Positive electrode active material for lithium secondary battery, method for preparing same, and secondary battery comprising same
By forming a coating of water-soluble polymer and oxygen deoxidant compounds on the surface of lithium-nickel-based metal oxide particles, the stability and side reaction problems of positive electrode active substances in lithium secondary batteries are solved, and a higher battery life is achieved and capacity.
Patent Information
- Application Number
- CN202410535090.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-04-30
- Publication Date
- 2024-11-12
AI Technical Summary
The operating stability and chemical reliability of the positive electrode active substances in lithium secondary batteries are insufficient, especially after the increase in nickel content, which leads to crystal structure deformation and side reactions, affecting the battery life and capacity maintenance.
The coating of water-soluble polymer and oxygen deodorant compound is formed on the surface of lithium-nickel-based metal oxide particles, and is prepared by heat treatment technology to inhibit oxygen production and side reactions and enhance crystal stability.
It effectively inhibits the capacity reduction and internal resistance caused by oxygen, improves the stability and chemical stability of active substance particles, extends the life of the battery and maintains high capacity characteristics.
Smart Images

Figure CN118943355A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material for a lithium secondary battery, a preparation method thereof, and a secondary battery comprising the positive electrode active material. More specifically, the present invention relates to a positive electrode active material for a lithium secondary battery containing lithium and nickel, a preparation method thereof, and a lithium secondary battery comprising the positive electrode active material. Background Art
[0002] Secondary batteries are batteries that can be repeatedly charged and discharged, and are widely used as power sources for portable electronic devices such as mobile phones and laptop computers. In addition, in recent years, battery packs including secondary batteries are being developed and used as power sources for environmentally friendly vehicles such as electric vehicles.
[0003] For example, lithium secondary batteries have high operating voltage and energy density per unit weight, and are advantageous in terms of charging speed and lightness, and therefore are being actively developed and applied.
[0004] As an active material for the positive electrode of a lithium secondary battery, a lithium-transition metal oxide can be used. Examples of the lithium-transition metal oxide include lithium-nickel-based metal oxides.
[0005] As the application range of lithium secondary batteries expands, longer life, high capacity and operational stability are required. In order to achieve a high-capacity positive electrode, the content of nickel contained in the lithium-nickel-based metal oxide is increasing. However, as the nickel content increases, deformation and damage to the crystal structure inside the positive electrode active material particles may occur. In addition, as the lithium secondary battery is repeatedly charged / discharged, side reactions may occur due to changes in the oxidation number of nickel. Summary of the invention
[0006] Technical issues to be solved
[0007] An object of the present invention is to provide a positive electrode active material for a lithium secondary battery having improved operational stability and chemical reliability.
[0008] An object of the present invention is to provide a method for preparing a positive electrode active material for a lithium secondary battery having improved operational stability and chemical reliability.
[0009] An object of the present invention is to provide a lithium secondary battery comprising the above-mentioned positive electrode active material for lithium secondary battery.
[0010] Technical Solution
[0011] A positive electrode active material for a lithium secondary battery includes: lithium-nickel-based metal oxide particles; and a coating layer formed on the surface of the lithium-nickel-based metal oxide particles and including a water-soluble polymer and an oxygen scavenger compound.
[0012] In some embodiments, the water-soluble polymer may include at least one selected from polydiallyldimethylammonium chloride, poly(acrylamide-co-diallyldimethylammonium chloride) copolymer, polyethyleneimine, polyethylene glycol, polyethylene glycol diglycidyl ether, dopamine, (3-glycidyloxypropyl)trimethoxysilane and poly(1-vinylpyrrolidone-co-2-dimethylaminoethyl methacrylate) copolymer.
[0013] In some embodiments, the oxygen scavenger compound may include an organic acid compound, a sulfite-based compound, or a phosphite-based compound.
[0014] In some embodiments, the organic acid compound may include ascorbic acid or a derivative thereof.
[0015] In some embodiments, the sulfite-based compound may include at least one of sodium sulfite, ammonium sulfite, calcium sulfite, potassium sulfite, and barium sulfite.
[0016] In some embodiments, the phosphite-based compound may be represented by Chemical Formula 3 below.
[0017] [Chemical formula 3]
[0018]
[0019] (In Chemical Formula 3, R 1 , R 2 and R 3 are independently hydrogen, C1-C 10 alkyl or silyl).
[0020] In some embodiments, a molar ratio of nickel among elements other than lithium and oxygen in the lithium-nickel-based metal oxide particles may be 0.8 or more.
[0021] In some embodiments, the water-soluble polymer may be present in an amount of 0.05-2 wt % relative to the weight of the lithium-nickel-based metal oxide particles.
[0022] In some embodiments, the content of the oxygen scavenger compound may be 0.02-1.5 wt % relative to the weight of the lithium-nickel-based metal oxide particles.
[0023] In some embodiments, the lithium-nickel-based metal oxide particles may have a secondary particle structure in which a plurality of primary particles are aggregated, and the coating layer may be formed at an outer surface of the secondary particle and an interface between the primary particles in an inner region of the secondary particle.
[0024] The lithium secondary battery includes: a positive electrode including the positive electrode active material of the above embodiment; and a negative electrode disposed opposite to the positive electrode.
