Strong heat dissipation gallium oxide device integrated with thermoelectric material and preparation method
By introducing thermoelectric cooling modules or units into β-Ga2O3 devices, the heat dissipation performance is improved by utilizing the thermoelectric effect, which solves the problem of low thermal conductivity of β-Ga2O3 devices, achieving efficient heat dissipation and improved stability, making them suitable for high-power environments.
Patent Information
- Application Number
- CN202410996356.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The low thermal conductivity of β-Ga2O3 devices makes it difficult to dissipate heat, which affects electron mobility and device stability, limiting their application in high-power, high-temperature environments.
A thermoelectric cooling module or unit is set between the substrate and the heat transfer interface layer. A current is generated by applying a voltage, and the heat dissipation performance is improved by utilizing the thermoelectric effect. Heat accumulation is reduced by using a substrate with high thermal conductivity such as SiC or AlN.
It improves the heat dissipation capacity of the device, reduces energy loss, avoids the introduction of additional stress, enhances the stability and reliability of the device, and is suitable for high-power environments.
Smart Images

Figure CN118946238A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor devices, and in particular relates to a gallium oxide device and a preparation method thereof, which can be used as a microwave power device and a power electronic device. Background Art
[0002] Ga2O3 is a kind of ultra-wide bandgap semiconductor material, which is divided into five categories according to different crystal structures: α-Ga2O3, β-Ga2O3, γ-Ga2O3, δ-Ga2O3 and ε-Ga2O3. Among all kinds of Ga2O3 crystal structures, β-Ga2O3 has the most stable crystal structure under normal temperature and pressure conditions due to its excellent physical and chemical stability, and has become the most preferred material for preparing Ga2O3 devices. Compared with traditional semiconductors Si, Ge and third-generation semiconductors SiC, GaN, etc., β-Ga2O3 semiconductor materials have a bandgap width of up to 4.8eV and a critical breakdown field strength of up to 8MV / cm, which has higher output power density and breakdown voltage. At the same time, because β-Ga2O3 materials can be grown in wafers using the melt method like Si, compared with the expensive production cost of other wide bandgap semiconductor materials, it has a natural low-cost advantage and is the most promising material for the next generation of electronic devices.
[0003] Although β-Ga2O3 devices have been widely studied and reported, and have performed well in the fields of microwave power devices and power electronic devices, there are still many problems with this material that need to be solved. The most critical problem is that the thermal conductivity of β-Ga2O3 is extremely low, which is only one-thirtieth of SiC and one-tenth of GaN. Under high-power working conditions, low thermal conductivity makes it difficult for heat to be effectively dissipated from the heat source of the device, causing heat to accumulate rapidly in a small area, thereby affecting electron mobility and device stability. In addition, high temperature can induce thermal stress inside the device, which can cause device performance failure or shorten its service life. The low thermal conductivity of β-Ga2O3 greatly limits the application of β-Ga2O3 devices in high-power and high-temperature environments. Therefore, optimizing the heat dissipation performance of β-Ga2O3 devices is extremely critical to enhancing the electrical performance and stability of the device.
[0004] Patent document with application number CN202111669320.2 discloses a method for preparing a highly efficient heat dissipation diamond / Ga2O3 heterojunction diode, which grows an n-type Ga2O3 epitaxial layer on a diamond substrate and manufactures the device, enhancing the high-temperature stability of the device. However, there is a significant interface thermal resistance between the high thermal conductivity substrate and Ga2O3, which limits the improvement of the device's heat dissipation performance, so further optimization is still needed to improve its heat dissipation effect.
[0005] Patent document with application number CN202210192776.2 discloses a Ga2O3 Schottky diode with a P-type diamond tilted table junction terminal, the device structure is as follows Figure 5 As shown in the figure, it includes anode metal, P-type diamond layer, n-Ga2O3 drift layer, n+-Ga2O3 layer, cathode metal from top to bottom; the device deposits a diamond layer on the surface of the Ga2O3 device, which can cause heat to be directly dissipated from the device surface close to the heat source. However, the diamond deposition process needs to be carried out at extremely high temperatures, which may generate additional stress at the diamond interface, thereby affecting the overall performance of the device.
