Lithium ion battery and electric equipment
By adding isoxazole compounds and limiting the content of silicon carbon materials in lithium-ion batteries, a stable SEI film is formed, which solves the problems of battery expansion and performance degradation, improves the magnification, low temperature and cycling performance, and extends the service life of the battery .
Patent Information
- Application Number
- CN202411353346.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-12
AI Technical Summary
When existing lithium-ion batteries increase their energy density, they are prone to lithium-ion separation, de-embedding imbalance and expansion problems, which affect the battery's rate performance, high and low temperature performance and cycling performance, resulting in capacity attenuation.
Add a specific content of isoxazole compounds to the electrolyte, and define the content of silicon-carbon materials in the negative electrode active material to form a stable SEI film, reduce the viscosity of the electrolyte, and improve the wettability and Li+ conductivity of the negative electrode silicon-carbon materials , promote charge transfer, enhance the mechanical strength and ionic conductivity of the SEI film.
Effectively suppress volume expansion, improve the battery's rate performance, high and low temperature performance and circulation performance, slow down capacity attenuation, improve charge and discharge rate and cycle stability, especially significantly improve battery performance under low temperature conditions.
Smart Images

Figure BDA0005062912430000021 
Figure BDA0005062912430000031 
Figure BDA0005062912430000032
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of secondary batteries, and specifically relates to a lithium-ion battery and electrical equipment. Background Art
[0002] With the growing demand for energy, high-performance, high-energy-density batteries have become the key to the development of modern science and technology. Lithium-ion batteries have been widely used in consumer electronics, new energy vehicles, and energy storage due to their high specific capacity, long cycle life, wide operating temperature range, and environmental friendliness. However, with the continuous expansion of the application fields of lithium-ion batteries, especially in the military, aviation, and new energy vehicles, higher requirements are placed on the electrical performance and safety of batteries.
[0003] Adding silicon-carbon materials to the negative electrode is an important means to increase energy density, but with the increase in surface density and silicon-carbon material content, problems such as lithium precipitation, unbalanced lithium insertion and extraction, and expansion often occur, resulting in battery capacity attenuation, rate performance, high and low temperature performance, and cycle performance. Therefore, how to increase energy density while suppressing expansion, thereby ensuring that the battery's rate performance, high and low temperature performance, and cycle performance are not affected or improved, and slowing down capacity attenuation, etc., is a technical problem that needs to be solved in the field. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present application is to overcome the defects in the prior art that in order to improve the energy density, expansion problems often occur, which in turn affects the battery's rate performance, high and low temperature performance, cycle performance and energy attenuation, thereby providing a lithium-ion battery and electrical equipment.
[0005] To this end, this application provides the following technical solutions:
[0006] According to one aspect of the present application, a lithium ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises an isoxazole compound, and the mass percentage content A% of the isoxazole compound is 1% to 40% based on the total mass of the electrolyte;
[0007] The negative electrode sheet comprises a negative electrode active material layer containing a negative electrode active material, wherein the negative electrode active material comprises a carbon-based material and a silicon-carbon material, and based on the total mass of the negative electrode active material layer, the mass percentage B% of the silicon-carbon material is 1.5% to 80%.
[0008] In some optional embodiments, the mass percentage A% of the isoxazole compound and the mass percentage B% of the silicon-carbon material satisfy: 0.4≤1.5×B / A≤4;
[0009] And / or, based on the total mass of the negative electrode active material layer, the mass percentage B% of the silicon-carbon material is 1.5% to 50%, preferably, B% is 3% to 40%;
[0010] And / or, based on the mass of the silicon-carbon material, the mass percentage E% of the silicon element is 35% to 70%.
[0011] In some optional embodiments, the isoxazole compound has the following structure:
[0012]
[0013] Wherein, R1, R2, and R3 are each independently selected from H, halogen, substituted or unsubstituted alkyl having 1 to 5 carbon atoms, substituted or unsubstituted cycloalkyl or heterocycloalkyl having 3 to 6 carbon atoms, substituted or unsubstituted alkenyl having 2 to 12 carbon atoms, substituted or unsubstituted alkynyl having 2 to 12 carbon atoms, CN, NH2, CHO, substituted or unsubstituted aryl or heteroaryl having 5 to 12 carbon atoms, substituted or unsubstituted aralkyl or heteroaralkyl having 6 to 24 carbon atoms, or, R2 and R3 together form a substituted or unsubstituted aromatic ring, wherein the substituents in the substituted alkyl, substituted alkyl or heterocycloalkyl, substituted alkenyl, substituted alkynyl, substituted aryl or heteroaryl, substituted aralkyl or heteroaralkyl, and substituted aromatic ring are selected from one or more of CN, NH2, halogen, and CHO; the heterocycloalkyl, heteroaryl, and heteroaralkyl refer to rings having nitrogen atoms, oxygen atoms, or sulfur atoms in the rings.
[0014] Preferably, the isoxazole compound comprises at least one of the following structures:
[0015]
[0016] In some optional embodiments, the electrolyte further includes fluorocarbonate, and the mass percentage C% of the fluorocarbonate is 7% to 20% based on the total mass of the electrolyte.
[0017] Preferably, the fluorinated carbonate includes at least one of fluoroethylene carbonate (FEC), bisfluoroethylene carbonate (DFEC), methyl trifluoroethyl carbonate (FEMC), difluoroethyl acetate (DFEA) and trifluoropropylene carbonate (TFPC).
[0018] In some optional embodiments, the carbon-based material includes graphite; preferably, the graphite includes artificial graphite and / or natural graphite; preferably, the Dv50 particle size of the carbon-based material is: 6 μm≤D1≤20 μm;
[0019] And / or, the Dv50 particle size of the silicon carbide material is: 5μm ≤ D2 ≤ 15μm.