[0025] In the method for preparing a positive electrode active material for a lithium secondary battery, lithium-nickel-based metal oxide particles are mixed with an aqueous solution containing a water-soluble polymer and an oxygen scavenger compound, and the lithium-nickel-based metal oxide particles mixed with the aqueous solution are heat-treated.
[0026] In some embodiments, the aqueous solution may include 5-20 wt % of water relative to the total weight of the lithium-nickel-based metal oxide particles.
[0027] In some embodiments, the aqueous solution may include 0.05-2 wt % of the water-soluble polymer and 0.02-1.5 wt % of the oxygen scavenger compound relative to the weight of the lithium-nickel-based metal oxide particles.
[0028] In some embodiments, the heat treatment may be performed at a temperature of 200-350°C.
[0029] Beneficial Effects
[0030] In the positive electrode active material for lithium secondary batteries according to an embodiment of the present invention, a coating comprising a water-soluble polymer and an oxygen scavenger compound can be formed on lithium-nickel-based metal oxide particles. The oxygen generated from the surface of the active material particles can be directly removed by the oxygen scavenger compound. Therefore, the capacity reduction and internal resistance increase caused by oxygen can be suppressed, and the crystal stability and chemical stability of the active material particles can be enhanced by the coating.
[0031] According to an exemplary embodiment, the active material particles including the coating layer may be prepared by mixing the primary active material particles with the aqueous solution in which the water-soluble polymer and the oxygen scavenger compound are dissolved and then heat-treating the mixture. Therefore, a separate water washing process using water may be omitted, and an impurity washing effect may be achieved while forming the coating layer.
[0032] The positive electrode active material for lithium secondary batteries of the present invention and the lithium secondary batteries containing the positive electrode active material can be widely used in electric vehicles, battery charging stations, other green technology fields such as solar power generation and wind power generation using batteries. The positive electrode active material and lithium secondary batteries of the present invention can be used in eco-friendly electric vehicles and hybrid vehicles, etc., to prevent climate change by suppressing air pollution and greenhouse gas emissions. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 and Figure 2 1 and 2 are a schematic plan view and a schematic cross-sectional view, respectively, showing a lithium secondary battery according to an exemplary embodiment.
[0034] Figure 3a , Figure 3b and Figure 3c The following are scanning electron microscope (SEM) images of the surfaces of the active material particles prepared according to Example 1, Example 4 and Comparative Example 1, respectively. DETAILED DESCRIPTION
[0035] According to an embodiment of the present invention, a positive electrode active material for a lithium secondary battery comprising lithium-nickel-based metal oxide particles and a coating layer and a preparation method thereof are provided. In addition, a lithium secondary battery comprising the positive electrode active material is provided.
[0036] Hereinafter, a positive electrode for a lithium secondary battery and a lithium secondary battery according to an exemplary embodiment will be described in more detail with reference to the accompanying drawings and embodiments. However, the accompanying drawings and embodiments are merely exemplary, and the present invention is not limited to the accompanying drawings and embodiments.
[0037] <Positive electrode active material for lithium secondary battery and preparation method thereof>
[0038] A positive electrode active material for a lithium secondary battery (hereinafter, may be simply referred to as a positive electrode active material) may include lithium-nickel-based metal oxide particles and a coating layer formed on the lithium-nickel-based metal oxide particles.
[0039] The lithium-nickel-based metal oxide particles contain lithium and nickel, and may further contain at least one metal element. For example, the lithium-nickel-based metal oxide particles may further contain at least one of manganese (Mn) and cobalt (Co). In one embodiment, the lithium-nickel-based metal oxide particles may further contain manganese and cobalt. In this case, the lithium-nickel-based metal oxide particles may contain Ni-Co-Mn (NCM) based lithium oxide.
[0040] According to an exemplary embodiment, among elements other than lithium and oxygen included in the lithium-nickel-based metal oxide particles, the content (molar ratio or atomic %) of Ni may be the largest.
[0041] For example, the content of Ni may be 0.6 or more, preferably 0.7 or more, and more preferably 0.8 or more. For example, the molar ratio of Ni may be 0.8 to 0.94, 0.82 to 0.94, 0.83 to 0.94, 0.84 to 0.94, 0.85 to 0.94, or 0.88 to 0.94.
[0042] Ni can be provided as a transition metal related to the power and capacity of a lithium secondary battery. Therefore, as described above, by applying a high-content (high-nickel (High-Ni)) composition to the positive electrode active material, a high-capacity positive electrode and a high-capacity lithium secondary battery can be provided.
[0043] However, as the Ni content increases, the long-term storage stability and life stability of the positive electrode or secondary battery may be relatively reduced. However, according to an exemplary embodiment, conductivity can be maintained by including Co, while life stability and capacity retention characteristics can be improved by Mn.
[0044] In some embodiments, the lithium-nickel-based metal oxide particles may include a layered structure or a crystal structure represented by the following Chemical Formula 1.
[0045] [Chemical formula 1]
[0046] Li a Ni x M b O2
[0047] In Chemical Formula 1, 0.8≤x≤0.94, 0.95≤a≤1.05, 0.06≤b≤0.2, and M may include at least one element of B, Al, Ti, V, Mn, Co, Zn, Y, Nb, Zr, Mo, Sn, Mg, Sr, Ba, and W.
[0048] In one embodiment, as described above, M may include Co and Mn, and may further include at least one element selected from B, Al, Ti, V, Zn, Y, Nb, Zr, Mo, Sn, Mg, Sr, Ba, and W.