[0006] Patent document with application number CN202310474680.X discloses a heterogeneous integrated Ga2O3 field effect transistor with microchannel and a preparation method. The device structure is as follows Figure 6 As shown, it includes a supporting substrate and a gallium oxide layer with a metal electrode thereon, the gallium oxide layer has a first groove penetrating the gallium oxide layer, the supporting substrate has a second groove and a third groove for the inlet and outlet of the cooling medium, and the second groove is used to connect the first groove and the third groove; the Ga2O3 field effect transistor is an embedded microchannel prepared in the substrate, allowing the coolant to flow directly through the area close to the heat source, effectively reducing the heat conduction distance and improving the heat dissipation capacity of the device. However, this method requires continuous delivery of coolant when the device is running, which increases additional energy consumption, and its process is complex and the manufacturing cost is high. Summary of the invention
[0007] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and propose a strong heat dissipation Ga2O3 device integrated with thermoelectric materials and a preparation method, so as to further improve the heat dissipation efficiency of the Ga2O3 device, avoid the negative impact of introducing additional stress on device performance, and reduce energy loss.
[0008] The technical solutions for achieving the purpose of the present invention include the following:
[0009] Technical solution 1:
[0010] A Ga2O3 metal oxide semiconductor field effect transistor MOSFET with strong heat dissipation integrated with thermoelectric materials, comprising from bottom to top: a heat sink layer, a heat transfer interface layer, a substrate, a buffer layer, a channel layer, a dielectric layer and metal electrodes located on the channel layer and the dielectric layer, characterized in that:
[0011] A plurality of sequentially arranged thermoelectric cooling modules are provided between the substrate and the heat transfer interface layer, each thermoelectric cooling module comprises a symmetrical N-type thermoelectric material layer and a P-type thermoelectric material layer, and a patterned upper metal electrode layer and a lower metal electrode layer are provided on the upper and lower surfaces thereof respectively;
[0012] A substrate insulating layer is provided between the upper surface of the upper metal electrode layer and the lower surface of the substrate to achieve electrical isolation between the thermoelectric cooling module and the substrate;
[0013] Each of the thermoelectric cooling modules is wrapped with an insulating support material on its periphery to support the deposition and patterning of the lower metal electrode layer and to achieve mutual isolation between each of the thermoelectric cooling modules.
[0014] Preferably, the N-type thermoelectric material layer and the P-type thermoelectric material layer in each thermoelectric cooling module are symmetrically distributed at a spacing of 10 μm to 20 μm, and two adjacent thermoelectric cooling modules are distributed at an equal spacing of 10 μm to 30 μm.
[0015] Preferably, the N-type thermoelectric material layer in the thermoelectric cooling module is any one of Bi2Te3, Bi2(TeSe)3, PbTe or other N-type materials with thermoelectric effect, with a thickness of 0.03 μm to 3000 μm and a side length of 60 μm to 200 μm;
[0016] The P-type thermoelectric material layer in the thermoelectric cooling module is made of any one of Sb2Te3, (BiSb)2Te3, Bi2Te3 or other P-type materials with thermoelectric effect, and its thickness and side length are the same as those of the N-type thermoelectric material layer.
[0017] Preferably, the patterned upper metal electrode layer and the lower metal electrode layer are both made of Ni / Au, Au / Cu, Ni / Cu or other metals matching the thermoelectric material, with a thickness of 240 to 2100 nm, and are connected in series with each thermoelectric cooling module to apply voltage to form current, so that a temperature difference is formed between the upper and lower surfaces of the thermoelectric cooling module, thereby improving the heat dissipation capacity of the device;
[0018] The substrate insulating layer is made of SiO2 or Si3N4, and its thickness is 0.1μm to 1μm;
[0019] The insulating support material is any one of SiO2, Si3N4 or photoresist, and its thickness is the sum of the thickness of the upper metal electrode layer and the thermoelectric cooling module.
