Multi-element modified single-crystal positive electrode material, preparation method thereof, lithium ion battery and power utilization device

By doping A and B elements into the single-crystal cathode material and forming a gradient-distributed ABO3 coating layer, the structural instability of the single-crystal cathode material under high lithium depletion is solved, thereby improving the cycle performance and capacity of the battery.

CN118943317APending Publication Date: 2024-11-12HUNAN SHANSHAN ENERGY TECH CO LTD
View PDF 0 Cites 10 Cited by

Patent Information

Application Number
CN202410859226.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing single-crystal cathode materials exhibit poor structural stability under high lithium delithiation levels, leading to deterioration in battery cycle performance and making it difficult to balance long-term and short-term performance.

Method used

A multi-element modified single-crystal cathode material is used by doping the single-crystal cathode material matrix with elements A and B, and forming a perovskite-like ABO3 coating layer on the surface. A is selected from La, Sr, Ca, Na, Nd, Ce, K, Rb, and Cs, and B is selected from Zr, Mo, W, Nb, Sn, Sb, Sc, Al, Ta, and Ti. The molar ratio of A to B is (0.033-1):1, and the concentrations of A and B elements gradually decrease from the surface to the center, forming a gradient distribution.

Benefits of technology

It enhances the structural stability and ionic conductivity of the material, improves lithium-ion transport, suppresses lattice strain and phase transition, and improves the cycle stability and capacity retention of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943317A_ABST
    Figure CN118943317A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-element modified single-crystal positive electrode material which comprises a single-crystal positive electrode material matrix, A and B are doped in the matrix, and the surface of the matrix is coated with an ABO3 coating layer of a perovskite-like structure. The invention further discloses a multi-element modified single-crystal positive electrode material, A and B are partially doped into a matrix body phase of the single-crystal positive electrode material, and a part of A and B form an ABO3 coating layer with a perovskite-like structure on the surface of the matrix of the single-crystal positive electrode material. The invention also discloses a preparation method of the multi-element modified single-crystal positive electrode material, and a lithium ion battery and an electric device comprising the multi-element modified single-crystal positive electrode material. In the multi-element modified single-crystal positive electrode material, the ABO3 coating layer improves the stability of the material, can be well fused with a single-crystal positive electrode material matrix, and has an obvious improvement effect on the capacity and the initial DCR of the single-crystal positive electrode material, and A and B doping and ABO3 coating can synergistically enhance the structural stability of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to a multi-element modified single crystal positive electrode material and a preparation method thereof, a lithium ion battery, and an electric device. Background Art

[0002] In recent years, electric vehicles have developed rapidly, and higher requirements have been placed on the energy density and cycle life of lithium-ion batteries. In order to achieve better battery performance, the operating voltage of single-crystal cathode materials has been continuously increased. As the amount of lithium desorption increases, the stability of the internal structure of the material deteriorates, resulting in a significant deterioration in the cycle performance, affecting the endurance and battery life of electric vehicles. At present, the problem of bulk stability of materials can be solved to a certain extent through doping, but the current doping work is difficult to take into account both long-term and short-term performance, and often leads to a certain capacity loss or an increase in initial impedance. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a multi-element modified single crystal positive electrode material and a preparation method thereof, a lithium ion battery, and an electrical device.

[0004] In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0005] A multi-element modified single crystal positive electrode material comprises a single crystal positive electrode material matrix, wherein the single crystal positive electrode material matrix is ​​doped with element A and element B, and the surface of the single crystal positive electrode material matrix is ​​coated with an ABO3 coating layer of a perovskite-like structure, wherein A is selected from at least one of La, Sr, Ca, Na, Nd, Ce, K, Rb, and Cs, and B is selected from at least one of Zr, Mo, W, Nb, Sn, Sb, Sc, Al, Ta, and Ti. In the multi-element modified single crystal positive electrode material, the molar ratio of A to B is (0.033-1):1.

[0006] Based on a general inventive concept, the present invention also provides a multi-element modified single crystal positive electrode material, characterized in that the multi-element includes element A and element B, and the element A and element B are partially doped into the bulk phase of the single crystal positive electrode material matrix, and partially form an ABO3 coating layer with a perovskite-like structure on the surface of the single crystal positive electrode material matrix, wherein the element A is selected from at least one of La, Sr, Ca, Na, Nd, Ce, K, Rb, and Cs, and the element B is selected from at least one of Zr, Mo, W, Nb, Sn, Sb, Sc, Al, Ta, and Ti. In the multi-element modified single crystal positive electrode material, the molar ratio of element A to element B is (0.033-1):1.

[0007] The above-mentioned multi-element modified single crystal positive electrode material, preferably, the single crystal positive electrode material matrix chemical formula is Lia Ni (1-x-y) Co x M y O₂, where 1 < a ≤ 1.1, 0 < x ≤ 0.4, 0 < y < 0.4, and M is selected from Mn or / and Al.

[0008] For the above-mentioned multi-element modified single-crystal cathode material, preferably, in the multi-element modified single-crystal cathode material, the element concentrations of A and B gradually decrease from the surface of the primary particles of the single-crystal cathode material towards the center of the primary particles of the single-crystal cathode material.

