydrous ethanol to the mixture C in a mass ratio of 1:(150-200), stirring and ultrasonically mixing evenly to obtain a positive electrode slurry D;
[0011] Step 5: Load the positive electrode slurry D on the nickel foam as the positive electrode current collector, place it on a hot plate at 100-150° C., wait for the anhydrous ethanol to completely evaporate, then roll it step by step with a roller press, and dry it again to obtain a cobalt phthalocyanine catalytic electrode.
[0012] Furthermore, the soaking in step 2 is firstly soaking in deionized water for at least 12 hours, then removing the upper suspended matter, and then changing the water for soaking, and repeating 2 to 3 times.
[0013] Furthermore, the cleaning in step 2 is performed by successively using anhydrous ethanol and deionized water for 2 to 3 times each.
[0014] Furthermore, the drying in step 2 is carried out at 80-105° C. for 12-24 hours.
[0015] Furthermore, in step 5, the positive electrode slurry D is loaded on the nickel foam serving as the positive electrode current collector by: immersing the nickel foam in the positive electrode slurry D; or coating the positive electrode slurry D on the nickel foam using a coating machine; or first placing the nickel foam on a hot plate at 100 to 150° C., and then dripping the positive electrode slurry D onto the nickel foam using a dropper.
[0016] Furthermore, the process of gradually rolling the nickel foam with a roller press in step 5 is: first use the roller press to roll the nickel foam with a small pressure, then cut it, and then press it with working thicknesses of 1.75-2mm, 1.25-1.5mm, 0.75-1.0mm and 0.25-0.75mm in sequence to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.25-0.75mm.
[0017] Furthermore, the re-drying in step 5 is carried out at 60-80° C. for 8-24 hours.
[0018] A cobalt phthalocyanine catalytic electrode.
[0019] Application of cobalt phthalocyanine catalytic electrode as positive electrode for rechargeable lithium / thionyl chloride batteries.
[0020] Compared with the prior art, the present invention has the following technical effects:
[0021] The present invention prepares the cobalt phthalocyanine catalyst material by a solid phase sintering method. Since phthalocyanine is a macrocyclic compound with a large π structure conjugated system, aromatic π electrons are conjugated on the entire phthalocyanine ring, and it has both electron-donating and electron-accepting properties, and can be used as a good electron donor and acceptor. The conjugated macromolecule has a highly planar property, and the catalytic reaction can occur at the axial position of the plane, and has excellent catalytic performance. Moreover, the cavities in the ring can accommodate metal elements to form a complex, and have good thermal stability and chemical stability. Therefore, using cobalt phthalocyanine as a catalyst reduces the close stacking of LiCl and promotes Cl2 is converted into SOCl2, which is mixed with acetylene black with good conductivity to make a slurry, and loaded on nickel foam. The rechargeable Li / SOCl2 battery positive electrode is prepared by roller pressing, which solves the problem of poor reversibility of the existing lithium / thionyl chloride battery positive electrode, increases the cycle life of the battery, and improves the cycle stability of the battery; in addition, the conductive network formed by the combination of acetylene black and cobalt phthalocyanine catalytic material not only contributes to the rapid transmission of electrons in the battery and reduces the internal resistance of the battery, but also contributes to the decomposition of LiCl in the carbon coating and the pores during charging, thereby increasing the cycle life and reversible capacity of the battery.
[0022] In the cobalt phthalocyanine catalytic electrode prepared by the present invention, acetylene black cannot store Cl2, and Cl2 escapes from the surface of the positive electrode. The cobalt phthalocyanine catalytic material can promote the rapid conversion of Cl2 into SOCl2, which not only reduces the potential danger caused by Cl2 causing the volume expansion of the electrode, but also improves the reversible capacity and cycle life of the lithium / thionyl chloride battery.