[0020] Technical solution 2:
[0021] A strong heat dissipation vertical Ga2O3 heterojunction diode HJD integrated with thermoelectric materials, comprising from bottom to top: a heat dissipation layer, a thermal interface layer, a cathode electrode, + β-Ga2O3 substrate layer, n - β-Ga2O3 epitaxial layer, p-type epitaxial layer, anode electrode, characterized by:
[0022] A plurality of sequentially arranged thermoelectric cooling units are provided between the cathode electrode and the thermal interface layer, each thermoelectric cooling unit comprising a symmetrically distributed N-type thermoelectric material layer and a P-type thermoelectric material layer, and a patterned upper electrode layer and a lower electrode layer are provided on the upper and lower surfaces thereof, respectively;
[0023] An isolation layer is provided on one side from the upper surface of the upper electrode layer to the lower surface of the cathode electrode to achieve electrical isolation between the thermoelectric cooling unit and the cathode electrode;
[0024] The thermoelectric cooling units are wrapped with insulating filling materials at their peripheries to support the deposition and patterning of the lower electrode layer and to achieve electrical isolation between adjacent thermoelectric cooling units.
[0025] Preferably, the N-type thermoelectric material layer in the thermoelectric cooling unit is any one of Bi2Te3, Bi2(TeSe)3, PbTe or other N-type materials with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm;
[0026] The P-type thermoelectric material layer in the thermoelectric cooling unit is any one of Sb2Te3, (BiSb)2Te3, Bi2Te3 or other P-type materials with thermoelectric effect, and has a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm;
[0027] The spacing between the N-type thermoelectric material layer and the P-type thermoelectric material layer in the single thermoelectric refrigeration unit is 10-20 μm, and the spacing between two adjacent thermoelectric refrigeration units is 10-30 μm;
[0028] The patterned upper electrode layer and lower electrode layer are both made of Ni / Au, Au / Cu, Ni / Cu or other metals matching the thermoelectric material, and have a thickness of 240 to 2100 nm, and are used to connect each thermoelectric cooling unit in series, and apply voltage to form current, so that a temperature difference is formed between the upper and lower surfaces of the thermoelectric cooling unit, thereby improving the heat dissipation capacity of the device;
[0029] The isolation layer is made of SiO2 or Si3N4, and its thickness is 0.1-1 μm;
[0030] The insulating filling material is any one of SiO2, Si3N4 or photoresist, and its thickness is the sum of the thickness of the upper electrode layer and the thermoelectric cooling unit.
[0031] Technical solution 3:
[0032] A method for preparing a device according to technical solution 1, characterized in that it comprises the following steps:
[0033] S1) heterogeneously bonding the pre-prepared β-Ga2O3 wafer having a buffer layer and a channel layer to a substrate by high temperature annealing, thinning the β-Ga2O3 wafer by ion cutting, and smoothing the surface of the channel layer;
[0034] S2) epitaxially growing a dielectric layer on the channel layer, then depositing electrode metal by electron beam evaporation E-Beam, and performing ion implantation isolation;
[0035] S3) connecting the upper surface of the device after electrode deposition to an external carrier wafer through a bonding process;
[0036] S4) pre-processing the back side of the substrate by thinning the substrate and polishing the surface;
[0037] S5) depositing a substrate insulating layer and an upper metal electrode layer on the lower surface of the pretreated substrate by plasma enhanced chemical vapor deposition (PECVD) and electron beam evaporation (E-Beam);
[0038] S6) defining N-type thermoelectric material and P-type thermoelectric material deposition regions and depositing N-type thermoelectric material layers and P-type thermoelectric material layers on the upper metal electrode layer by photolithography and metal organic chemical vapor deposition (MOCVD) to form a thermoelectric cooling module;
[0039] S7) depositing an insulating support material on the periphery of the thermoelectric cooling module by plasma enhanced chemical vapor deposition (PECVD) or spin coating;
[0040] S8) depositing a metal electrode layer on the thermoelectric cooling module and the insulating support material by electron beam evaporation (E-Beam);
[0041] S9) Bonding the heat sink material to the surface of the lower metal electrode layer through the heat transfer interface material, and removing the carrier wafer to complete the device manufacturing.