[0049] For example, an element other than Co and Mn among the elements represented by M may be provided as a doping element or a surface coating element of the lithium-nickel-based metal oxide particles. The lithium-nickel-based metal oxide particles are passivated by the doping element or the surface coating element, thereby further improving the crystal stability and chemical stability of the lithium-nickel-based metal oxide particles.
[0050] The chemical structure represented by Chemical Formula 1 indicates a bonding relationship included in a layered structure or a crystal structure of the lithium-nickel-based metal oxide particle, and does not exclude other additional elements.
[0051] According to an embodiment of the present invention, a coating layer comprising a water-soluble polymer and an oxygen scavenger compound may be formed on the surface of the lithium-nickel-based metal oxide particles. The water-soluble polymer may provide a polymer matrix that fixes the oxygen scavenger compound to the surface of the lithium-nickel-based metal oxide particles.
[0052] According to an exemplary embodiment, the water-soluble polymer may include a polymer having increased solubility in water. Thus, the entire surface of the lithium-nickel-based metal oxide particles may be uniformly coated through a wet process.
[0053] In some embodiments, the water-soluble polymer may include a polymer having a solubility in water of 5% or more.
[0054] For example, the water-soluble polymer may include poly(diallyldimethyl ammonium chloride), poly(acrylamide-co-diallyldimethylammonium chloride), poly(acrylamide-co-diallyldimethylammonium chloride), poly(ethylene imine), poly(ethylene glycol), poly(ethylene glycol), dopamine, (3-glycidyloxypropyl)trimethoxysilane, poly(1-vinylpyrrolidone-co-2-dimethylaminoethyl methacrylate), poly(1-vinylpyrrolidone-co-2-dimethylaminoethyl methacrylate), etc. These may be used alone or in combination of two or more.
[0055] The oxygen scavenger compound may include a compound that can capture, remove, or decompose oxygen generated due to lattice structure deformation of the lithium-nickel-based metal oxide particles, a side reaction with an electrolyte, and the like.
[0056] The oxygen scavenger compound may contain a plurality of hydroxyl groups, a plurality of oxygen anions (oxyanion, -O - ) group or multiple alkoxy groups.
[0057] In an exemplary embodiment, the oxygen scavenger compound may include an organic acid compound containing a plurality of hydroxyl groups, a sulfite-based compound, and a phosphite-based compound.
[0058] In one embodiment of the present invention, the organic acid compound may include ascorbic acid or a derivative thereof. Non-limiting examples of the ascorbic acid derivative include ascorbyl glucoside, ethyl ascorbyl ether, sodium ascorbyl phosphate, etc. These may be used alone or in combination of two or more.
[0059] The sulfite-based compound may contain a sulfite anion represented by Chemical Formula 2 below.
[0060] [Chemical formula 2]
[0061]
[0062] For example, the sulfite-based compound may include a sulfite containing the sulfite anion. In some embodiments, the sulfite-based compound may include sodium sulfite, ammonium sulfite, calcium sulfite, potassium sulfite, barium sulfite, etc. In one embodiment, the sulfite-based compound may include sodium sulfite (Na2SO3). These may be used alone or in combination of two or more.
[0063] The phosphite-based compound may be represented by Chemical Formula 3 below.
[0064] [Chemical formula 3]
[0065]
[0066] In chemical formula 3, R 1 , R 2 and R 3 can be independently hydrogen, C1-C 10 an alkyl or silyl group.
[0067] In one embodiment, R 1 , R 2 , R 3 Each may independently be a C1-C5 alkyl group or a silyl group.
[0068] Hydrogen or a C1-C5 alkyl group may be bonded to the silicon atom of the silyl group. In one embodiment, a C1-C5 alkyl group may be bonded to the silicon atom of the silyl group.
[0069] In some embodiments, the phosphite-based compound may include tris(trimethylsilyl)phosphite (TMSPi), triethylphosphite (TEPi), and the like.
[0070] As described above, the lithium-nickel-based metal oxide particles may contain a high content of nickel (high nickel). In the high nickel positive active material, insertion / deinsertion of lithium ions may be repeated with repeated charging and discharging.
[0071] Therefore, the oxidation number of Ni changes (for example, Ni 3+ →Ni 4+ →Ni 2+ ), and may cause oxygen to be detached in the lattice structure or crystal structure of the positive electrode active material. The detached oxygen is released in the form of active free radicals, which may cause a side reaction with the electrolyte. Due to the side reaction, gases such as CO2 may be generated. The gases generated by the side reaction cause the volume expansion of the battery and may reduce the cycle characteristics and capacity retention rate of the battery.
[0072] According to an embodiment of the present invention, an oxygen scavenger compound can be distributed on the surface of the lithium-nickel-based metal oxide particles to directly capture and remove oxygen generated from the active material particles. Therefore, by directly reducing or removing the amount of active oxygen generated with repeated charge / discharge, side reactions with the electrolyte can be effectively blocked.
[0073] Furthermore, the oxygen scavenger compound can be uniformly distributed and fixed within the matrix provided by the water-soluble polymer, thereby continuously providing oxygen scavenging activity at the site where active oxygen is generated.
[0074] For example, when ascorbic acid is used as the oxygen scavenger compound, ascorbic acid may be converted into a dehydroascorbic acid (DHAA) form by dehydrogenation according to the following reaction formula 1, and may capture oxygen radicals to generate water according to reaction formula 2.