[0009] For the above-mentioned multi-element modified single-crystal cathode material, preferably, the primary particles of the multi-element modified single-crystal cathode material are regionally divided. The region with a distance of 0 ≤ L ≤ 0.3R from the surface of the primary particle is the first region, and the region with a distance of 0.3R < L ≤ R from the surface of the primary particle is the second region. In the first region: the concentrations of A and B elements decrease from the outside to the inside in a gradient distribution with a decreasing amplitude of 10.9% - 62% per 0.1R. In the second region: the concentrations of A and B elements decrease from the outside to the inside in a gradient distribution with a decreasing amplitude of 0.1% - 10% per 0.1R; for each of the above 0.1R intervals, the decreasing amplitude is obtained by dividing the concentration difference at both ends of the interval by the concentration at the outer end within the interval, where R is the radius of the primary particle of the multi-element modified single-crystal cathode material, and R is 0.3 - 1.5 μm.

[0010] In the single-crystal cathode material of the present invention, multi-element modification is adopted. The concentrations of A and B elements on the surface layer of the material are relatively high, and the formed ABO₃ coating layer is beneficial to resisting the erosion of the electrolyte, enhancing the cycle stability, and the formed perovskite coating layer of ABO₃ has a high ionic conductivity, which is beneficial to the rapid transmission of lithium ions. The ABO₃ coating layer can stabilize the oxygen on the surface of the material and also improve the cycle performance of the material; the low-concentration A and B element bulk doping is beneficial to suppressing the inherent lattice strain in the layered oxide, enhancing the mechanical strength of the material, and improving the crystal structure of the material. As is well known, when the doping amount of some elements is too much, it is not conducive to the capacity and cycle performance of the material, and the concentration gradient design of A and B elements in the single-crystal cathode material of the present invention enables the synergistic effect of doping and coating to not only optimize the capacity, but also enhance the stability of the material and inhibit gas release.

[0011] In the present invention, the doped elements enter the bulk phase, which can stabilize the interface / lattice, improve ion diffusion, and the coexistence of multiple structures improves the bulk phase stability. A perovskite coating is formed on the surface of the material, and the surface coating layer protects the interface and prevents electrolyte erosion.

[0012] Based on a general inventive concept, the present invention also provides a preparation method for the above-mentioned multi-element modified single-crystal cathode material, including the following steps:

[0013] (1) adding a single crystal positive electrode material precursor, a lithium source, a compound containing element A, and a compound containing element B into a solvent, performing wet ball milling and mixing, drying, and performing a first sintering after grinding;

[0014] (2) Grinding the material sintered in step (1) again, and then sintering the ground material for a second time. After sintering, naturally cooling to room temperature to obtain a multi-element modified single crystal positive electrode material.

[0015] In the above preparation method, preferably, in step (1), the amount of the compound containing element A added is 200-1500 ppm, and the amount of the compound containing element B added is 200-3000 ppm.

[0016] In the above preparation method, preferably, in step (1), the lithium source is selected from one or more of lithium hydroxide, lithium carbonate, lithium acetate or lithium nitrate;

[0017] The compound containing element A includes one or more of oxides, hydroxides, fluorides, nitrates, phosphates or sulfates containing element A;

[0018] The compound containing element B includes one or more of oxides, hydroxides, fluorides, nitrates, phosphates or sulfates containing element B.

[0019] In the above preparation method, preferably, in step (1), the rotation speed of the wet ball milling is 240-360 rpm / min, the time is 7-12 h, and the solvent is ethanol.

[0020] In the above preparation method, preferably, in step (1), the drying includes vacuum drying, the vacuum drying temperature is 60-120° C., and the vacuum drying time is 6-12 h.

[0021] In the above preparation method, preferably, in step (1), the first sintering is carried out in an oxygen atmosphere, the temperature of the first sintering is 400-700° C., and the sintering time is 2-5 hours.

[0022] In the above preparation method, preferably, in step (2), the second sintering is carried out in an oxygen atmosphere, and the second sintering is a staged sintering, firstly heating from room temperature to 400-600°C, keeping warm and calcining for 1-3h, then heating to 800-900°C, keeping warm and calcining for 7-12h.

[0023] Based on a general inventive concept, the present invention also provides a lithium-ion battery, which includes the above-mentioned multi-element modified single-crystal positive electrode material or the multi-element modified single-crystal positive electrode material prepared by the above-mentioned preparation method.

[0024] Based on a general inventive concept, the present invention also provides an electrical device, comprising the above-mentioned lithium-ion battery.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] (1) In the multi-element modified single crystal positive electrode material of the present invention, the coordination number of element A is XII, and the ion radius is relatively close to that of O ions. The coordination number of element B is VI. Part of A and B are doped into the bulk phase of the single crystal positive electrode material, which is beneficial to suppress the inherent lattice strain in the layered oxide, enhance the mechanical strength of the material, and improve the crystal structure of the material. A perovskite-like ABO3 coating layer is partially formed on the surface of the single crystal positive electrode material to improve the stability of the material. The ABO3 coating layer and the single crystal positive electrode material matrix can be well integrated, which has a significant improvement effect on the capacity and initial DCR of the positive electrode material. Doping and coating can synergistically enhance the structural stability of the material.