[0042] Technical solution 4:
[0043] A method for preparing a device according to technical solution 2, characterized in that it comprises the following steps:
[0044] 1) For n + The upper surface of the β-Ga2O3 substrate was first cleaned by organic ultrasonic cleaning, and then epitaxially deposited by metal organic chemical vapor deposition (MOCVD) and magnetron sputtering. - β-Ga2O3 epitaxial layer and p-type epitaxial layer;
[0045] 2) In n + The cathode electrode is deposited on the back of the β-Ga2O3 substrate by electron beam evaporation E-beam, followed by rapid thermal annealing;
[0046] 3) Firstly, an anode electrode region is formed on the p-type epitaxial layer by photolithography, and then an anode electrode is deposited by electron beam evaporation (E-beam);
[0047] 4) Connecting the upper surface of the device on which the anode electrode deposition is completed to an external carrier wafer through a bonding process;
[0048] 5) Depositing an isolation layer and an upper electrode layer on the lower surface of the cathode electrode by plasma enhanced chemical vapor deposition (PECVD) and electron beam evaporation (E-Beam);
[0049] 6) defining N-type thermoelectric material and P-type thermoelectric material deposition regions and depositing N-type thermoelectric material layers and P-type thermoelectric material layers on the upper electrode layer by photolithography and metal organic chemical vapor deposition (MOCVD) to form a thermoelectric cooling unit;
[0050] 7) depositing insulating filling material on the periphery of the thermoelectric cooling unit by plasma enhanced chemical vapor deposition (PECVD) or spin coating;
[0051] 8) depositing a lower electrode layer on the thermoelectric cooling unit and the insulating filling material by electron beam evaporation E-Beam;
[0052] 9) Bonding the heat sink material to the surface of the lower electrode layer through the heat transfer interface material, and removing the carrier wafer to complete the device manufacturing.
[0053] Compared with the prior art, the present invention has the following advantages:
[0054] Firstly, the Ga2O3 device of technical solution 1 of the present invention has a thermoelectric cooling module between the substrate and the heat transfer interface layer, and voltage is applied through the upper and lower metal electrode layers on the upper and lower surfaces of the thermoelectric cooling module, thereby forming an electric current in the thermoelectric cooling module, so that the upper surface of the thermoelectric cooling module close to the substrate maintains a low temperature, accelerates the heat conduction of the substrate, and optimizes the heat dissipation capacity of the device; at the same time, since the thermoelectric cooling technology used only needs to apply voltage to the thermoelectric cooling module to form an electric current, the energy consumed for transporting the coolant compared with the microchannel cooling technology is reduced, thereby reducing energy loss; since a high thermal conductivity substrate SiC or AlN is used, the heat accumulation phenomenon of the device is greatly reduced, further improving the heat dissipation performance; in addition, since the heat dissipation structure of the device is optimized directly during device manufacturing, the cumbersome process and process damage of subsequent heat dissipation optimization of the device are avoided.
[0055] Secondly, the Ga2O3 device of technical solution 2 of the present invention has a thermoelectric cooling unit between the cathode electrode and the thermal interface layer, and voltage is applied through the upper and lower electrode layers on the upper and lower surfaces of the thermoelectric cooling unit, so that the thermoelectric material in the thermoelectric cooling unit can produce heat and thermoelectric effect, so that the temperature of the upper surface of the thermoelectric cooling unit decreases, thereby significantly improving the heat dissipation performance of the device; at the same time, the thermoelectric cooling technology used as an active cooling strategy can more effectively reduce the thermal resistance of the device, thereby achieving a better heat dissipation effect, and this solution also solves the problem of additional stress that may be generated when high thermal conductivity materials are in direct contact with Ga2O3 devices; in addition, by directly heterogeneously integrating the thermoelectric cooling unit on the device, not only the heat propagation path is shortened, but also the overall heat dissipation efficiency of the device is improved. This integration method also facilitates the miniaturization of the device, helps to reduce the size and weight of the device, and thus improves the reliability and stability of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a structural schematic diagram of a device of technical solution 1 of the present invention;
[0057] Figure 2 It is a structural schematic diagram of a device of technical solution 2 of the present invention;
[0058] Figure 3 It is a schematic diagram of the manufacturing process flow of the device of technical solution 1 of the present invention;
[0059] Figure 4 It is a schematic diagram of the manufacturing process flow of the device of technical solution 2 of the present invention;
[0060] Figure 5 It is a schematic diagram of the structure of a gallium oxide Schottky diode with a P-type diamond tilted mesa junction terminal in the patent document with application number CN202210192776.2;
[0061] Figure 6 It is a schematic diagram of the structure of a heterogeneous integrated gallium oxide field effect transistor with a microchannel in the patent document with application number CN202310474680.X. DETAILED DESCRIPTION
[0062] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.