[0020] In some alternative embodiments, the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon carbide material satisfy: 1 ≤ D1 / D2 ≤ 2.5.
[0021] In some alternative embodiments, for the mass percentage content A% of the isoxazole compound, the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon carbide material satisfy:
[0022]
[0023] In some alternative embodiments, the positive electrode sheet includes a positive electrode active material, and the general composition formula of the positive electrode active material is: Li x Co y M 1-y O2, where 0 < x < 1, 0 < y < 1, 0 < x + y < 1, and M is selected from one or more of Mg, Zn, Ga, Ba, Al, Fe, Cr, W, Sn, V, Mn, Sc, Ti, Nb, Mo, Zr.
[0024] In some alternative embodiments, the electrolyte further includes a polynitrile compound;
[0025] Preferably, based on the total mass of the electrolyte, the mass percentage content D% of the polynitrile compound is 1% to 7%;
[0026] Preferably, the polynitrile compound includes at least one of succinonitrile (SN), adiponitrile (ADN), 1,3,6-hexanetricarbonitrile (HTCN), glutaronitrile, suberonitrile, glycerol trinitrile (CAS No.: 2465-93-2), tetraether nitrile (CAS No.: 2465-94-3), pentaether nitrile (CAS No.: 55726-81-3).
[0027] According to another aspect of the present application, there is provided an electrical device including the lithium-ion battery provided above.
[0028] The technical solution of the present application has the following advantages:
[0029] In the present application, by adding a specific amount of isoxazole compounds to the electrolyte and limiting the content of silicon-carbon materials in the negative electrode active material to a reasonable range, a stable SEI film is formed while improving the energy density, inhibiting volume expansion, thereby ensuring the rate performance, high and low temperature performance and cycle performance of the battery, and slowing down capacity decay. Compared with conventional graphite, the expansion rate of silicon-carbon materials during the charging and discharging process is higher. Under low temperature conditions, the interface wettability of the negative electrode silicon-carbon material region is poor, and the electronic conductivity of the silicon-carbon material itself is also poor, resulting in its low electron transfer efficiency. In order to ensure the energy density while improving the electrical properties of silicon-carbon materials, the present application can reduce the viscosity of the electrolyte and improve the wettability of the negative electrode silicon-carbon material region at low temperatures by adding a specific amount of isoxazole compounds, thereby increasing the Li + The electrolyte is the medium for ion transport in the battery, and the reduction of its viscosity can also significantly enhance the mobility of ions, thereby improving Li + The migration speed in the electrolyte increases with the Li + With the increase in migration speed, the charge transfer process inside the battery is accelerated, thereby improving the current output capacity of the battery and the charge and discharge rate of the battery; at the same time, the aromaticity and nitrogen-oxygen-containing properties of isoxazole compounds enable them to form an SEI film rich in inorganic and organic polymers on the surface of the silicon-containing negative electrode. This film has good ionic conductivity and high mechanical strength, can adapt to the volume changes of silicon-carbon particles, maintain the integrity and stability of the silicon-carbon material, thereby reducing the expansion of silicon-carbon particles leading to the rupture of the negative electrode SEI film and the failure of the electrode, improving the cycle performance of the material, especially the low-temperature performance, and slowing down the capacity decay. DETAILED DESCRIPTION
[0030] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0031] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0032] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0033] According to one aspect of the present application, a lithium ion battery is provided, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises an isoxazole compound, and the mass percentage content A% of the isoxazole compound is 1% to 40% based on the total mass of the electrolyte;
[0034] The negative electrode sheet comprises a negative electrode active material layer containing a negative electrode active material, wherein the negative electrode active material comprises a carbon-based material and a silicon-carbon material, and based on the total mass of the negative electrode active material layer, the mass percentage B% of the silicon-carbon material is 1.5% to 80%.
[0035] In some optional embodiments, the mass percentage A% of the isoxazole compound is 1%, 3%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, or is within the range of any of the above values; the mass percentage B% of the silicon-carbon material is 1.5%, 2%, 5%, 7%, 9%, 10%, 12%, 14%, 16%, 18%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, or is within the range of any of the above values.
[0036] In some optional embodiments, based on the total mass of the electrolyte, the mass percentage A% of the isoxazole compound is 5% to 25%.
[0037] In the present application, by adding a specific content of isoxazole compounds to the electrolyte and limiting the content of silicon-carbon materials in the negative electrode active material layer to a reasonable range, a stable SEI film is formed while improving the energy density, inhibiting volume expansion, thereby ensuring the rate performance, high and low temperature performance and cycle performance of the battery, and slowing down capacity decay. Compared with conventional graphite, the expansion rate of silicon-carbon materials during the charging and discharging process is higher. Under low temperature conditions, the interface wettability of the negative electrode silicon-carbon material region is poor, and the electronic conductivity of the silicon-carbon material itself is also poor, resulting in its low electron transfer efficiency. In order to ensure the energy density while improving the electrical properties of silicon-carbon materials, the present application can reduce the viscosity of the electrolyte and improve the wettability of the negative electrode silicon-carbon material region by adding a specific content of isoxazole compounds, thereby increasing the Li + The electrolyte is the medium for ion transport in the battery, and the reduction of its viscosity can also significantly enhance the mobility of ions, thereby improving Li + The migration speed in the electrolyte increases with the Li +With the increase in migration speed, the charge transfer process inside the battery is accelerated, thereby improving the current output capacity of the battery and the charge and discharge rate of the battery; at the same time, the aromaticity and nitrogen-oxygen-containing properties of isoxazole compounds enable them to form an SEI film rich in inorganic and organic polymers on the surface of the silicon-containing negative electrode. This film has good ionic conductivity and high mechanical strength, can adapt to the volume changes of silicon-carbon particles, maintain the integrity and stability of the silicon-carbon material, thereby reducing the expansion of silicon-carbon particles leading to the rupture of the negative electrode SEI film and the failure of the electrode, improving the cycle performance of the material, especially the low-temperature performance, and slowing down the capacity decay.