[0075] [Reaction 1]
[0076]
[0077] [Reaction 2]
[0078] AA+1 / 2O2→DHAA+H2O
[0079] As shown in the reaction formula, the coating can provide a barrier that directly removes oxygen before it is released to the outside of the active material. Therefore, the amount of gas that may be generated in the battery can be directly and effectively reduced.
[0080] The lithium-nickel-based metal oxide particles may have a secondary particle structure formed by the aggregation of a plurality of primary particles (e.g., more than 10, more than 20, more than 30, more than 40, more than 50 primary particles). According to an exemplary embodiment, the coating may be formed on the outer surface of the secondary particles, and may also be formed at the interface between the primary particles in the inner region of the secondary particles.
[0081] Therefore, the release of active oxygen from the outer surface of the lithium-nickel-based metal oxide particles can be suppressed, and active oxygen can be removed from the inside of the lithium-nickel-based metal oxide particles.
[0082] In some embodiments, the water-soluble polymer may be present in an amount of 0.05-2 wt % relative to the weight of the lithium-nickel-based metal oxide particles. Within the above range, the coating layer may be easily induced to penetrate into the interface of the primary particles, and the coating layer may be uniformly formed on the entire surface of the lithium-nickel-based metal oxide particles.
[0083] In one embodiment, the water-soluble polymer may be present in an amount of 0.1-1.5 wt%, 0.2-1 wt%, 0.4-1 wt%, or 0.5-1 wt%.
[0084] In some embodiments, the content of the oxygen scavenger compound can be 0.02-1.5 wt % relative to the weight of the lithium-nickel-based metal oxide particles. Within the above range, the capacity of the positive electrode active material can be prevented from decreasing while achieving sufficient deoxygenation efficiency. In addition, the dispersibility of the oxygen scavenger compound in the water-soluble polymer is enhanced, so that the oxygen scavenger compound molecules can be evenly distributed in the polymer matrix.
[0085] In one embodiment, the oxygen scavenger compound may be present in an amount of 0.1-1.5 wt % or 0.2-1 wt %.
[0086] The active material particles may be defined by the lithium-nickel-based metal oxide particles and the coating layer formed on the surface of the lithium-nickel-based metal oxide particles. The positive electrode active material may include a plurality of the active material particles.
[0087] For example, the amount of the active material particles may be 50 wt % or more of the total weight of the positive electrode active material. Preferably, the amount of the active material particles may be 60 wt % or more, 70 wt % or more, 80 wt % or more, or 90 wt % or more of the total weight of the positive electrode active material.
[0088] In one embodiment, the positive electrode active material may consist essentially of the active material particles.
[0089] In some embodiments, the positive electrode active material may further include a lithium cobalt oxide-based active material, a lithium manganese oxide-based active material, a lithium nickel oxide-based active material or a lithium iron phosphate (LFP)-based active material (e.g., LiFePO4) in addition to the above-mentioned active material particles.
[0090] In some embodiments, the positive electrode active material may optionally further include a lithium-rich layered oxide (LLO) / over-lithiated oxide (OLO)-based active material, a manganese-rich (Mn-rich)-based active material, a cobalt-less (Co-less)-based active material, etc. These may be used alone or in combination of two or more.
[0091] Hereinafter, a method for preparing the above-mentioned positive electrode active material will be described.
[0092] Lithium-nickel-based metal oxide particles may be prepared. For example, lithium-nickel-based metal oxide particles having a composition of Chemical Formula 1 may be prepared.
[0093] According to an exemplary embodiment, the lithium-nickel-based metal oxide particles may be prepared by reacting a nickel-containing precursor and a lithium precursor. The nickel-containing precursor may further contain, for example, manganese and / or cobalt.
[0094] In some embodiments, the nickel-containing precursor can be prepared in the form of a Ni-Co-Mn precursor (e.g., (NCM)-hydroxide). For example, the nickel-containing precursor can be prepared by reacting a nickel source, a cobalt source, and a manganese source together by coprecipitation. The nickel source, the cobalt source, and the manganese source can contain hydroxides, sulfates, carbonates, acetates, nitrates, etc. of nickel, cobalt, and manganese, respectively.
[0095] The lithium-nickel-based metal oxide particles in the form of secondary particles may be prepared by reacting the nickel-containing precursor with the lithium precursor (eg, lithium hydroxide or lithium carbonate) by, for example, a co-precipitation method.
[0096] In order to promote the coprecipitation reaction, a precipitant and / or a chelating agent may be used. The precipitant may include an alkaline compound such as sodium hydroxide (NaOH), sodium carbonate (Na2CO3), etc. The chelating agent may include, for example, aqueous ammonia, ammonium carbonate, etc.
[0097] In some embodiments, a doping element source represented by M in Chemical Formula 1 may be reacted together in addition to nickel, cobalt, and manganese.
[0098] In some embodiments, after the lithium-nickel-based metal oxide particles are prepared, a calcination process may be further performed. For example, the calcination process may be performed at a temperature of about 600-1000° C. Through the calcination process, the layered structure of the lithium-nickel-based metal oxide particles may be stabilized, and the doping elements may be fixed.
[0099] According to an exemplary embodiment, the lithium-nickel-based metal oxide particles may be mixed with an aqueous solution including the water-soluble polymer and an oxygen scavenger compound.