[0063] Reference Figure 1 The Ga2O3 metal oxide semiconductor field effect transistor MOSFET with integrated thermoelectric material of the present invention comprises a heat sink layer 1, a heat transfer interface layer 2, a thermoelectric cooling module 3, a substrate insulating layer 41, a substrate 4, a buffer layer 5, a channel layer 6, a dielectric layer 7, and a source electrode S, a drain electrode D, and a gate electrode G, wherein:
[0064] The substrate 4 is made of SiC or AlN, and has a thickness of 100-400 μm.
[0065] The buffer layer 5 is made of β-Ga2O3 and has a thickness of 0.3-3 μm. It is located on the substrate 4 .
[0066] The channel layer 6 is made of β-Ga2O3 and has a thickness of 10-500 nm. It is located on the buffer layer 5 .
[0067] The dielectric layer 7 is made of Al2O3 or NiO or Al2O3 and Hf 0.5 Zr 0.5 O2, with a thickness of 20-100 nm, is located on the channel layer 6.
[0068] The source S and drain D are made of Ti / Au with a thickness of 20-60 / 60-300 nm, and are located on the channel layer 6 ; the gate G is made of Ni / Au with a thickness of 20-60 / 60-300 nm, and is located between the source S and drain D and on the dielectric layer 7 .
[0069] The substrate insulating layer 41 is made of SiO2 or Si3N4, has a thickness of 0.1-1 μm, and is located on the back side of the substrate 4 .
[0070] The adjacent thermoelectric cooling modules 3 are 10 to 30 μm apart, and each thermoelectric cooling module 3 includes an N-type thermoelectric material layer and a P-type thermoelectric material layer 10 to 20 μm apart. The N-type thermoelectric material layer adopts any one of Bi2Te3, Bi2(TeSe)3, PbTe or other N-type materials with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm. The P-type thermoelectric material layer adopts any one of Sb2Te3, (BiSb)2Te3, Bi2Te3 or other P-type materials with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm, and is located on the lower surface of the substrate insulating layer 41.
[0071] The upper and lower surfaces of the thermoelectric cooling module 3 are respectively provided with an upper metal electrode layer 31 and a lower metal electrode layer 32, both of which have a thickness of 240-2100 nm and are deposited by Ni / Au, Au / Cu, Ni / Cu or other metals matching the thermoelectric material.
[0072] The periphery of the thermoelectric cooling module 3 is filled with an insulating support material 33 , which is any one of SiO 2 , Si 3 N 4 or photoresist, and the thickness is the sum of the thickness of the upper metal electrode layer 31 and the thermoelectric cooling module 3 .
[0073] The heat transfer interface layer 2 is made of any one of silica gel, silicone grease or epoxy resin, has a thickness of 1 to 50 μm, and is located on the lower surface of the lower metal electrode layer.
[0074] The heat sink layer 1 is made of any one of copper alloy, aluminum alloy or high thermal conductivity ceramic material, with a thickness of 0.1-10 mm, and is located on the lower surface of the heat transfer interface layer.
[0075] Reference Figure 2 The invention discloses a highly heat dissipating vertical Ga2O3 heterojunction diode HJD with integrated thermoelectric materials, comprising a heat dissipation layer a, a thermal interface layer b, a thermoelectric cooling unit c, an isolation layer d, a cathode electrode e, and a + β-Ga2O3 substrate f, n - β-Ga2O3 epitaxial layer g, p-type epitaxial layer h, anode electrode i, where:
[0076] The + β-Ga2O3 substrate f, thickness is 300~500μm.
[0077] The - β-Ga2O3 epitaxial layer g, with a thickness of 5 to 30 μm, is located at n + On β-Ga2O3 substrate f.
[0078] The p-type epitaxial layer h is made of NiO and has a thickness of 300-600 nm. - On top of the β-Ga2O3 epitaxial layer g.
[0079] The anode electrode i is made of Ni / Au, with a thickness of 20-60 / 60-300 nm, and is located on the p-type epitaxial layer h.