[0027] (2) The present invention partially introduces element A and element B into the bulk phase and partially locates them on the surface to form an ABO3 perovskite phase. Due to its structural compatibility, the perovskite phase can grow consistently into a layered structure, which can greatly suppress the inherent lattice strain in the layered oxide, thereby resulting in lasting structural and morphological stability, preventing side reactions and irreversible phases from extending into the overall particles. The multi-element modified single crystal positive electrode material has excellent long-term cycle stability at a high cut-off voltage of 4.45V.

[0028] (3) The multi-element modified single crystal positive electrode material of the present invention has an ABO3 type perovskite structure formed on its surface with an oxygen vacancy structure, which can serve as a transfer station for internal lattice oxygen. This structure can be introduced into the surface of the cathode material as an oxygen accommodating layer, thereby reducing the oxygen loss rate by increasing the energy barrier for the lattice oxide to escape from the cathode, thereby reducing oxygen release, stabilizing the bulk structure stability, and alleviating irreversible phase changes, which is beneficial to improving the gas production performance of the single crystal positive electrode material during long-term circulation or storage.

[0029] (4) The ABO3 type perovskite structure formed by the present invention can significantly improve the ionic conductivity of the material, which is beneficial to the rapid transmission of lithium ions. In addition, part of the ABO3 is located on the surface of the material, which can effectively inhibit the phase change caused by the contact between the material surface and the electrolyte, stabilize the cathode-electrolyte interface, and thus improve the stability and storage performance of the material.

[0030] (5) In the modified single crystal positive electrode material of the present invention, the concentrations of elements A and B gradually decrease from the surface of the single crystal positive electrode material primary particle to the center of the positive electrode material primary particle. The concentrations of elements A and B are distributed in a specific gradient in the material. Combined with the protective layer formed by the surface coating layer, the Li +Transport behavior reduces the structural degradation and phase transition behavior at the grain boundaries of high-nickel single crystal positive electrode materials, inhibits the generation of cracks in the particles, thereby improving the capacity and cycle stability of the material, and maintaining the intact structure even after multiple cycles.

[0031] (6) The preparation method of the present invention has a simple process. The use of wet grinding increases the fluidity between materials and generates greater friction between materials and between materials and equipment, which ultimately makes the prepared materials mixed more evenly. Some elements in the combination of A and B have a melting effect, which can reduce the sintering temperature and save sintering costs. The process is highly controllable, which is conducive to the partial doping of materials into the bulk phase and partial doping on the surface of the material, and the surface layer constructed by it has good uniformity. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 TEM and FFT data of the single crystal positive electrode material prepared in Example 1 of the present invention.

[0033] Figure 2 EPMA data of the single crystal positive electrode material prepared in Example 2 of the present invention.

[0034] Figure 3 EPMA point scan data of concentration variation from surface to bulk phase of the single crystal positive electrode material prepared in Example 2 of the present invention.

[0035] Figure 4 These are the high temperature DCR growth rate performance data of the single crystal positive electrode materials prepared in Examples 1-6 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION

[0036] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0037] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0039] In the following embodiments, the radius R of a primary particle is obtained by measuring the diameters of multiple single crystal particles using nano-measurer software and dividing the average by 2.

[0040] In the following embodiments, the gradient distribution of the concentrations of elements A and B from the outside to the inside is tested in the following manner: by using an electron probe X-ray microanalyzer (EPMA), 11 points with uniform spacing are selected from the surface of the single crystal particle to the center R, and the mass fractions of the elements contained in each embodiment are obtained by testing and converted into specific values ​​by calculation.

[0041] Embodiment 1:

[0042] A multi-element modified single crystal positive electrode material, comprising a single crystal positive electrode material matrix, the chemical formula of the single crystal positive electrode material matrix is ​​LiNi 0.8 Co 0.06 Mn 0.14 O2, Ca and Zr elements are doped in the single crystal positive electrode material matrix, and the surface of the matrix is ​​coated with a CaZrO3 coating layer with a perovskite-like structure. The molar ratio of Ca and Zr elements in the multi-element modified single crystal positive electrode material is 0.545:1.

[0043] The preparation method of the multi-element modified single crystal positive electrode material of this embodiment comprises the following steps:

[0044] (1) LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and dopant A: CaCO3, 600 ppm, and dopant B: ZrO2, 2500 ppm were weighed at the same time. The weighed raw materials were mixed with ethanol and ground for 9 h using a planetary ball mill with polyurethane balls and zirconium oxide grinding media. The speed of wet ball milling was 300 rpm / min.

[0045] (2) drying the wet raw material after ball milling in step (1) in a vacuum drying oven at 120° C. for 12 h to remove ethanol;

[0046] (3) grinding the raw material dried in step (2), then placing it in an alumina crucible, and sintering it at 600° C. in an oxygen atmosphere for 3 h;

[0047] (4) grinding the powder sintered in step (3) again;

[0048] (5) The powder ground in step (4) is placed in a zirconia crucible, and the temperature is increased from room temperature to 500°C at a heating rate of 3°C / min in an oxygen atmosphere, and the crucible is sintered for 3 hours. The crucible is then heated to 870°C, sintered for 12 hours, and cooled naturally to room temperature to obtain a multi-element modified single crystal positive electrode material, in which Ca and Zr elements are partially doped into the bulk of the single crystal positive electrode material, and partially form a CaZrO3 coating layer with a perovskite-like structure on the surface of the single crystal positive electrode material.