[0038] If the content of isoxazole (IZ) compounds is too low, the interface will be unstable, and the side reactions inside the battery will increase, thus affecting the battery performance; if the content is too high, the chemical stability will deteriorate at high temperatures; if the content of silicon-carbon materials in the negative electrode active material is too low, the effect of increasing the energy density will not be achieved; if the content is too high, the initial coulombic efficiency will be low, and the volume will expand and shrink, and the mechanical stability of the electrode material will deteriorate, thus affecting the cycle life of the battery.
[0039] In some optional embodiments, the mass percentage content A% of the isoxazole compound and the mass percentage content B% of the silicon-carbon material satisfy: 0.4≤1.5×B / A≤4; as an example, the value of 1.5×B / A can be 0.4, 0.5, 1, 1.3, 1.5, 1.8, 2, 2.2, 2.5, 2.7, 3, 3.5, 4, or within the range of any of the above values. The present application defines that the relationship between the mass percentage content A% of the isoxazole compound and the mass percentage content B% of the silicon-carbon material meets the above requirements, ensuring that as the content of the silicon-carbon material increases, the content of the isoxazole compound also increases, thereby ensuring the stability of the negative electrode interface, alleviating the expansion caused by the silicon-carbon material, while further improving the energy density, inhibiting the expansion, and thus improving the cycle performance.
[0040] And / or, based on the total mass of the negative electrode active material layer, the mass percentage B% of the silicon-carbon material is 1.5% to 50%, preferably, B% is 3% to 40%;
[0041] And / or, the mass percentage E% of silicon element in the silicon-carbon material is 35% to 70%. The present application optimizes the silicon-carbon material content and silicon content in the negative electrode material, thereby improving the energy density and avoiding the instability of the electrode structure due to excessive silicon-carbon material content, while ensuring that the required content of isoxazole compounds is appropriate.
[0042] In some optional embodiments, the isoxazole compound has the following structure:
[0043]
[0044] Wherein, R1, R2, and R3 are each independently selected from H, halogen, substituted or unsubstituted alkyl having 1 to 5 carbon atoms, substituted or unsubstituted cycloalkyl or heterocycloalkyl having 3 to 6 carbon atoms, substituted or unsubstituted alkenyl having 2 to 12 carbon atoms, substituted or unsubstituted alkynyl having 2 to 12 carbon atoms, CN, NH2, CHO, substituted or unsubstituted aryl or heteroaryl having 5 to 12 carbon atoms, substituted or unsubstituted aralkyl or heteroaralkyl having 6 to 24 carbon atoms, or, R2 and R3 together form a substituted or unsubstituted aromatic ring, wherein the substituents in the substituted alkyl, substituted alkyl or heterocycloalkyl, substituted alkenyl, substituted alkynyl, substituted aryl or heteroaryl, substituted aralkyl or heteroaralkyl, and substituted aromatic ring are selected from one or more of CN, NH2, halogen, and CHO; the heterocycloalkyl, heteroaryl, and heteroaralkyl refer to rings having nitrogen atoms, oxygen atoms, or sulfur atoms in the rings.
[0045] In some optional embodiments, the isoxazole compound has any of the following structures:
[0046]
[0047] In some optional embodiments, the electrolyte further includes a fluorocarbonate, and the mass percentage C% of the fluorocarbonate is 7% to 20% based on the total mass of the electrolyte. As an example, the mass percentage C% of the fluorocarbonate is 7%, 9%, 11%, 13%, 15%, 17%, 19%, 20%, or within the range of any of the above values. The fluorocarbonate includes but is not limited to at least one of fluoroethylene carbonate (FEC), bisfluoroethylene carbonate (DFEC), methyl trifluoroethyl carbonate (FEMC), difluoroethyl acetate (DFEA) and trifluoropropylene carbonate (TFPC).
[0048] In the present application, fluorocarbonate can form a stable solid electrolyte interface (SEI) layer at the negative electrode, effectively preventing the lithium ions in the electrolyte from directly contacting the silicon-carbon material, slowing down the volume expansion and structural damage of the silicon-carbon material, in addition, the NO bond in the isoxazole compound is relatively weak, which may lead to easy fracture or rearrangement reaction at high temperature, thereby affecting its stability, and fluorocarbonate, due to the electron-withdrawing effect of its fluorinated substituent, usually has a higher oxidation potential, can improve the overall stability of the electrolyte, which helps to reduce the decomposition of the isoxazole compound in the electrolyte at high temperature, thereby extending the service life of the battery, therefore, when the content of isoxazole compounds is high, it is necessary to combine fluorocarbonate to further take into account high temperature performance. That is, the addition of fluorocarbonate can improve the cycle life, suppress the volume expansion and structural damage of silicon-carbon materials, while taking into account high temperature performance. If the content of fluorocarbonate is too low to effectively form a long-term stable solid electrolyte interface (SEI) film, the cycle stability and safety of the battery are reduced, and the excessively high content will increase the viscosity and internal resistance of the electrolyte, which is not conducive to lithium ion deintercalation.