[0023] The preparation method of the present invention has the characteristics of simple operation, good stability, good uniformity, high yield, low energy consumption and good repeatability. The catalyst can be effectively and evenly added to the carbon electrode, thereby improving the reversibility and charge-discharge performance of the lithium / thionyl chloride battery. Compared with the rechargeable lithium / thionyl chloride battery assembled with pure acetylene black as the electrode, the average coulombic efficiency of the rechargeable lithium / thionyl chloride battery assembled with the cobalt phthalocyanine catalyzed carbon electrode is improved by about 15%, and at a cycle specific capacity of 800 mAhg-1, it can be stably cycled 100 times. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a photo of the cobalt phthalocyanine catalytic electrode prepared in Example 1;
[0025] Figure 2 This is a SEM image of the cobalt phthalocyanine catalytic electrode prepared in Example 1;
[0026] FIG3( a) is a SEM image of the cobalt phthalocyanine catalytic material prepared in Example 1;
[0027] FIG3( b ) is a TEM image of the cobalt phthalocyanine catalytic material prepared in Example 1;
[0028] Figure 4 This is the FT-IR spectrum of the cobalt phthalocyanine catalytic material prepared in Example 1;
[0029] Figure 5 The cycle performance diagram of the rechargeable Li / SOCl2 battery assembled with the cobalt phthalocyanine catalytic electrode prepared in Example 1;
[0030] Figure 6 The charge and discharge curves of the rechargeable Li / SOCl2 battery assembled with the cobalt phthalocyanine catalytic electrode prepared in Example 1;
[0031] Figure 7 Schematic diagram of the structure of a rechargeable Li / SOCl2 battery assembled with the cobalt phthalocyanine catalytic electrode prepared in Example 1. DETAILED DESCRIPTION
[0032] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0033] Example 1
[0034] Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 0.82:1.2:0.61:0.12 to obtain a mixture A;
[0035] Step 2, placing mixture A in a muffle furnace, heating from room temperature to 140°C at a heating rate of 10°C / min in an air atmosphere and keeping the temperature for 0.5h, then heating to 270°C at a heating rate of 10°C / min, keeping the temperature for 2h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for at least 12h, removing the upper suspended matter, and then soaking in water, repeating this for 3 times, then washing with anhydrous ethanol 3 times, and then washing with deionized water 3 times, and drying at 105°C for 12h to obtain cobalt phthalocyanine catalytic material powder, recorded as CoPc;
[0036] Step 3, acetylene black and CoPc are mixed and stirred evenly in a mass ratio of 6:1, and repeatedly ground to obtain a mixed positive electrode powder B;
[0037] Step 4, the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% are mixed in a mass ratio of 100:10, and stirred evenly to obtain a mixture C, and the mixture C is added with anhydrous ethanol in a mass ratio of 1:150, stirred and ultrasonically mixed evenly to obtain a positive electrode slurry D;
[0038] Step 5. Place the nickel foam on a hot plate at 150°C, and use a disposable dropper to add positive electrode slurry D to the nickel foam. After the anhydrous ethanol is completely evaporated, first use a roller press to roll the nickel foam with a small pressure, then cut it, and then press it with working thicknesses of 1.75mm, 1.25mm, 0.75mm and 0.25mm in turn, and then dry it at 60°C for 24h to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.25mm.
[0039] from Figure 1 It can be seen that the cobalt phthalocyanine catalytic material is uniformly loaded on the foam nickel current collector.
[0040] from Figure 2 It can be seen that rod-shaped cobalt phthalocyanine CoPc is dispersed on acetylene black and uniformly loaded on the surface of nickel grains.
[0041] As can be seen from FIG. 3( a ) and FIG. 3( b ), cobalt phthalocyanine CoPc presents a rod-like structure with a length of 2 μm.
[0042] from Figure 4 It can be seen that Example 1 successfully synthesized the cobalt phthalocyanine catalytic material CoPc.
[0043] The cobalt phthalocyanine catalytic electrode prepared in Example 1 was assembled into a rechargeable Li / SOCl2 battery as shown in Figure 7. In the figure, the black color is the cobalt phthalocyanine catalytic positive electrode, and the purple color is the cobalt phthalocyanine catalytic material. The performance test of the assembled rechargeable Li / SOCl2 battery was performed. The results are as follows: Figure 5-6 As shown:
[0044] from Figure 5It can be seen that the rechargeable Li / SOCl2 battery assembled with the cobalt phthalocyanine catalytic electrode prepared in Example 1 has a high capacity of 800 mAh g -1 At the reversible specific capacity, it can be cycled about 100 times, and the coulombic efficiency is always maintained at about 98%, and the charge and discharge rate can reach 2000mAg -1 .
[0045] from Figure 6 It can be seen that the charging and discharging platforms of the rechargeable Li / SOCl2 battery assembled with the cobalt phthalocyanine catalytic electrode prepared in Example 1 are particularly stable.