[0049] The TEM and FFT data of the single crystal positive electrode material in this embodiment are as follows: Figure 1 As shown, a coating layer can be observed on the surface of the single crystal particles, which can be attributed to the (020) plane of the CaZrO3 perovskite phase, confirming that a CaZrO3 coating layer is indeed formed on the surface of the single crystal positive electrode material.

[0050] The multi-element modified single crystal positive electrode material particles are divided into regions, the region with a distance of 0≤L≤0.3R from the surface of the primary particle is the first region, and the region with a distance of 0.3R<L≤R from the surface of the particle is the second region. In the first region, each 0.1R is divided into three intervals. In these three intervals, the concentration of element A decreases from the outside of the particle to the inside by 59.8%, 51.38% and 14.71% in a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 57.3%, 29.45% and 10.98% in a gradient distribution. ; In the second region, it is divided into 7 intervals every 0.1R. In these 7 intervals, the concentration of element A decreases from the outside of the particle to the inside by 9.7%, 8.64%, 7.11%, 5.99%, 4.97%, 3.15% and 2.71% in sequence, showing a gradient distribution; the concentration of element B decreases from the outside of the particle to the inside by 8.46%, 7.69%, 6.19%, 5.13%, 4.7%, 3.14% and 2.32% in sequence, showing a gradient distribution, wherein R is the radius of the primary particle of the multi-element modified single crystal positive electrode material, and R is 1.17μm.

[0051] Embodiment 2:

[0052] A multi-element modified single crystal positive electrode material, comprising a single crystal positive electrode material matrix, the chemical formula of the single crystal positive electrode material matrix is ​​LiNi 0.8 Co 0.06 Mn 0.14 O2, Ca and Nb elements are doped in the single crystal positive electrode material matrix, and the surface of the matrix is ​​coated with a CaNbO3 coating layer with a perovskite-like structure. The molar ratio of Ca and Nb elements in the multi-element modified single crystal positive electrode material is 0.93:1.

[0053] The preparation method of the multi-element modified single crystal positive electrode material of this embodiment comprises the following steps:

[0054] (1) LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and dopant A: CaCO3, 600 ppm, and dopant B: Nb2O5, 1500 ppm were weighed at the same time. The weighed raw materials were mixed with ethanol and ground for 9 h using a planetary ball mill with polyurethane balls and zirconium oxide grinding media. The speed of wet ball milling was 300 rpm / min.

[0055] (2) drying the wet raw material after ball milling in step (1) in a vacuum drying oven at 120° C. for 12 h to remove alcohol;

[0056] (3) grinding the raw material dried in step (2), then placing it in an alumina crucible, heating it to 600° C. in an oxygen atmosphere and sintering it for 3 h;

[0057] (4) grinding the powder sintered in step (3) again;

[0058] (5) The powder ground in step (4) is placed in a zirconia crucible, and the temperature is increased from room temperature to 500°C at a heating rate of 3°C / min in an oxygen atmosphere, and the crucible is sintered for 3 hours. The crucible is then heated to 880°C, sintered for 12 hours, and cooled naturally to room temperature to obtain a multi-element modified single crystal positive electrode material, in which Ca and Nb elements are partially doped into the bulk of the single crystal positive electrode material, and partially form a CaNbO3 coating layer with a perovskite-like structure on the surface of the single crystal positive electrode material.

[0059] The EPMA data of the single crystal positive electrode material prepared in this example are as follows: Figure 2 As shown in the figure, it can be observed that Nb and C elements are enriched on the surface of the single crystal particles, and a clear gradient distribution is formed from the surface to the center. The EPMA line scan concentration change data from the surface to the bulk is shown in Figure 3 As shown in the figure, the concentrations of Ca and Nb elements decrease in different amplitudes from the surface to the bulk phase. The area with a distance of 0≤L≤0.3R from the surface of the primary particle is the first area, and the area with a distance of 0.3R<L≤R from the surface of the particle is the second area. In the first area, it is divided into three intervals at every 0.1R. In these three intervals, the concentration of element A decreases from the outside of the particle to the inside by 61.04%, 52.27% and 15.76% in a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 59.75%, 30.56% and 11.16% in a gradient distribution. degree distribution; in the second region, it is divided into 7 intervals every 0.1R, in which the concentration of element A decreases from the outside of the particle to the inside by 9.02%, 6.17%, 5.7%, 5.37%, 4.96%, 2.99% and 2.31% in sequence, showing a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 8.33%, 6.67%, 5.19%, 4.11%, 3.57%, 2.96% and 2.29% in sequence, showing a gradient distribution, wherein R is the radius of the primary particle of the multi-element modified single crystal positive electrode material, and R is 1.03μm.

[0060] Embodiment 3:

[0061] A multi-element modified single crystal positive electrode material, comprising a single crystal positive electrode material matrix, the chemical formula of the single crystal positive electrode material matrix is ​​LiNi 0.8 Co 0.06 Mn 0.14 O2, the positive electrode material matrix is ​​doped with Sr and Zr elements, the surface of the matrix is ​​coated with a SrZrO3 coating layer with a perovskite-like structure, and the element molar ratio of Sr and Zr in the positive electrode material is 0.41:1.