[0049] In some optional embodiments, the negative electrode active material also includes a carbon-based material, and the carbon-based material includes graphite; preferably, the graphite includes artificial graphite and / or natural graphite, wherein the Dv50 particle size of the carbon-based material is: 6μm≤D1≤20μm; the Dv50 particle size of the silicon-carbon material is: 5μm≤D2≤15μm. As an example, the Dv50 particle size of the carbon-based material is 6μm, 8μm, 10μm, 12μm, 14μm, 15μm, 16μm, 18μm, 20μm, or within the range of any of the above values; the Dv50 particle size of the silicon-carbon material is 5μm, 7μm, 9μm, 10μm, 11μm, 13μm, 15μm, or within the range of any of the above values. The present application improves the rate performance by limiting the particle size of carbon-based materials and silicon-carbon materials, while ensuring the cycle performance of the battery. This is because smaller carbon-based material particle sizes are conducive to the rapid diffusion of lithium ions, thereby improving the rate performance of the battery; however, too small a particle size can easily lead to an increase in the specific surface area, increase side reactions with the electrolyte, and affect the cycle life of the battery. Although larger carbon-based material particle sizes can reduce specific surface area and side reactions, they will reduce the rate performance of the battery. The same is true for silicon-carbon materials, but small particles of silicon-carbon materials are more likely to undergo drastic volume changes during the charge and discharge process, thereby increasing the stress inside the battery and causing instability in the electrode structure. Silicon-carbon material particles with larger particle sizes can alleviate the impact of volume expansion to a certain extent, but too large a particle size is not conducive to the insertion and removal of lithium ions.
[0050] In some optional embodiments, the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon-carbon material satisfy: 1≤D1 / D2≤2.5. As an example, the ratio D1 / D2 of the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon-carbon material is 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.5, or within the range of any of the above values. By limiting the particle size ratio, the present application enables small particles to fill the gaps in large particles, which helps to increase the compaction density of the pole piece, thereby improving the energy density of the battery.
[0051] In the present invention, the term "Dv50" refers to the particle size corresponding to when the cumulative volume particle size distribution percentage of a sample reaches 50%. Dv50 can be tested using a laser particle size analyzer.
[0052] In some optional embodiments, the mass percentage content A% of the isoxazole compound, the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon-carbon material satisfy: As an example, the mass percentage of the isoxazole compound A%, the relationship between the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon-carbon material The value is 0.5, 0.7, 0.9, 1, 1.2, 1.4, 1.5, 1.8, 2.0, 2.5, 3, or within the range of any of the above values. The present application is limited to make the Dv50 particle size of the carbon-based material, the Dv50 particle size of the silicon-carbon material, and the mass percentage of the isoxazole compound meet the above requirements, which can further reduce the impedance improvement kinetics, accelerate the insertion and extraction of lithium ions, enhance the stability of the negative electrode interface, reduce the interface side reaction, and extend the battery life while reducing the risk of thermal runaway. Appropriate carbon-based material particle size and silicon-carbon material particle size can utilize the buffering effect between the particles of the carbon-based material to effectively alleviate the volume expansion problem of the silicon-carbon material during the lithium insertion process. This helps to improve the cycle stability and capacity retention rate of the battery. As D1 / D2 increases, the interface side reaction intensifies, the electrode structure is unstable, the internal resistance increases, the heat accumulation increases, and the risk of thermal runaway increases. It is necessary to appropriately increase the content of the isoxazole compound to further reduce the impedance improvement kinetics, accelerate the insertion and extraction of lithium ions, reduce the interface side reaction, and extend the battery life.
[0053] In some optional embodiments, the positive electrode sheet includes a positive electrode active material, and the type of the positive electrode active material is a cobalt-containing positive electrode material, including one or more of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and transition metal lithium oxide. Preferably, the general formula of the positive electrode active material is: Li x Co y M 1-yO2, where 0 < x < 1, 0 < y < 1, 0 < x + y < 1, and M is selected from one or more of Mg, Zn, Ga, Ba, Al, Fe, Cr, W, Sn, V, Mn, Sc, Ti, Nb, Mo, Zr. In this application, doping the M element into the lithium cobalt oxide cathode material can improve the electronic conductivity and lattice stability of the cathode material, enhance the stability of the CEI film interface formed on the cathode, thereby inhibiting phase transformation and reducing Co dissolution, indirectly reducing side reactions at the anode interface, promoting long-cycle stability and excellent rate performance. In addition, when lithium cobalt oxide operates at high voltage, its structure may undergo irreversible changes, such as the slippage and phase transformation of the layered structure. Doping metal oxides can stabilize the crystal structure of lithium cobalt oxide and reduce the occurrence of these adverse changes. Doping metal oxides can also endow the battery with certain high-voltage resistance performance.
[0054] In some optional embodiments, the electrolyte further includes polynitrile compounds. Based on the total mass of the electrolyte, the mass percentage content D% of the polynitrile compounds is 1% - 7%. The polynitrile compounds include at least one of succinonitrile (SN), adiponitrile (ADN), 1,3,6-hexanetricarbonitrile (HTCN), glutaronitrile, suberonitrile, glycerol trinitrile, tetraether nitrile, pentaether nitrile. The applicant's research found that polynitrile compounds can form a protective film on the surface of the lithium cobalt oxide cathode, significantly improving the high-temperature performance of the lithium-ion battery. If the content of polynitrile compounds is too low, it is not conducive to forming a protective film on the cathode surface; if it is too high, the internal resistance increases, which is not conducive to the intercalation and deintercalation of lithium ions.
[0055] In this application, other compositions, content ranges, and preparation methods of the lithium-ion battery are all conventional in the art.