[0046] Example 2
[0047] Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 0.65:1.60:0.70:0.30 to obtain a mixture A;
[0048] Step 2, placing mixture A in a muffle furnace, heating from room temperature to 150°C at a heating rate of 15°C / min in an air atmosphere and keeping the temperature for 1h, then heating to 290°C at a heating rate of 8°C / min, keeping the temperature for 3h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for at least 12h, removing the upper suspended matter, and then soaking in water, repeating this process twice, then washing with anhydrous ethanol 3 times, and then washing with deionized water 3 times, and drying at 100°C for 18h to obtain a cobalt phthalocyanine catalytic material powder, recorded as CoPc;
[0049] Step 3, acetylene black and CoPc are mixed and stirred evenly in a mass ratio of 7:2, and repeatedly ground to obtain a mixed positive electrode powder B;
[0050] Step 4, the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% are mixed in a mass ratio of 100:7, and stirred evenly to obtain a mixture C, and the mixture C is added with anhydrous ethanol in a mass ratio of 1:200, stirred and ultrasonically mixed evenly to obtain a positive electrode slurry D;
[0051] Step 5. Place a nickel foam with a diameter of 15 mm on a hot plate at 135°C, and use a disposable dropper to add positive electrode slurry D to the nickel foam. After the anhydrous ethanol is completely evaporated, first use a roller press to roll the nickel foam with a small pressure, then cut it, and then press it with working thicknesses of 1.75 mm, 1.25 mm, 0.75 mm and 0.25 mm in turn, and then dry it at 80°C for 12 hours to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.25 mm.
[0052] Example 3
[0053] Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 0.72:1.43:0.65:0.24 to obtain a mixture A;
[0054] Step 2, placing mixture A in a muffle furnace, heating from room temperature to 160°C at a heating rate of 20°C / min in an air atmosphere and keeping the temperature for 0.5h, then heating to 280°C at a heating rate of 5°C / min, keeping the temperature for 2.5h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for at least 12h, removing the upper suspended matter, and then soaking in water, repeating this for 3 times, then washing with anhydrous ethanol twice, and then washing with deionized water twice, drying at 80°C for 24h, and obtaining a cobalt phthalocyanine catalytic material powder, recorded as CoPc;
[0055] Step 3, acetylene black and CoPc are mixed and stirred evenly according to a mass ratio of 5.2:0.8, and repeatedly ground to obtain a mixed positive electrode powder B;
[0056] Step 4, the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% are mixed in a mass ratio of 100:8, and stirred evenly to obtain a mixture C, and the mixture C is added with anhydrous ethanol in a mass ratio of 1:175, stirred and ultrasonically mixed evenly to obtain a positive electrode slurry D;
[0057] Step 5. Soak the nickel foam with a diameter of 15 mm in the positive electrode slurry D for 1 minute, then take it out and place it on a hot plate at 100°C. After the anhydrous ethanol is completely evaporated, first use a roller press to roll the nickel foam with a small pressure, then cut it, and then press it with a working thickness of 2 mm, 1.5 mm, 1.0 mm and 0.75 mm in turn, and then dry it at 70°C for 16 hours to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.75 mm.
[0058] Example 4
[0059] Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 0.58:1.12:0.51:0.11 to obtain a mixture A;
[0060] Step 2, placing mixture A in a muffle furnace, heating from room temperature to 150°C at a heating rate of 10°C / min in an air atmosphere and keeping the temperature for 1.5h, then heating to 270°C at a heating rate of 5°C / min, keeping the temperature for 3h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for at least 12h, removing the upper suspended matter, and then soaking in water, repeating this process twice, then washing with anhydrous ethanol twice, and then washing with deionized water three times, and drying at 90°C for 20h to obtain a cobalt phthalocyanine catalytic material powder, recorded as CoPc;
[0061] Step 3, acetylene black and CoPc are mixed and stirred evenly according to a mass ratio of 6.4:1.5, and repeatedly ground to obtain a mixed positive electrode powder B;
[0062] Step 4, the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% are mixed in a mass ratio of 100:9, and stirred evenly to obtain a mixture C, and the mixture C is added with anhydrous ethanol in a mass ratio of 1:150, stirred and ultrasonically mixed evenly to obtain a positive electrode slurry D;
[0063] Step 5. Soak the nickel foam with a diameter of 15 mm in the positive electrode slurry D for 3 minutes, then take it out and place it on a hot plate at 125°C. After the anhydrous ethanol is completely evaporated, first use a roller press to roll the nickel foam with a small pressure, then cut it, and then press it with a working thickness of 2 mm, 1.5 mm, 1.0 mm and 0.5 mm in turn, and then dry it at 80°C for 8 hours to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.5 mm.