[0080] The cathode electrode e is made of Ti / Au with a thickness of 20-60 / 60-300 nm. + Back side of β-Ga2O3 substrate f.
[0081] The isolation layer d is made of SiO2 or Si3N4, has a thickness of 0.1-1 μm, and is located on the back side of the cathode electrode e.
[0082] The adjacent thermoelectric cooling units c are 10 to 30 μm apart, and each thermoelectric cooling unit c includes an N-type thermoelectric material layer and a P-type thermoelectric material layer 10 to 20 μm apart. The N-type thermoelectric material layer adopts any one of Bi2Te3, Bi2(TeSe)3, PbTe or other N-type materials with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm. The P-type thermoelectric material layer adopts any one of Sb2Te3, (BiSb)2Te3, Bi2Te3 or other P-type materials with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm, and is located on the lower surface of the isolation layer d.
[0083] The upper and lower surfaces of the thermoelectric cooling unit c are respectively provided with an upper electrode layer c1 and a lower electrode layer c2, both of which have a thickness of 240-2100 nm and are deposited using Ni / Au, Au / Cu, Ni / Cu or other metals matching the thermoelectric material.
[0084] The periphery of the thermoelectric cooling unit c is filled with an insulating filling material c3, which is any one of SiO2, Si3N4 or photoresist, and the thickness is the sum of the thickness of the upper electrode layer c1 and the thermoelectric cooling unit c.
[0085] The thermal interface layer b is made of any one of silica gel, silicone grease or epoxy resin, has a thickness of 1 to 50 μm, and is located on the lower surface of the lower electrode layer.
[0086] The heat dissipation layer a is made of any one of copper alloy, aluminum alloy or high thermal conductivity ceramic material, with a thickness of 0.1-10 mm, and is located on the lower surface of the thermal interface layer.
[0087] Reference Figure 3 The present invention provides three embodiments of manufacturing a Ga2O3 metal oxide semiconductor field effect transistor MOSFET structure with integrated thermoelectric materials, but the embodiments of the present invention are not limited thereto. The experimental methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials described can be obtained from commercial sources unless otherwise specified.
[0088] In the first embodiment, a Ga2O3 metal oxide semiconductor field effect transistor MOSFET is manufactured in which the N-type thermoelectric material layer is Bi2Te3, the P-type thermoelectric material layer is Sb2Te3 with a thickness of 50nm, the dielectric layer is Al2O3 with a thickness of 20nm.
[0089] Step 1: heterogeneously bond the pre-prepared β-Ga2O3 wafer with the buffer layer 5 and the channel layer 6 to the substrate 4, thin the β-Ga2O3 wafer, and then smooth the channel layer 6, as shown in FIG. Figure 3 (a).
[0090] 1.1) A SiC substrate 4 with a thickness of 600 μm was selected and organic ultrasonic cleaning was performed with acetone, isopropanol, and deionized water in sequence. The cleaning time was 15 min, 10 min, and 5 min, respectively, and the ultrasonic power was 100 W. After the cleaning was completed, the surface of the SiC substrate 4 was blown dry with N2;
[0091] 1.2) A pre-prepared β-Ga2O3 wafer is selected, which includes a β-Ga2O3 buffer layer 5 with a thickness of 0.3 μm and an unintentionally doped β-Ga2O3 layer 5 with a thickness of 500 μm and a doping concentration of 1×10 18 cm -3 β-Ga2O3 channel layer 6, H ion implantation is performed on one side of the buffer layer 5 of the β-Ga2O3 wafer, aiming to form defects in the β-Ga2O3 wafer at 1 μm from the surface of the buffer layer 5;
[0092] 1.3) The front side of the SiC substrate 4 is bombarded with Ar ions for 2 minutes to form an amorphous layer, and then the front side of the SiC substrate 4 and one side of the β-Ga2O3 wafer buffer layer 5 are subjected to high-temperature annealing bonding in vacuum at a temperature of 860° C. for 30 seconds;
[0093] 1.4) placing the bonded wafers in a N2 environment and performing secondary annealing at 830°C for 20 min to remove the β-Ga2O3 wafer from the defects, leaving a buffer layer 5 with a thickness of 0.3 μm and a channel layer 6 with a thickness of 0.7 μm on the surface of the SiC substrate;
[0094] 1.5) The surface of the channel layer 6 is ground and polished by using chemical mechanical polishing (CMP) technology to reduce the thickness of the channel layer 6 to 50 nm.