[0056] The electrolyte is a non-aqueous electrolyte. In addition to isoxazole compounds, fluorinated carbonates, and polynitrile compounds, the electrolyte also includes organic solvents, lithium salts, and other functional additives. Among them, the organic solvent can be selected from carbonates and / or carboxylates. The carbonate solvents can be selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl butyrate (EB), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and fluorinated derivatives of the above solvents. The carboxylate solvents can be selected from ethyl acetate (EA), propyl acetate, n-butyl acetate, isobutyl acetate, methyl propionate (MP), propyl propionate (PP), ethyl propionate (EP), methyl butyrate, n-ethyl butyrate, and fluorinated derivatives of the above solvents. The additives include one or more of vinylene carbonate (VC), ethylene vinylene carbonate (VEC), 1,3-propane sultone (PS), etc.
[0057] In the present application, the lithium salt includes one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI), lithium difluorooxalatoborate (LiDFOB), lithium bis(oxalatoborate) (LiBOB), lithium bis(fluorosulfonyl imide) (LiFSI) and lithium 4,5-dicyano-2-trifluoromethylimidazole (LiDTI), lithium difluorophosphate (LiPO2F2), and lithium difluorobis(oxalatophosphate).
[0058] The separator of the present application is not limited, and a conventional lithium-ion battery separator is selected.
[0059] In the present application, the positive electrode sheet includes a current collector and a positive electrode active material layer disposed on the surface of the current collector, and may also include a safety primer disposed between the current collector and the positive electrode active material layer on the surface, and the positive electrode active material layer includes 80% to 99.8% of positive electrode active material, 0.1% to 10% of conductive agent, and 0.1% to 10% of binder according to the mass percentage. Preferably, the positive electrode active material layer includes 90% to 99.6% of positive electrode active material, 0.2% to 5% of conductive agent, and 0.2% to 5% of binder according to the mass percentage.
[0060] The present application does not particularly limit the conductive agent in the positive electrode sheet, which can be selected from conductive agents conventionally used in the art, including but not limited to one or more of acetylene black, conductive carbon black, Ketjen black, conductive graphite, carbon nanotubes, conductive carbon fibers, and graphene.
[0061] The present application does not particularly limit the binder in the positive electrode sheet, which can be selected from binders conventionally used in the art, including but not limited to one or more of polyvinylidene fluoride, polytetrafluoroethylene, sodium carboxymethyl cellulose, styrene-butadiene rubber, and polyethylene oxide.
[0062] In a specific embodiment, the specific steps of preparing the transition metal lithium oxide include: firstly mixing the transition metal component with lithium cobalt oxide, performing a high temperature doping and sintering treatment at 1000-1100°C, and then performing a secondary high temperature coating and modification treatment at 800-1000°C to obtain the synthesized product.
[0063] The negative electrode sheet in the present application can be selected from the negative electrode sheets commonly used in the art, wherein the negative electrode sheet includes a current collector and a negative electrode active material layer disposed on the surface of the current collector. The negative electrode current collector can be selected from the negative electrode current collector commonly used in the art, such as copper foil.
[0064] In a specific embodiment, the negative electrode active material layer includes 80% to 99.8% of negative electrode active material, 0.1% to 10% of conductive agent, and 0.1% to 10% of binder by mass percentage. Preferably, the negative electrode active material layer includes 90% to 99.6% of negative electrode active material, 0.2% to 5% of conductive agent, and 0.2% to 5% of binder by mass percentage.
[0065] The types of negative electrode active materials in this application are mainly carbon-based materials and silicon-carbon materials, wherein the carbon-based materials may also include at least one of hard carbon, soft carbon, and graphene; the content of silicon element is 35% to 70% based on the total mass of the silicon-carbon material; the negative electrode active materials may also include other negative electrode active materials, such as lithium titanate, etc. This application does not specifically limit the types of conductive agents and binders in the negative electrode sheet, and the selection range can refer to the types of conductive agents and binders in the positive electrode sheet, which will not be repeated here.
[0066] The negative electrode sheet of the present application can be prepared by the following method: dispersing the negative electrode active material, the conductive agent and the binder in a solvent to form a negative electrode active slurry; then coating the negative electrode active slurry on the negative electrode collector, and drying to obtain the negative electrode sheet. The preparation method of the positive electrode sheet is similar to that of the negative electrode sheet, and will not be repeated here.
[0067] The present application does not specifically limit the preparation method of the lithium-ion battery, and the lithium-ion battery can be prepared by conventional preparation methods in the art. For example, the positive electrode sheet, the separator and the negative electrode sheet are stacked in sequence, so that the separator is located between the positive electrode sheet and the negative electrode sheet, and the battery core is obtained by stacking or winding, and then the lithium-ion battery of the present application is obtained through baking, liquid injection, formation, packaging and other processes.
[0068] According to another aspect of the present application, there is provided an electric device, comprising the lithium-ion battery provided above. The lithium-ion battery can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.
[0069] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0070] Example A1
[0071] This embodiment provides a lithium ion battery, the composition and specific preparation method of which are as follows:
[0072] 1) Preparation of positive electrode sheet: LiCo 0.95 Mg 0.03 Al 0.02 O2, conductive agent carbon black, and binder polyvinylidene fluoride were dispersed in N-methylpyrrolidone at a mass ratio of 97:2:1, and fully stirred to form a uniform positive electrode slurry. The positive electrode slurry was coated on aluminum foil (control surface density: 0.018 g / cm 2 ), after drying, rolling and cutting, the positive electrode sheet is obtained.