[0062] The preparation method of the multi-element modified single crystal positive electrode material of this embodiment comprises the following steps:

[0063] (1) LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and dopant A: SrO, 1000 ppm, and dopant B: ZrO2, 2500 ppm were weighed. The weighed raw materials were mixed with ethanol and ground using a planetary ball mill with polyurethane balls and zirconium oxide grinding media for 9 h. The speed of wet ball milling was 330 rpm / min.

[0064] (2) drying the wet raw material after ball milling in step (1) in a vacuum drying oven at 120° C. for 12 h to remove alcohol;

[0065] (3) grinding the raw material dried in step (2), then placing it in an alumina crucible, heating it to 600° C. in an oxygen atmosphere and sintering it for 3 h;

[0066] (4) grinding the powder sintered in step (3) again;

[0067] (5) The powder ground in step (4) is placed in a zirconia crucible, and the temperature is increased from room temperature to 500°C at a heating rate of 3°C / min in an oxygen atmosphere, and the crucible is sintered for 3 hours. The crucible is then heated to 870°C, sintered for 12 hours, and cooled naturally to room temperature to obtain a multi-element modified single crystal positive electrode material, in which Sr and Zr elements are partially doped into the bulk phase of the single crystal positive electrode material, and partially form a SrZrO3 coating layer with a perovskite-like structure on the surface of the single crystal positive electrode material.

[0068] The primary particles of the multi-element modified single crystal positive electrode material are divided into regions, the region with a distance of 0≤L≤0.3R from the surface of the primary particle is the first region, and the region with a distance of 0.3R<L≤R from the surface of the primary particle is the second region. In the first region, each 0.1R is divided into three intervals. In these three intervals, the concentration of element A decreases from the outside of the particle to the inside by 57.8%, 49.78% and 17.9% in a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 54.43%, 22.81% and 15.93% in a gradient distribution. In the second region, it is divided into 7 intervals at every 0.1R. In these 7 intervals, the concentration of element A decreases from the outside of the particle to the inside by 9.13%, 8.17%, 6.68%, 5.78%, 4.46%, 3.25% and 2.34% in sequence, showing a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 9.35%, 8.17%, 7.02%, 6.18%, 5.5%, 4.71% and 3.36% in sequence, showing a gradient distribution, wherein R is the radius of the multi-element modified single crystal positive electrode material particle, and R is 1.24μm.

[0069] Embodiment 4:

[0070] A multi-element modified single crystal positive electrode material, comprising a single crystal positive electrode material matrix, the chemical formula of the single crystal positive electrode material matrix is ​​LiNi 0.8 Co 0.06 Mn 0.14 O2, Sr and Ti elements are doped in the single crystal positive electrode material matrix, and the surface of the matrix is ​​coated with a SrTiO3 coating layer with a perovskite-like structure. The molar ratio of Sr and Ti elements in the positive electrode material is 0.547:1.

[0071] The preparation method of the multi-element modified single crystal positive electrode material of this embodiment comprises the following steps:

[0072] (1) LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and dopant A: SrO, 1000 ppm, dopant B: TiO2, 1000 ppm were weighed at the same time. The weighed raw materials were mixed with ethanol and ground for 10 h using a planetary ball mill with polyurethane balls and zirconium oxide grinding media. The speed of wet ball milling was 350 rpm / min.

[0073] (2) drying the wet raw material after ball milling in step (1) in a vacuum drying oven at 120° C. for 12 h to remove alcohol;

[0074] (3) grinding the raw material dried in step (2), then placing it in an alumina crucible, heating it to 600° C. in an oxygen atmosphere and sintering it for 3 h;

[0075] (4) grinding the powder sintered in step (3) again;

[0076] (5) The powder ground in step (4) is placed in a zirconia crucible, and the temperature is increased from room temperature to 500°C at a heating rate of 3°C / min in an oxygen atmosphere, and the crucible is sintered for 3 hours. The crucible is then heated to 880°C, sintered for 12 hours, and cooled naturally to room temperature to obtain a multi-element modified single crystal positive electrode material, in which the Sr and Ti elements are partially doped into the bulk phase of the single crystal positive electrode material, and partially form a SrTiO3 coating layer with a perovskite-like structure on the surface of the single crystal positive electrode material.

[0077] The primary particles of the multi-element modified single crystal positive electrode material are divided into regions, the region with a distance of 0≤L≤0.3R from the surface of the primary particle is the first region, and the region with a distance of 0.3R<L≤R from the surface of the primary particle is the second region. In the first region, each 0.1R is divided into 3 intervals. In these 3 intervals, the concentration of element A decreases from the outside of the particle to the inside by 60.08%, 53.48% and 21.9% in a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 57.53%, 24.17% and 17.33% in a gradient distribution. Distribution; in the second region, it is divided into 7 intervals every 0.1R, in these 7 intervals, the concentration of element A decreases from the outside of the particle to the inside by 9.35%, 7.97%, 6.43%, 5.4%, 4.51%, 3.75% and 2.04% in sequence, showing a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 8.97%, 8.04%, 7.38%, 6.23%, 5.49%, 4.43% and 3.19% in sequence, showing a gradient distribution, wherein R is the radius of the primary particle of the multi-element modified single crystal positive electrode material, and R is 1.13μm.