[0100] The aqueous solution may penetrate into interfaces of primary particles included in the lithium-nickel-based metal oxide particles by capillary force.
[0101] In some embodiments, the aqueous solution may contain 5-20 wt % water relative to the total weight of the lithium-nickel-based metal oxide particles, and in one embodiment, the aqueous solution may contain 10-20 wt % water. Within the above range, capillary phenomena may be promoted, and a coating at the interface of the primary particles may be easily formed.
[0102] The contents of the water-soluble polymer and the oxygen scavenger compound in the aqueous solution may be within the above content ranges.
[0103] The aqueous solution and the lithium-nickel-based metal oxide particles may be uniformly mixed and then vacuum dried, for example, at a temperature range of 100-140°C, preferably at a temperature range of 110-130°C.
[0104] Afterwards, the dried particles may be heat-treated in an oxygen atmosphere to obtain active material particles with a coating formed thereon. The heat treatment may be performed at a temperature in the range of 150-400° C., and in one embodiment, the heat treatment may be performed at a temperature in the range of 200-350° C. Within the above temperature range, the oxygen scavenger compound may be effectively fixed without damaging the matrix of the water-soluble polymer.
[0105] In some embodiments, the impurities remaining on the surface of the lithium-nickel-based metal oxide particles can be reduced or removed by the wet coating process. For example, during the wet coating process, lithium impurities such as LiOH and Li2CO3 generated by unreacted lithium can be dissolved in the aqueous solution and removed.
[0106] Therefore, a separate water washing process using water (pure water) can be omitted. Therefore, surface damage and oxidation of the lithium-nickel-based metal oxide particles caused during the water washing process can be prevented.
[0107] <Lithium Secondary Battery>
[0108] Figure 1 and Figure 2 1 and 2 are schematic plan views and schematic cross-sectional views respectively showing a lithium secondary battery according to an exemplary embodiment. Figure 2 It is along Figure 1 A cross-sectional view taken along line I-I'.
[0109] Figure 1 and Figure 2 An exemplary battery structure is provided for the convenience of illustration, and the lithium secondary battery of the present invention is not limited to Figure 1 and Figure 2 The form shown.
[0110] Reference Figure 1 and Figure 2 The lithium secondary battery may include a positive electrode 100 and a negative electrode 130 , wherein the positive electrode 100 includes a positive electrode active material layer including the positive electrode active material for the lithium secondary battery, and the negative electrode 130 is disposed opposite to the positive electrode 100 .
[0111] The positive electrode 100 may include a positive electrode active material layer 110 formed by coating the positive electrode active material on a positive electrode collector 105 .
[0112] For example, the slurry can be prepared by mixing and stirring the positive active material according to the above embodiment with a binder, a conductive material and / or a dispersing material in a solvent. The positive active material layer 110 can be formed by coating the slurry on the positive current collector 105, drying and rolling.
[0113] The positive electrode current collector 105 may include, for example, stainless steel, nickel, aluminum, titanium, copper, or alloys thereof, and preferably may include aluminum or an aluminum alloy.
[0114] The adhesive may include an organic adhesive such as polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethylmethacrylate, or a water-based adhesive such as styrene-butadiene rubber (SBR), and may be used together with a thickener such as carboxymethyl cellulose (CMC).
[0115] For example, a PVDF-based binder may be used as a binder for forming a positive electrode. In this case, the amount of the binder used to form the positive active material layer 110 may be reduced, and the amount of the positive active material may be relatively increased, thereby improving the power and capacity of the secondary battery.
[0116] The conductive material may be included to promote electron migration between active material particles. For example, the conductive material may include carbon-based conductive materials such as graphite, carbon black, graphene, and carbon nanotubes and / or metal-based conductive materials such as perovskite materials such as tin, tin oxide, titanium oxide, LaSrCoO3, and LaSrMnO3.
[0117] The negative electrode 130 may include a negative electrode collector 125 and a negative electrode active material layer 120 formed by coating a negative electrode active material on the negative electrode collector 125 .
[0118] The negative electrode active material can be used without particular limitation as long as it is a material known in the art that can embed and de-embed lithium ions. For example, carbon-based materials such as crystalline carbon, amorphous carbon, carbon composites, and carbon fibers; lithium alloys; silicon (Si)-based compounds or tin, etc. can be used.
[0119] Examples of the amorphous carbon include hard carbon, coke, mesocarbon microbeads (MCMB), and mesophase pitch-based carbon fibers (MPCF).
[0120] Examples of the crystalline carbon include graphite-based carbon such as natural graphite, artificial graphite, graphitized coke, graphitized MCMB, and graphitized MPCF.
[0121] Examples of the element contained in the lithium alloy include aluminum, zinc, bismuth, cadmium, antimony, silicon, lead, tin, gallium, and indium.
[0122] The silicon-based compound may include, for example, silicon (Si), silicon oxide (e.g., SiO x, silicon-carbon composite compounds such as silicon carbide (SiC) where 0 < x < 2).
[0123] For example, the negative electrode active material can be mixed and stirred with the above-mentioned binder, conductive material, thickener, etc. in a solvent to form a slurry. The negative electrode 130 can be manufactured by coating the slurry on at least one surface of the negative electrode current collector 125 and then calendering and drying.