[0073] 2) Preparation of negative electrode sheet: artificial graphite (Dv50 is 14 μm), silicon-carbon composite material (Dv50 is 9.5 μm, the proportion of silicon in the silicon-carbon composite material is 40%), conductive agent carbon black, binder styrene-butadiene rubber, and thickener sodium carboxymethyl cellulose are weighed, and dispersed in deionized water according to the mass ratio of 84.2:12.9:0.5:1.1:1.3, and stirred thoroughly to form a uniform negative electrode slurry. The negative electrode slurry is coated on the negative electrode current collector copper foil (control surface density: 0.0068 g / cm 2 ), and then dried, rolled and cut to obtain the negative electrode sheet.
[0074] 3) Preparation of electrolyte: In a glove box filled with argon (H2O < 0.1ppm, O2 < 0.1ppm), EC, PC, and EB were mixed in a mass ratio of 10:15:65 to obtain a basic electrolyte solvent, and then 9.7% of 3-aminoisoxazole and 14% of lithium hexafluorophosphate (LiPF6) based on the total mass of the electrolyte were added to the basic electrolyte solvent. After dissolution, 4.5% of polynitrile compounds (1.5% of SN, 1.5% of ADN, 1.5% of HTCN) and 14% of FEC based on the total mass of the electrolyte were added, and the mixture was stirred evenly. After passing the moisture and free acid tests, the electrolyte was obtained.
[0075] 4) Diaphragm: PE porous polymer film is used as the isolation membrane.
[0076] 5) Assembly of lithium-ion battery: The positive electrode sheet, negative electrode sheet and separator prepared above are stacked in order so that the separator is between the positive electrode sheet and the negative electrode sheet, and then the pole ears are welded and wound to obtain a roll core, and the roll core is placed in an aluminum-plastic film packaging bag, and then the CA526477S lithium-ion battery is prepared through the processes of liquid injection, formation (85°C, 0.1Mpa, 0.2C constant current charging for 15min, 0.7C constant current charging for 60min), secondary sealing, and sorting.
[0077] Example A2-Example A20
[0078] The difference from Example A1 is that the mass percentage of the isoxazole compound is A%, the mass percentage of the silicon carbon is B% (the sum of the contents of artificial graphite and silicon carbon material in the negative electrode active material layer is 97.1%, and the artificial graphite is adjusted accordingly according to the content of the silicon carbon material), 1.5×B / A, the mass percentage of the fluorocarbonate is C%, the Dv50 of the carbon-based material, the Dv50 of the silicon carbon material, D1 / D2, The mass percentage content D% of the polynitrile compounds is different, as shown in Table 1.
[0079] Table 1
[0080]
[0081] Example A21
[0082] The difference from Example A1 is that the specific selection of the isoxazole compound is different. In this example, an isoxazole compound of formula (1) of equal mass is used to replace 3-aminoisoxazole in Example A1.
[0083] Example A22
[0084] The difference from Example A1 is that the specific selection of the isoxazole compound is different. In this example, an isoxazole compound of formula (3) of equal mass is used to replace 3-aminoisoxazole in Example A1.
[0085] Example A23
[0086] The difference from Example A1 is that the specific selection of the isoxazole compound is different. In this example, an isoxazole compound of formula (4) of equal mass is used to replace 3-aminoisoxazole in Example A1.
[0087] Example A24
[0088] The difference from Example A1 is that the specific selection of the isoxazole compound is different. In this example, an isoxazole compound of formula (5) of equal mass is used to replace 3-aminoisoxazole in Example A1.
[0089] Embodiment A25
[0090] The difference from Example A1 is that the specific selection of the positive electrode active material is different. In this example, lithium cobalt oxide of equal mass is used to replace the positive electrode active material LiCo in Example A1. 0.95 Mg 0.03 Al 0.02 O2.
[0091] Example A26
[0092] The difference from Example A1 is that the specific selection of the positive electrode active material is different. In this example, LiCo 0.95 Mg 0.03 Zn 0.02 O2 replaces the positive electrode active material LiCo in Example A1 0.95 Mg 0.03 Al 0.02 O2.
[0093] Example A27
[0094] The difference from Example A1 is that the specific selection of the negative electrode active material is different. In this example, natural graphite of equal mass is used to replace the artificial graphite in Example A1.
[0095] Example B1
[0096] The difference from Example A1 is that in the preparation step of the negative electrode sheet, the Dv50 of the artificial graphite and the silicon-carbon negative electrode materials are different, and FEC and polynitrile compounds are not added during the preparation of the electrolyte.
[0097] Example B2-Example B7
[0098] The difference from Example B1 is that the mass percentage of isoxazole compounds is A%, the mass percentage of the silicon-carbon material is B%, 2B / A, the mass percentage of fluorocarbonate is C, the Dv50 of carbon-based materials, the Dv50 of silicon-carbon materials, D1 / D2, A / 5ⅹ(D1 / D2), and the mass percentage of polynitrile compounds is D. See Table 2 for details.
[0099] Table 2
[0100]
[0101] Comparative Example 1
[0102] The difference from Example B1 is that the electrolyte does not include an isoxazole compound component, that is, A is 0.
[0103] Comparative Example 2
[0104] The difference from Example B1 is that, in the negative electrode active material, artificial graphite of equal mass is used instead of silicon-carbon material.
[0105] Comparative Example 3
[0106] The difference from Example B1 is that the content of isoxazole compounds in the electrolyte is 0.5%, and the mass percentage of silicon-carbon material in the negative electrode active material is 82%.
[0107] Comparative Example 4
[0108] The difference from Example B1 is that the content of isoxazole compounds in the electrolyte is 45%, and the mass percentage of silicon-carbon material in the negative electrode active material is 1%.