[0078] Embodiment 5:

[0079] A multi-element modified single crystal positive electrode material, comprising a single crystal positive electrode material matrix, the chemical formula of the single crystal positive electrode material matrix is ​​LiNi 0.8 Co 0.06 Mn 0.14 O2, Na and Nb elements are doped in the single crystal positive electrode material matrix, and the surface of the matrix is ​​coated with a NaNbO3 coating layer with a perovskite-like structure. The element molar ratio of Na and Nb in the single crystal positive electrode material is 0.675:1.

[0080] The preparation method of the multi-element modified single crystal positive electrode material of this embodiment comprises the following steps:

[0081] (1) LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and the dopant Na2CO3, 500 ppm, and the dopant B: Nb2O5, 1500 ppm were weighed at the same time. The weighed raw materials were mixed with ethanol and ground for 10 h using a planetary ball mill with polyurethane balls and zirconium oxide grinding media. The speed of wet ball milling was 340 rpm / min.

[0082] (2) drying the wet raw material after ball milling in step (1) in a vacuum drying oven at 120° C. for 12 h to remove alcohol;

[0083] (3) grinding the raw material dried in step (2), then placing it in an alumina crucible, heating it to 600° C. in an oxygen atmosphere and sintering it for 3 h;

[0084] (4) grinding the powder sintered in step (3) again;

[0085] (5) The powder ground in step (4) is placed in a zirconia crucible, and the temperature is increased from room temperature to 500°C at a heating rate of 3°C / min in an oxygen atmosphere, and the crucible is sintered for 3 hours. The crucible is then heated to 870°C, sintered for 12 hours, and cooled naturally to room temperature to obtain a multi-element modified single crystal positive electrode material, in which Na and Nb elements are partially doped into the bulk phase of the single crystal positive electrode material, and partially form a NaNbO3 coating layer with a perovskite-like structure on the surface of the single crystal positive electrode material.

[0086] The primary particles of the multi-element modified single crystal positive electrode material are divided into regions, the region with a distance of 0≤L≤0.3R from the surface of the primary particle is the first region, the region with a distance of 0.3R<L≤R from the surface of the primary particle is the second region, and the first region is divided into three intervals at every 0.1R. In these three intervals, the concentration of the A element decreases from the outside of the particle to the inside by 57.43%, 49.31% and 18.64% in a gradient distribution, and the concentration of the B element decreases from the outside of the particle to the inside by 56.18%, 26.94% and 14.33% in a gradient distribution. degree distribution; in the second region, it is divided into 7 intervals every 0.1R, in which the concentration of element A decreases from the outside of the particle to the inside by 9.17%, 8.11%, 6.98%, 5.35%, 4.66%, 3.81% and 2.15% in sequence, and the concentration of element B decreases from the outside of the particle to the inside by 8.78%, 7.83%, 7.01%, 6.49%, 5.11%, 4.08% and 3.2% in sequence, showing a gradient distribution, wherein R is the radius of the primary particle of the multi-element modified single crystal positive electrode material, and R is 1.08μm.

[0087] Embodiment 6:

[0088] A multi-element modified single crystal positive electrode material, comprising a single crystal positive electrode material matrix, the chemical formula of the single crystal positive electrode material matrix is ​​LiNi 0.8 Co 0.06 Mn 0.14 O2, the single crystal positive electrode material matrix is ​​doped with Na, La and Ti elements, and the surface of the matrix is ​​coated with Na 0.35 La 0.55 TiO3 coating layer, in which the element molar ratio of Na+La to Ti is 0.87:1.

[0089] The preparation method of the multi-element modified single crystal positive electrode material of this embodiment comprises the following steps:

[0090] (1) LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and dopant A: La2O3, 1000ppm, Na2CO3, 500ppm, and dopant B: TiO2, 1000ppm were weighed at the same time. The weighed raw materials were mixed with ethanol and ground for 11 hours using a planetary ball mill with polyurethane balls and zirconium oxide grinding media. The speed of wet ball milling was 355rpm / min.

[0091] (2) drying the wet raw material after ball milling in step (1) in a vacuum drying oven at 120° C. for 12 h to remove alcohol;

[0092] (3) grinding the raw material dried in step (2), then placing it in an alumina crucible, heating it to 600° C. in an oxygen atmosphere and sintering it for 3 h;

[0093] (4) grinding the powder sintered in step (3) again;

[0094] (5) placing the powder ground in step (4) into a zirconia crucible, heating the mixture from room temperature to 500° C. at a heating rate of 3° C. / min in an oxygen atmosphere, sintering the mixture for 3 h, then heating the mixture to 875° C., sintering the mixture for 12 h, and cooling the mixture naturally to room temperature to obtain a multi-element modified single crystal positive electrode material, wherein Na, La, and Ti elements are partially doped into the bulk phase of the single crystal positive electrode material, and Na, La, and Ti elements are partially doped into the surface of the single crystal positive electrode material to form a perovskite-like structure. 0.35 La 0.55 TiO3 coating layer.