[0064] Example 5
[0065] Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate in a mass ratio of 0.86:1.73:0.78:0.36 to obtain a mixture A;
[0066] Step 2, placing mixture A in a muffle furnace, heating from room temperature to 140°C at a heating rate of 20°C / min in an air atmosphere and keeping the temperature for 2h, then heating to 290°C at a heating rate of 10°C / min, keeping the temperature for 2h, cooling naturally to room temperature, grinding into powder, soaking in deionized water for at least 12h, removing the upper suspended matter, and then soaking in water, repeating this for 3 times, then washing with anhydrous ethanol 3 times, then washing with deionized water 2 times, and drying at 105°C for 15h to obtain cobalt phthalocyanine catalytic material powder, recorded as CoPc;
[0067] Step 3, acetylene black and CoPc are mixed and stirred evenly according to a mass ratio of 7.6:2.2, and repeatedly ground to obtain a mixed positive electrode powder B;
[0068] Step 4, the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% are mixed in a mass ratio of 100:12, and stirred evenly to obtain a mixture C, and the mixture C is added with anhydrous ethanol in a mass ratio of 1:200, stirred and ultrasonically mixed evenly to obtain a positive electrode slurry D;
[0069] Step 5. Use a coating machine to coat the positive electrode slurry D on a nickel foam with a diameter of 15 mm. Place the nickel foam coated with the positive electrode slurry D on a hot plate at 140°C. After the anhydrous ethanol is completely evaporated, first use a roller press to roll the nickel foam with a small pressure, then cut it, and then press it in working thicknesses of 2 mm, 1.5 mm, 1.0 mm and 0.75 mm in turn. Then, dry it at 60°C for 20 hours to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.75 mm.
Claims
1. A method for preparing a cobalt phthalocyanine catalytic electrode, characterized in that: The steps include: Step 1, mixing and grinding phthalic anhydride, urea, cobalt chloride hexahydrate and ammonium molybdate tetrahydrate according to a mass ratio of (0.58-0.86):(1.12-1.73):(0.51-0.78):(0.11-0.36) to obtain a mixture A; Step 2, placing mixture A into a muffle furnace, heating from room temperature to 140-160° C. at a heating rate of 10-20° C. / min in an air atmosphere and keeping the temperature for 0.5-2 h, then heating to 270-290° C. at a heating rate of 5-10° C. / min, keeping the temperature for 2-3 h, cooling naturally to room temperature, grinding, soaking, washing and drying in sequence to obtain a phthalocyanine cobalt catalyst material powder; Step 3, mixing acetylene black and cobalt phthalocyanine catalyst material powders in a mass ratio of (5.2-7.6):(0.8-2.2) and stirring evenly to obtain a mixed positive electrode powder B; Step 4, mixing the mixed positive electrode powder B and the polytetrafluoroethylene emulsion with a solid content of 60% in a mass ratio of 100:(7-12), stirring evenly to obtain a mixture C, adding anhydrous ethanol to the mixture C in a mass ratio of 1:(150-200), stirring and ultrasonically mixing evenly to obtain a positive electrode slurry D; Step 5: Load the positive electrode slurry D on the nickel foam as the positive electrode current collector, place it on a hot plate at 100-150° C., wait for the anhydrous ethanol to completely evaporate, then roll it step by step with a roller press, and dry it again to obtain a cobalt phthalocyanine catalytic electrode.
2. The method for preparing the cobalt phthalocyanine catalytic electrode according to claim 1, characterized in that: The soaking in step 2 is to first soak in deionized water for at least 12 hours, then remove the upper suspended matter, and then change the water for soaking, and repeat 2 to 3 times.
3. The method for preparing the cobalt phthalocyanine catalytic electrode according to claim 1, characterized in that: The cleaning in step 2 is performed by using anhydrous ethanol and deionized water for 2 to 3 times respectively.
4. The method for preparing the cobalt phthalocyanine catalytic electrode according to claim 1, characterized in that: The drying in step 2 is carried out at 80-105° C. for 12-24 hours.
5. The method for preparing the cobalt phthalocyanine catalytic electrode according to claim 1, characterized in that: In step 5, the positive electrode slurry D is loaded on the nickel foam as the positive electrode current collector by: immersing the nickel foam in the positive electrode slurry D; or coating the positive electrode slurry D on the nickel foam using a coating machine; or first placing the nickel foam on a hot plate at 100 to 150° C., and then dripping the positive electrode slurry D onto the nickel foam using a dropper.
6. The method for preparing the cobalt phthalocyanine catalytic electrode according to claim 1, characterized in that: The process of step 5 of rolling the nickel foam with a roller press is as follows: first, the nickel foam is rolled with a small pressure using a roller press, and then cut, and then pressed with working thicknesses of 1.75-2 mm, 1.25-1.5 mm, 0.75-1.0 mm and 0.25-0.75 mm in sequence to obtain a cobalt phthalocyanine catalytic electrode with a thickness of 0.25-0.75 mm.
7. The method for preparing a cobalt phthalocyanine catalytic electrode according to claim 1, characterized in that: The second drying in step 5 is performed at 60-80° C. for 8-24 hours.
8. A cobalt phthalocyanine catalytic electrode prepared by the method according to any one of claims 1 to 7.
9. Use of the cobalt phthalocyanine catalytic electrode according to claim 8 as a positive electrode of a rechargeable lithium / thionyl chloride battery.