[0109] Test Case
[0110] 1. Low temperature performance test: The battery is discharged to 3V at 0.2C constant current, and after standing for 5 minutes, the lithium-ion battery is placed in a 5℃ environment. After standing for 4 hours, it is charged to the upper limit voltage (4.53V) at 0.3C constant current, and the thickness is measured as H0 after standing for 5 minutes; then it is discharged to 3.0V (the first cycle discharge capacity) at 0.5C constant current, and the thickness is measured as H0; the charge and discharge cycle is 100 times. The highest discharge capacity of the first three cycles is recorded as the initial capacity Q0, the discharge capacity of the 100th cycle is Q1, and the thickness after the battery is fully charged is H1. Calculate the battery capacity retention rate = Q1 / Q0×100%; thickness change rate = H1 / H0×100%.
[0111] 2. High temperature performance test: Place the lithium-ion battery in a 45°C environment, let it stand for 2 hours, and when the battery temperature is 45±2°C, charge it to the upper limit voltage (4.53V) at a constant current of 1.2C, then charge it to 0.05C at a constant voltage of 4.53V, let it stand for 5 minutes and measure the thickness as H2; then discharge it to 3.0V at a constant current of 0.5C, let it stand for 5 minutes, this is a charge and discharge cycle, and the charge and discharge cycle is 500 times. The highest discharge capacity of the first three cycles is recorded as the initial capacity Q2, the discharge capacity of the 500th time is Q3, and the thickness after the battery is fully charged is H3. Calculate the battery capacity retention rate = Q3 / Q2×100%; thickness change rate = H3 / H2×100%.
[0112] 3. Energy density: At 25°C, charge the lithium-ion battery at a constant current of 0.7C to an upper voltage of 4.53V, and then discharge it at 0.5C to a lower voltage of 3.0V. The discharge capacity is ED in Ah. The energy density of the lithium-ion battery is calculated using the following formula: Energy density = ED × operating voltage (3.82V) / (volume of the lithium-ion battery).
[0113] 4. 128℃ thermal shock test: The above lithium-ion battery is subjected to a 128℃ thermal shock test. The test process is as follows: First, the battery is charged at a constant current of 0.7C to an upper limit voltage of 4.53V, then charged at a constant voltage of 4.53V to 0.05C, and then the battery is placed in a convection or circulating hot air box, heated at an initial temperature of 25±3℃, with a heating rate of 5±2℃, and the test is terminated after the temperature is raised to 128±2℃ and maintained for 60 minutes. The passing standard of the 128℃ thermal shock test is: the battery cell does not catch fire or explode.
[0114] 5. Rate performance: Place the lithium-ion battery in a 45°C environment, charge it at a constant current of 1.2C to the upper limit voltage (4.53V), then charge it at a constant voltage of 4.53V to 0.05C, then discharge it at a constant current of 1C to 3.0V, and let it stand for 5 minutes. This is a charge and discharge cycle, and the charge and discharge cycle is repeated 5 times. The highest discharge capacity of the first three cycles of 1C discharge is recorded as the initial capacity Q4, and the discharge capacity of the 500th time is Q5. Calculate the capacity retention rate of batteries discharged at different rates = Q5 / Q4×100%, and compare it with the capacity retention rate in cycle test 2 = Q3 / Q2×100%;
[0115] 6. High-voltage performance comparison: The lithium-ion battery provided in Example A1 was subjected to a high-voltage performance test with reference to the high-temperature performance test in Part 2 above, except that the charge cut-off voltage was adjusted from 4.53V to 4.5V.
[0116] The specific test results are shown in the table below:
[0117] Table 3
[0118]
[0119] Table 4
[0120]
[0121] From the data in the table, it can be seen from the data comparison of Example A1 (4.53V) to Example A4 that isoxazole compounds can significantly improve low-temperature performance, and the addition amount in the preferred range can take into account high-temperature performance; from the data comparison of Example A1 (4.53V) and A5 to A9, it can be seen that the overall performance of silicon-carbon material content is better in the preferred range, but too little energy density decreases, too much thickness expansion is larger, and the rate performance is improved; from the data comparison of Example A1 (4.53V) and A10 to A12, it can be seen that the overall performance of fluorocarbonate is better in the limited range, but too much dosage will increase the viscosity of the electrolyte, which is not conducive to the cycle capacity retention and rate performance, and the risk of thermal runaway increases; from Example A1 (4.53V) and A13 to A15, it can be seen that the overall performance of graphite particle size is better in the limited range. The particle size of silicon-carbon material is good within the specified range, but when it is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large, the energy density is slightly reduced and the thickness is greatly expanded. When the particle size of silicon-carbon material is too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance. When the particle size of silicon-carbon material is too large or too small, it is not conducive to the cycle capacity retention and rate performance.
[0122] It can be seen from Examples B1 to B7 and Comparative Examples D1 to D4 that: Example B2, compared with B1, satisfies the parameter range of 1.5B / A, which is beneficial to cycle stability and improved energy density; Example B3, compared with B1, adds fluorocarbonate, which is beneficial to cycle stability and improved energy density; Example B4, compared with B1, is beneficial to cycle stability by limiting the particle sizes of graphite materials and silicon-carbon materials; Example B5, compared with B1, is beneficial to cycle stability, improved energy density and safety performance by limiting the particle sizes of carbon-based materials and silicon-carbon materials and making their ratios meet a specific proportional relationship; Example B6, compared with B1, is beneficial to high The low-temperature cycle stability, energy density and safety performance are improved, achieving a balance of performance; compared with Example B7 and B1, the addition of polynitrile compounds is beneficial to the high-temperature cycle stability; compared with Example B1, the low-temperature performance of Comparative Example D1 is significantly deteriorated without the addition of isoxazole compounds; compared with Example B1, Comparative Example D2 does not include silicon-carbon materials in the negative electrode active material, which will significantly reduce the energy density; compared with Example B1, the content of silicon-carbon materials in the negative electrode active material layer is too high, while the content of isoxazole compounds is too low, the energy density is improved, but the cycle performance is significantly deteriorated; compared with Example B1, Comparative Example D4 is too low in the negative electrode active material layer, while the content of isoxazole compounds is too high, and the high-temperature performance is significantly deteriorated.