[0095] The primary particles of the multi-element modified single crystal positive electrode material are divided into regions, the region with a distance of 0≤L≤0.3R from the surface of the primary particle is the first region, and the region with a distance of 0.3R<L≤R from the surface of the primary particle is the second region. In the first region, each 0.1R is divided into three intervals. In these three intervals, the concentration of element A decreases from the outside of the particle to the inside by 60.88%, 43.21% and 14.7% in a gradient distribution, and the concentration of element B decreases from the outside of the particle to the inside by 57.61%, 24.98% and 13.93% in a gradient distribution. In the second region, it is divided into 7 intervals every 0.1R. In these 7 intervals, the concentration of element A decreases from the outside of the particle to the inside by 9.54%, 8.36%, 7.15%, 6.45%, 4.99%, 3.64% and 2.17% in sequence, and the concentration of element B decreases from the outside of the particle to the inside by 8.17%, 7.04%, 6.15%, 5.39%, 4.78%, 3.79% and 3.04% in sequence, showing a gradient distribution, wherein R is the radius of the multi-element modified single crystal positive electrode material particle, and R is 1.15μm.

[0096] Comparative Example 1:

[0097] Except for dopant A: CaCO3, 2000ppm, dopant B: ZrO2, 2500ppm, the remaining steps and process parameters are the same as Example 1.

[0098] Comparative Example 2:

[0099] Except for dopant A: BaCO3, 1000ppm, dopant B: ZrO2, 2500ppm, the remaining steps and process parameters are the same as Example 1.

[0100] Comparative Example 3:

[0101] The preparation method of the single crystal positive electrode material in this comparative example is: LiOH·H2O and Ni 0.8 Co 0.06 Mn 0.14 The (OH)2 precursor was weighed at a molar ratio of 1.06:1, and dopant A: CaCO3, 600ppm, dopant B: ZrO2, 2500ppm were weighed and mixed evenly, and then placed in a zirconia crucible, and heated from room temperature to 500°C at a heating rate of 3°C / min in an oxygen atmosphere, and sintered for 3h, then heated to 870°C, sintered for 12h, and naturally cooled to room temperature. The prepared positive electrode material has the chemical formula of LiNi 0.8 Co 0.058 Mn 0.13785 Ca 0.00146 Zr 0.00269 O2, the single crystal positive electrode material has no coating layer.

[0102] The single crystal positive electrode material samples prepared in Examples 1-6 of the present invention and Comparative Examples 1-3 were used as ternary positive electrode active materials to assemble into CR2025 button half-cells: First, a single crystal positive electrode active material, acetylene black conductive agent, and polyvinylidene fluoride (PVDF) binder were mixed in a ratio of 8:1:1, and then an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added. The collected slurry was evenly coated on an aluminum foil. After drying at 120°C for 12 hours, the prepared cathode active material had a loading mass of 2.5 mg / cm 2 The battery was assembled in a glove box filled with Ar, with lithium metal as the anode, polypropylene (Celgard 2400) as the separator, and 1 mol / L LiPF6 dissolved in a mixture of ethyl carbonate and dimethyl carbonate (EC:DMC=1:1 by volume) as the electrolyte. The button-type half-cell was assembled and the electrochemical performance was tested.

[0103] Button half-cells assembled with the single crystal positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 were tested at a voltage window of 3.0-4.45 V. The obtained capacity, DCR, room temperature cycle performance, high temperature cycle performance and high temperature DCR growth rate performance are shown in Table 1.

[0104] Table 1 Single crystal positive electrode material buckling performance test results

[0105]

[0106]

[0107] It can be seen from Table 1 that the multi-element modified single crystal positive electrode materials prepared in Examples 1-6 can significantly improve DCR, room temperature cycle, high temperature cycle and high temperature DCR growth rate without losing capacity, especially Example 1, compared with Comparative Example 3, the capacity is slightly improved, the initial DCR at 10% SOC is reduced by 5.5Ω, and the capacity retention rate is still 96.2% after 30 cycles at 45°C. This is due to the fact that Ca and Zr are partially doped into the bulk phase to improve the material structure, and part of them are located on the surface of the material to form a CaZrO3 perovskite coating layer to improve stability, and CaZrO3 and the positive electrode material matrix can be well fused.

[0108] Comparative Example 1: Due to excessive CaCO3 doping, it is not conducive to suppressing phase change and the resulting structural instability, and the coating layer is too thick, which is not conducive to Li + The rapid transmission of the prepared material deteriorates the performance of the capacity, cycle and DCR. The introduction of Ba in Comparative Example 2 forms a BaZrO3 perovskite coating layer that is not conducive to DCR. In Comparative Example 3, no CaZrO3 coating layer is formed, and the electrochemical performance of the material is poor.

[0109] The button-type half-cells assembled with the single crystal positive electrode materials prepared in Examples 1-6 and Comparative Examples 1-3 have a DCR growth rate performance of 30 cycles at 45°C when the voltage window is 3.0-4.45V. Figure 4 As shown in the figure, it can be seen that the multi-element modified single crystal positive electrode material prepared in Example 3 has the best DCR growth rate. In addition, other embodiments also have better DCR growth rates than comparative examples 1-3, which is due to the improvement effect of the ABO3 structure on the material structure and stability.

Claims

1. A multi-element modified single crystal positive electrode material, characterized in that: It includes a single crystal positive electrode material matrix, wherein the single crystal positive electrode material matrix is ​​doped with element A and element B, and the surface of the single crystal positive electrode material matrix is ​​coated with an ABO3 coating layer with a perovskite-like structure, wherein element A is selected from at least one of La, Sr, Ca, Na, Nd, Ce, K, Rb, and Cs, and element B is selected from at least one of Zr, Mo, W, Nb, Sn, Sb, Sc, Al, Ta, and Ti. In the multi-element modified single crystal positive electrode material, the molar ratio of element A to element B is (0.033-1):

1.