[0124] Substantially the same or similar materials as those used in the positive electrode active material layer 110 can be used for the binder and the conductive material. In some embodiments, for compatibility with carbon-based active materials, the binder used to form the negative electrode can include, for example, water-based binders such as styrene-butadiene rubber (SBR), and can be used together with thickeners such as carboxymethyl cellulose (CMC).
[0125] A separator 140 can be inserted between the positive electrode 100 and the negative electrode 130. The separator 140 can include a porous polymer membrane prepared from polyolefin-based polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, ethylene / methacrylate copolymer, etc. The separator 140 can also include a non-woven fabric formed from glass fibers with a high melting point, polyethylene terephthalate fibers, etc.
[0126] The separator 140 can also contain a ceramic-based material. For example, inorganic particles are coated on or dispersed in the polymer membrane, thereby improving heat resistance.
[0127] The separator 140 can have a single-layer or multi-layer structure including the above-mentioned polymer membrane and / or non-woven fabric.
[0128] In some embodiments, the area (e.g., the contact area with the separator 140) and / or volume of the negative electrode 130 can be larger than that of the positive electrode 100. Therefore, for example, lithium ions formed from the positive electrode 100 can migrate smoothly to the negative electrode 130 without precipitation in the middle.
[0129] According to an exemplary embodiment, a battery cell is defined by the positive electrode 100, the negative electrode 130, and the separator 140, and a plurality of battery cells can be stacked to form an electrode assembly 150 in the form of, for example, a jelly roll. For example, the electrode assembly 150 can be formed by winding, stacking, folding, etc. of the separator 140.
[0130] The electrode assembly 150 is accommodated in a housing 160 together with an electrolyte, thereby defining a lithium secondary battery. According to an exemplary embodiment, a non-aqueous electrolyte can be used for the electrolyte.
[0131] The non-aqueous electrolyte solution contains a lithium salt as an electrolyte and an organic solvent. + X - Indicates that, as the anion of the lithium salt (X - ), we can exemplify F - , Cl - Br - ,I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - wait.
[0132] The organic solvent may be, for example, propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl propyl carbonate, dipropyl carbonate, dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, vinylene carbonate, sulfolane, γ-butyrolactone, propylene sulfite, tetrahydrofuran, etc. These may be used alone or in combination of two or more.
[0133] like Figure 1As shown, the tabs (positive tabs and negative tabs) may protrude from the positive current collector 105 and the negative current collector 125 belonging to each battery cell and extend to one side of the shell 160. The tabs may be fused to the one side of the shell 160 and connected to the electrode leads (positive lead 107 and negative lead 127) extending to the outside of the shell 160 or exposed to the outside of the shell 160.
[0134] The lithium secondary battery may be manufactured in, for example, a cylindrical shape using a can, a prismatic shape, a pouch shape, a coin shape, or the like.
[0135] Below, experimental examples including specific embodiments are proposed to help understand the present invention, but these embodiments are only used to illustrate the content of the present invention and are not used to limit the claims. Various changes and modifications can be made to the embodiments within the scope of the scope of the present invention and technical ideas. This is obvious to those skilled in the art, and it is natural that such changes and modifications fall within the scope of the claims.
[0136] Examples and Comparative Examples
[0137] Preparation of Li[Ni 0.8 Co 0.1 Mn 0.1 ] Lithium-nickel-based metal oxide particles composed of ]O2. Specifically, lithium hydroxide as a lithium precursor and nickel-cobalt-manganese hydroxide as a composite metal precursor having a molar ratio corresponding to the above composition are uniformly mixed at a molar ratio of 1.01:1 to form a mixture. The mixture is placed in a calcining furnace, oxygen is supplied at a flow rate of 10L / min, and the temperature is increased to a temperature between 700-800°C at a heating rate of 2°C / min, and maintained at the increased temperature for 10 hours. After calcination, it is naturally cooled to room temperature, and subjected to a crushing and classification process to obtain lithium-nickel-based metal oxide particles as a positive electrode active material.
[0138] As shown in Table 1, a water-soluble polymer, an oxygen scavenger compound, and water were mixed to prepare an aqueous solution.
[0139] The prepared lithium-nickel-based metal oxide particles and the aqueous solution were mixed and stirred at the contents listed in Table 1 for 1 hour, and dried at 130° C. for 1 hour. Thereafter, heat treatment was performed at the temperature listed in Table 1 for 10 hours under an oxygen atmosphere to obtain active material particles having a coating layer formed thereon.
[0140] In Comparative Example 1, the aqueous solution coating process was omitted.
[0141] [Table 1]
[0142]
[0143]
[0144] Figure 3a , Figure 3b and Figure 3c The following are scanning electron microscope (SEM) images of the surfaces of the active material particles prepared according to Example 1, Example 4 and Comparative Example 1, respectively.
[0145] Reference Figure 3a to Figure 3c It can be confirmed that, when compared with Comparative Example 1 in which formation of a coating layer is omitted, on the lithium-nickel-based metal oxide particles in the example, the oxygen scavenger compound is fixed and distributed in the water-soluble polymer matrix.
[0146] See also Figure 3b , in Example 4, due to the increase in heat treatment temperature, areas where the polymer matrix was damaged and areas where the coating was uneven were observed.
[0147] Experimental example
[0148] (1) Measurement of residual lithium
[0149] 2.5 g of the active material particles of the embodiment and the comparative example were added to a 250 mL flask, and 110 g of deionized water was added, and then a magnetic bar was placed and stirred at 200 rpm for 10 minutes. After that, 100 g was taken after filtering using a reduced pressure flask. The solution was placed in an automatic measuring instrument (auto titrator) container, and the Li2CO3 value in the solution was measured by automatic titration with 0.1 N HCl according to the Wader method.