[0123] From the data comparison of Example A1 (4.53V), A25 and Example A1 (4.5V), it can be seen that doping with metal oxides is beneficial to promoting long-cycle stability and rate performance. In addition, while high voltage ensures performance, energy density is also improved.
[0124] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection created by this application.
Claims
1. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the electrolyte comprises an isoxazole compound, and the mass percentage content A% of the isoxazole compound is 1% to 40% based on the total mass of the electrolyte; The negative electrode sheet comprises a negative electrode active material layer containing a negative electrode active material, wherein the negative electrode active material comprises a carbon-based material and a silicon-carbon material, and based on the total mass of the negative electrode active material layer, the mass percentage B% of the silicon-carbon material is 1.5% to 80%.
2. The lithium-ion battery according to claim 1, characterized in that The mass percentage content A% of the isoxazole compound and the mass percentage content B% of the silicon-carbon material satisfy: 0.4≤1.5×B / A≤4; And / or, based on the total mass of the electrolyte, the mass percentage A% of the isoxazole compound is 5% to 25%; And / or, based on the total mass of the negative electrode active material layer, the mass percentage B% of the silicon-carbon material is 1.5% to 50%, preferably, B% is 3% to 40%; And / or, based on the mass of the silicon-carbon material, the mass percentage E% of the silicon element is 35% to 70%.
3. The lithium ion battery according to claim 1 or 2, characterized in that: The isoxazole compound has the following structure: wherein R1, R2, and R3 are each independently selected from H, halogen, substituted or unsubstituted alkyl having 1 to 5 carbon atoms, substituted or unsubstituted cycloalkyl or heterocycloalkyl having 3 to 6 carbon atoms, substituted or unsubstituted alkenyl having 2 to 12 carbon atoms, substituted or unsubstituted alkynyl having 2 to 12 carbon atoms, CN, NH2, CHO, substituted or unsubstituted aryl or heteroaryl having 5 to 12 carbon atoms, substituted or unsubstituted aralkyl or heteroaralkyl having 6 to 24 carbon atoms, or R2 and R3 together form a substituted or unsubstituted aromatic ring, wherein the substituents in the substituted alkyl, substituted alkyl or heterocycloalkyl, substituted alkenyl, substituted alkynyl, substituted aryl or heteroaryl, substituted aralkyl or heteroaralkyl, and substituted aromatic ring are selected from one or more of CN, NH2, halogen, and CHO; Preferably, the isoxazole compound comprises at least one of the following structures:
4. The lithium ion battery according to claim 1 or 2, characterized in that: The electrolyte also includes a fluorocarbonate; Preferably, based on the total mass of the electrolyte, the mass percentage C% of the fluorocarbonate is 7% to 20%; Preferably, the fluorocarbonate includes at least one of fluoroethylene carbonate, bisfluoroethylene carbonate, methyl trifluoroethyl carbonate, difluoroethyl acetate and trifluoropropylene carbonate.
5. The lithium ion battery according to claim 1 or 2, characterized in that: The carbon-based material includes graphite; preferably, the graphite includes artificial graphite and / or natural graphite; preferably, the Dv50 particle size of the carbon-based material is: 6 μm≤D1≤20 μm; And / or, the Dv50 particle size of the silicon-carbon material is: 5 μm≤D2≤15 μm.
6. The lithium-ion battery according to claim 5, characterized in that: The Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon-carbon material satisfy: 1≤D1 / D2≤2.
5.
7. The lithium-ion battery according to claim 6, characterized in that: The mass percentage content of the isoxazole compound is A%, the Dv50 particle size D1 of the carbon-based material and the Dv50 particle size D2 of the silicon-carbon material satisfy the following:
8. The lithium ion battery according to claim 1 or 2, characterized in that: The positive electrode sheet includes a positive electrode active material, and the positive electrode active material includes a composition with the general formula Li x Co y M 1-y O2, where 0 < x < 1, 0 < y < 1, 0 < x + y < 1, and M is selected from one or more of Mg, Zn, Ga, Ba, Al, Fe, Cr, W, Sn, V, Mn, Sc, Ti, Nb, Mo, Zr.
9. The lithium ion battery according to claim 1 or 2, characterized in that: The electrolyte also includes a polynitrile compound; Preferably, based on the total mass of the electrolyte, the mass percentage D% of the polynitrile compound is 1% to 7%; Preferably, the polynitrile compound includes at least one of succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile, glutaronitrile, suberonitrile, glyceroltrinitrile, tetraethernitrile and pentaethernitrile.
10. An electrical device, characterized in that: A lithium ion battery comprising any one of claims 1 to 9.
Citation Information
Patent Citations
Quick-charging electrolyte and application thereof in lithium ion battery
CN114614096A
High and low temperature universal electrolyte and lithium ion battery containing electrolyte
CN114628784A
Low-temperature organic electrolyte taking isoxazole derivative as basic solvent and application of low-temperature organic electrolyte
CN116053579A
Low-temperature high-rate lithium ion battery electrolyte and application
CN116154302A
Battery
CN118645706A
Cited By
Lithium ion battery with silicon-carbon negative electrode
CN119518067A
Lithium ion secondary battery
CN119890408A
A lithium-ion secondary battery
CN119890408B
Fast-charging negative electrode sheet, lithium-ion battery and electric device
WO2025213970A1
Electrolyte and secondary battery using same
WO2026129442A1