[0095] Step 2: epitaxially grow a dielectric layer 7 on the channel layer 6, and then deposit source S, drain D and gate G metals on the channel layer 6 and the dielectric layer 7 respectively, and perform ion implantation to isolate the device, such as Figure 3 (b).
[0096] 2.1) using atomic layer deposition (ALD) technology, under process conditions of a reaction chamber temperature of 360° C. and a pressure of 1.5 mbar, depositing an Al2O3 dielectric layer 7 with a thickness of 20 nm on the channel layer 6;
[0097] 2.2) Photolithography is performed on the surface of the dielectric layer 7, that is, a layer of photoresist is first coated on the dielectric layer 7, and then alignment, exposure, development, and pattern detection are performed in sequence to form a device active area from the source S to the drain D;
[0098] 2.3) Using inductively coupled plasma etching (ICP) to etch the dielectric layer 7 outside the active area until the channel layer 6 is exposed, and then placing the wafer in a photoresist stripping solution to remove the photoresist;
[0099] 2.4) The surface of the channel layer 6 is photolithographically formed into source and drain regions, and the channel layer 6 in the source and drain regions is ion implanted to reduce the resistance of the source and drain regions. The doping element is Si, and the doping concentration is 1×10 19 cm -3 ;
[0100] 2.5) Through electron beam evaporation E-Beam, the vacuum in the working room is evacuated to 2.0×10 -4 Under the process conditions of 100 nm Pa, electron gun acceleration voltage of 6 Kv, electron gun beam current of 1 A, and evaporation time of 80 s, Ti / Au with a thickness of 20 / 60 nm is deposited in the source and drain regions as the source S and drain D, and then the wafer is placed in a photoresist stripping solution to remove the photoresist;
[0101] 2.6) The wafer after the metal deposition of the source S and the drain D is rapidly annealed in a N2 environment for 35 seconds at a temperature of 860° C. to form a good ohmic contact at the contact surface of the source, drain and channel layer 6;
[0102] 2.7) The surface of the dielectric layer 7 is again photolithographically formed into a gate region, and the vacuum is evacuated to 2.0×10 -4 Under the process conditions of 100 nm Pa, electron gun acceleration voltage of 6 Kv, electron gun beam current of 1 A, and evaporation time of 80 s, Ni / Au with a thickness of 20 / 60 nm is deposited on the gate region as the gate G, and then the wafer is placed in a photoresist stripping solution to remove the photoresist;
[0103] 2.8) Using ion implantation technology, the implantation energy is 360keV and the ion concentration is 1×10 14 cm -2 Under the process conditions, high-energy ions are implanted into the surface of the channel layer outside the active area of the wafer to complete device isolation.
[0104] Step 3: The upper surface of the device with electrode metal deposition completed is bonded to the external carrier wafer through bonding glue, and pressure is applied to bond them, such as Figure 3 (c).
[0105] Step 4: Pre-treat the back side of the SiC substrate 4, such as Figure 3 (d).
[0106] 4.1) The back side of the SiC substrate 4 of the device having the substrate 4, the buffer layer 5, the channel layer 6, the dielectric layer 7, the source electrode S, the drain electrode D, and the gate electrode G is thinned by grinding to reduce the thickness to 100 μm;
[0107] 4.2) The back side of the thinned SiC substrate 4 is finely processed by polishing technology to improve the smoothness and flatness of the wafer surface.
[0108] Step 5: Deposit a substrate insulating layer 41 and an upper metal electrode layer 31 on the back of the pre-treated substrate 4 in sequence, as shown in FIG. Figure 3 (e).