[0150] (2) Evaluation of coin-type half-cell capacity retention
[0151] The positive electrode active material prepared according to the embodiment and the comparative example, carbon black as a conductive material and polyvinylidene fluoride (PVDF) as a binder were mixed in a weight ratio of 92:5:3 to prepare a slurry. The slurry was uniformly coated on an aluminum foil having a thickness of 15 μm and vacuum dried at 130 ° C to manufacture a positive electrode for a lithium secondary battery. The positive electrode, a lithium foil as a counter electrode, and a porous polyethylene film (thickness: 21 μm) as a separator were used to form an electrode assembly.
[0152] A 2 mAh battery cell in the form of a coin-type half-cell was manufactured using the electrode assembly and a liquid electrolyte, wherein the liquid electrolyte was an electrolyte in which LiPF6 with a concentration of 1.0 M was dissolved in a solvent of ethylene carbonate and ethyl methyl carbonate mixed in a volume ratio of 3:7.
[0153] 1) Measurement of initial discharge capacity
[0154] The battery cells according to the examples and comparative examples were charged (CC / CV 0.1C 4.3V 0.005C CUT-OFF) and discharged (CC 0.1C 3.0V CUT-OFF) once to measure the initial discharge capacity (CC: constant current, CV: constant voltage).
[0155] 2) Measurement of capacity retention rate
[0156] For the cells according to the examples and comparative examples, charging (CC / CV 0.5C 4.3V 0.05C cut-off) and discharging (CC 1.0C 3.0V cut-off) were repeated 100 times as 1 cycle. The capacity retention was evaluated by dividing the discharge capacity of the 100th cycle by the discharge capacity of the 1st cycle.
[0157] (3) Evaluation of full cell characteristics
[0158] The positive electrode active material prepared by the embodiment and the comparative example, acetylene carbon black (Denka Black) as a conductive material and PVDF as a binder were mixed in a mass ratio of 94:3:3 to prepare a positive electrode mixture, and then the positive electrode mixture was coated on an aluminum current collector and dried and rolled to manufacture a positive electrode. The electrode density of the positive electrode after rolling was adjusted to 3.5 g / cubic centimeter (cc) or more.
[0159] A negative electrode slurry was prepared, which contained 93 wt% of natural graphite as a negative electrode active material, 5 wt% of a flake type conductive material KS6 as a conductive material, 1 wt% of styrene butadiene rubber (SBR) as a binder, and 1 wt% of carboxymethyl cellulose (CMC) as a thickener. The negative electrode slurry was coated on a copper substrate, dried, and rolled to manufacture a negative electrode.
[0160] The positive electrode and negative electrode manufactured as described above are cut (notching) into specified sizes respectively. A separator (polyethylene, 25 μm thick) is inserted between the positive electrode and the negative electrode to form a battery cell, and then the tabs of the positive electrode and the negative electrode are welded respectively. The welded positive electrode / separator / negative electrode assembly is placed in a soft package, and the three surfaces except the electrolyte injection surface are sealed. The portion with the tab is contained in the sealing portion. The electrolyte is injected through the electrolyte injection surface. The electrolyte injection surface is also sealed and immersed for more than 12 hours to manufacture a 20Ah level secondary battery.
[0161] The electrolyte used was an electrolyte prepared by adding 1 wt % vinylene carbonate (VC), 0.5 wt % 1,3-propylene sultone (PRS) and 0.5 wt % lithium bis(oxalatoborate) (LiBOB) to a 1 M LiPF6 solution using a mixed solvent of EC / EMC / DEC (25 / 45 / 30, volume ratio).
[0162] 1) Evaluation of 16-week capacity retention rate
[0163] The lithium secondary batteries of the above-mentioned embodiments and comparative examples were charged (CC-CV 0.1C, 4.2V, 0.05C cut-off) and discharged (CC 0.1C, 2.5V) to measure the initial discharge capacity. After that, the battery was charged (CC-CV 0.1C, 4.2V, 0.05C cut-off) and discharged to a depth of discharge (DOD) of 3%, thereby preparing a battery with a state of charge (SOC) of 97%.
[0164] The prepared battery was stored in a constant temperature chamber at 60°C, and the discharge capacity was measured by charging (CC-CV 0.1C 4.2V 0.05C cutoff) and discharging (CC 0.1C 2.5V cutoff) at week 16. The capacity retention rate was calculated by the percentage of the measured discharge capacity relative to the initial discharge capacity.
[0165] 2) Measurement of gas generation / CO2 content
[0166] The battery with SOC 97% prepared in 1) was stored in a constant temperature chamber at 60°C, and the amount of gas generated inside the battery was measured at week 16. Specifically, each battery was placed in a fixture designed according to the battery size, and a needle was passed through the fixture, and then the pressure change in the fixture was measured and converted into the amount of gas generated.
[0167] The gas extracted at week 16 was collected in a cartridge. The cartridge was mounted on a gas chromatograph-residual gas analyzer (GC-RGA) and the CO2 content (volume ratio) in the total gas was analyzed.
[0168] The evaluation results are shown in Table 2 below.