2. A multi-element modified single crystal positive electrode material, characterized in that: The multi-element comprises element A and element B, wherein element A and element B are partially doped into the bulk phase of the single crystal positive electrode material matrix, and partially form an ABO3 coating layer of a perovskite-like structure on the surface of the single crystal positive electrode material matrix, wherein element A is selected from at least one of La, Sr, Ca, Na, Nd, Ce, K, Rb, and Cs, and element B is selected from at least one of Zr, Mo, W, Nb, Sn, Sb, Sc, Al, Ta, and Ti. In the multi-element modified single crystal positive electrode material, the molar ratio of element A to element B is (0.033-1):

1.

3. The multi-element modified single crystal positive electrode material according to claim 1 or 2, characterized in that: The chemical formula of the single-crystal cathode material matrix is Li a Ni (1-x-y) Co x M y O2, where 1 < a ≤ 1.1, 0 < x ≤ 0.4, 0 < y < 0.4, and M is selected from Mn or / and Al.

4. The multi-element modified single crystal positive electrode material according to claim 1 or 2, characterized in that: In the multi-element modified single crystal positive electrode material, the element concentrations of elements A and B gradually decrease from the surface of the single crystal positive electrode material primary particle to the center of the single crystal positive electrode material primary particle.

5. The multi-element modified single crystal positive electrode material according to claim 4, characterized in that: The primary particles of the multi-element modified single crystal positive electrode material are divided into regions, and the region with a distance of 0≤L≤0.3R from the surface of the primary particle is the first region, and the region with a distance of 0.3R<L≤R from the surface of the primary particle is the second region. In the first region: the concentrations of the A and B elements are distributed in a gradient from the outside to the inside, decreasing by 10.9%-62% per 0.1R; in the second region: the concentrations of the A and B elements are distributed in a gradient from the outside to the inside, decreasing by 0.1%-10% per 0.1R, wherein R is the radius of the primary particles of the multi-element modified single crystal positive electrode material.

6. The multi-element modified single crystal positive electrode material according to claim 1 or 2, characterized in that: The A element is selected from one, two or three of La, Sr, Ca, Na, Nd, Ce, K, Rb and Cs, and the B element is selected from one or two of Zr, Mo, W, Nb, Sn, Sb, Sc, Al, Ta and Ti.

7. A method for preparing a multi-element modified single crystal positive electrode material according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) adding a single crystal positive electrode material precursor, a lithium source, a compound containing element A, and a compound containing element B into a solvent, performing wet ball milling and mixing, drying, and performing a first sintering after grinding; (2) Grinding the material sintered in step (1) again, sintering the ground material for a second time, and naturally cooling to room temperature after sintering to obtain a multi-element modified single crystal positive electrode material.

8. The preparation method according to claim 7, characterized in that: In step (1), the amount of the compound containing element A added is 200-1500 ppm, and the amount of the compound containing element B added is 200-3000 ppm.

9. The preparation method according to claim 7, characterized in that: In step (1), the lithium source is selected from one or more of lithium hydroxide, lithium carbonate, lithium acetate or lithium nitrate; The compound containing element A includes one or more of oxides, hydroxides, fluorides, nitrates, phosphates or sulfates containing element A; The compound containing element B includes one or more of oxides, hydroxides, fluorides, nitrates, phosphates or sulfates containing element B.

10. The preparation method according to claim 7, characterized in that: In step (1), the rotation speed of wet ball milling is 240-360 rpm / min, and the ball milling time is 7-12 h.

11. The preparation method according to claim 7, characterized in that: In step (1), the drying includes vacuum drying, the vacuum drying temperature is 60-120° C., and the vacuum drying time is 6-12 hours.

12. The preparation method according to claim 7, characterized in that: In step (1), the first sintering is carried out in an oxygen atmosphere, the temperature of the first sintering is 400-700° C., and the sintering time is 2-5 hours.

13. The preparation method according to claim 7, characterized in that: In step (2), the second sintering is carried out in an oxygen atmosphere. The second sintering is a staged sintering, firstly heating from room temperature to 400-600°C, keeping the temperature for 1-3 hours, then heating to 800-900°C, keeping the temperature for 7-12 hours.

14. A lithium ion battery, characterized in that: The lithium-ion battery comprises the multi-element modified single crystal positive electrode material according to any one of claims 1 to 6 or the multi-element modified single crystal positive electrode material prepared by the preparation method according to any one of claims 7 to 13.

15. An electrical device, characterized in that: Includes the lithium ion battery as claimed in claim 14.

Citation Information

Cited By

  • Positive electrode material, preparation method and lithium ion battery

    CN119381445A

  • Cathode Material, Preparation Method and Lithium-Ion Battery

    CN119381445B

  • Low-cobalt high-voltage ternary positive electrode material and preparation method and application thereof

    CN119517962A

  • Coated modified positive electrode material precursor, preparation method thereof, positive electrode material and secondary battery

    CN119569140A

  • Coated modified positive electrode material precursor and preparation method thereof, positive electrode material, and secondary battery

    CN119569140B