[0169] [Table 2]
[0170]
[0171] Referring to Table 2, improved capacity retention and gas inhibition characteristics were achieved in Examples 1 to 3 in which the coating layer including the water-soluble polymer and the oxygen scavenger compound including the organic acid, the sulfite-based compound, or the phosphite-based compound was formed.
[0172] In Example 4, where the heat treatment temperature was slightly increased, Figure 3bAs shown, the polymer matrix was partially damaged, and the CO2 suppression property was slightly reduced. In Example 5, where the heat treatment temperature was slightly low, the amount of lithium impurities increased because sufficient cleaning was not performed.
[0173] Compared to Example 3 using a phosphite-based compound as an oxygen scavenger, in Example 6 using a phosphate-based compound as an oxygen scavenger, the capacity characteristics were relatively reduced as a whole, and the generation of residual lithium / gas increased.
[0174] In Example 7 using inorganic particles as the deoxidizer, residual lithium and gas generation slightly increased due to reduced solubility in water.
[0175] In Example 8, in which the amounts of the water-soluble polymer and the oxygen scavenger were slightly increased, the initial capacity was relatively decreased.
[0176] In Example 9 using excess water, the residual lithium was sufficiently reduced and the initial capacity was improved because the deoxidizer was evenly applied. However, due to the damage of water to the positive electrode surface, the generation of gas was slightly increased and the capacity retention rate was relatively reduced.
[0177] In the comparative examples where the wet coating process is omitted or the water-soluble polymer or the oxygen scavenger compound is omitted, the generation of gas is significantly increased and the capacity retention rate is also reduced. For example, as shown in Comparative Examples 2 and 3, when the water-soluble polymer or the oxygen scavenger compound is used alone, the oxygen scavenging performance is substantially not achieved.
Claims
1. A positive electrode active material for a lithium secondary battery, comprising: Lithium-nickel based metal oxide particles; and A coating layer is formed on the surface of the lithium-nickel-based metal oxide particles and comprises a water-soluble polymer and an oxygen scavenger compound.
2. The positive electrode active material for lithium secondary battery according to claim 1, wherein The water-soluble polymer comprises at least one selected from the group consisting of polydiallyldimethylammonium chloride, poly(acrylamide-co-diallyldimethylammonium chloride) copolymer, polyethyleneimine, polyethylene glycol, polyethylene glycol diglycidyl ether, dopamine, (3-glycidyloxypropyl)trimethoxysilane and poly(1-vinylpyrrolidone-co-2-dimethylaminoethyl methacrylate) copolymer.
3. The positive electrode active material for lithium secondary battery according to claim 1, wherein The oxygen scavenger compound includes an organic acid compound, a sulfite-based compound, or a phosphite-based compound.
4. The positive electrode active material for lithium secondary battery according to claim 3, wherein The organic acid compound includes ascorbic acid or a derivative thereof.
5. The positive electrode active material for lithium secondary battery according to claim 3, wherein The sulfite-based compound includes at least one selected from the group consisting of sodium sulfite, ammonium sulfite, calcium sulfite, potassium sulfite, and barium sulfite.
6. The positive electrode active material for lithium secondary battery according to claim 3, wherein The phosphite-based compound is represented by the following Chemical Formula 3: [Chemical formula 3] In chemical formula 3, R 1 , R 2 and R 3 are independently hydrogen, C1-C 10 an alkyl or silyl group.
7. The positive electrode active material for lithium secondary battery according to claim 1, wherein The molar ratio of nickel in elements other than lithium and oxygen in the lithium-nickel-based metal oxide particles is 0.8 or more.
8. The positive electrode active material for lithium secondary battery according to claim 1, wherein The content of the water-soluble polymer is 0.05-2 wt % relative to the weight of the lithium-nickel-based metal oxide particles.
9. The positive electrode active material for lithium secondary battery according to claim 1, wherein The content of the oxygen scavenger compound is 0.02-1.5 wt % relative to the weight of the lithium-nickel-based metal oxide particles.
10. The positive electrode active material for lithium secondary battery according to claim 1, wherein The lithium-nickel-based metal oxide particles have a secondary particle structure formed by a plurality of primary particles agglomerating. The coating layer is formed at an interface between an outer surface of the secondary particle and the primary particle in an inner region of the secondary particle.
11. A lithium secondary battery comprising: A positive electrode, the positive electrode comprising the positive electrode active material for a lithium secondary battery according to claim 1; and A negative electrode is arranged opposite to the positive electrode.
12. A method for preparing a positive electrode active material for a lithium secondary battery, comprising the following steps: mixing lithium-nickel-based metal oxide particles with an aqueous solution comprising a water-soluble polymer and an oxygen scavenger compound; and The lithium-nickel-based metal oxide particles mixed with the aqueous solution are heat-treated.
13. The method for preparing a positive electrode active material for a lithium secondary battery according to claim 12, wherein: The aqueous solution contains 5-20 wt % of water relative to the total weight of the lithium-nickel-based metal oxide particles.
14. The method for preparing a positive electrode active material for a lithium secondary battery according to claim 13, wherein: The aqueous solution comprises 0.05-2 wt % of the water-soluble polymer and 0.02-1.5 wt % of the oxygen scavenger compound relative to the weight of the lithium-nickel-based metal oxide particles.
15. The method for preparing a positive electrode active material for a lithium secondary battery according to claim 12, wherein: The heat treatment is performed at a temperature of 200-350°C.