[0109] 5.1) Plasma enhanced chemical vapor deposition (PECVD) technology was used with flow rates of SiH4 and NH3 at 10 cm 3 / min、5cm 3 / min, temperature of 200°C, growth pressure of 100Pa, and RF power of 50W, depositing a Si3N4 substrate insulating layer 41 with a thickness of 0.1μm on the back side 4 of the SiC substrate;
[0110] 5.2) Photolithography is performed on the surface of the substrate insulating layer 41, that is, a layer of photoresist is first coated on the substrate insulating layer 41, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing the upper metal electrode;
[0111] 5.3) Through electron beam evaporation E-Beam, the vacuum in the working room is evacuated to 2.5×10 -4 Under the process conditions of 100 nm Au / Ni with a thickness of 200 / 60 nm is deposited in the area where the upper metal electrode is deposited as the upper metal electrode layer 31, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0112] Step 6: Deposit the thermoelectric cooling module 3 on the upper metal electrode layer 31, such as Figure 3 (f).
[0113] 6.1) Photolithography is performed on the surface of the upper metal electrode layer 31, that is, a layer of photoresist is first coated on the upper metal electrode layer 31, and then alignment, exposure, development, and pattern detection are performed in sequence to form multiple areas for depositing N-type thermoelectric materials, each area having a side length of 60 μm and a spacing of 80 μm;
[0114] 6.2) using metal organic chemical vapor deposition (MOCVD) technology, under the process conditions of a flow rate ratio of DipTe to TMBi of 5, a temperature of 350° C., and a growth pressure of 450 mbar, depositing a 50 nm thick N-type Bi2Te3 layer as an N-type thermoelectric material layer in the area where the N-type thermoelectric material is deposited, and then placing the wafer in a photoresist stripping solution to remove the photoresist;
[0115] 6.3) The surface of the upper metal electrode layer 31 is again photolithographically processed to form a plurality of regions for depositing P-type thermoelectric material, each region having a side length of 60 μm and a distance of 10 μm from the adjacent N-type thermoelectric material layer;
[0116] 6.4) Using metal organic chemical vapor deposition (MOCVD) technology, under the process conditions of a flow rate ratio of DipTe to TDSb of 2, a temperature of 300°C, and a growth pressure of 350 mbar, a P-type Sb2Te3 layer with a thickness of 50 nm is deposited as a P-type thermoelectric material layer in the area where the P-type thermoelectric material is deposited, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, thereby completing the production of the thermoelectric cooling module 3.
[0117] Step 7: Deposit insulating support material 33 on the periphery of the thermoelectric cooling module 3, such as Figure 3 (g).
[0118] 7.1) Photolithography is performed again on the surface of the substrate insulating layer 41, that is, a layer of photoresist is first coated on the substrate insulating layer 41, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing insulating support material;
[0119] 7.2) Plasma enhanced chemical vapor deposition (PECVD) technology was used with flow rates of SiH4 and NH3 at 30 cm 3 / min、20cm 3 / min, temperature of 400°C, growth pressure of 150Pa, and RF power of 500W, Si3N4 is deposited as insulating support material 33 in the area where the insulating support material is deposited until the height is flush with the thermoelectric cooling module, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0120] Step 8: Deposit a metal electrode layer 32 on the thermoelectric cooling module 3 and the insulating support material 33, such as Figure 3 (h).
[0121] 8.1) Photolithography is performed on the surfaces of the thermoelectric cooling module 3 and the insulating support material 33, that is, a layer of photoresist is first coated on the thermoelectric cooling module 3 and the insulating support material 33, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing a lower metal electrode layer;
[0122] 8.2) Through electron beam evaporation E-Beam, the vacuum in the working room is evacuated to 2.5×10 -4 Under the process conditions of 100 Pa, electron gun acceleration voltage of 8 Kv, electron gun beam current of 1 A, and evaporation time of 260 s, Ni / Au with a thickness of 60 / 200 nm is deposited in the area where the lower metal electrode is deposited as the lower metal electrode layer 32, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0123] Step 9: Bond the heat sink layer 1 to the surface of the lower metal electrode layer 32 through the heat transfer interface layer 2, and remove the carrier wafer, such as Figure 3 (i).
[0124] 9.1) Using a spin coating process, epoxy resin is dripped onto a copper-molybdenum alloy heat sink 1 with a thickness of 0.1 mm, and then the heat sink is rotated at a speed of 4000 r / s for 40 seconds to obtain an epoxy resin film with a thickness of 2 μm as a heat transfer interface layer 2, and the lower metal electrode layer surface 32 and the epoxy resin film are bonded, and then the epoxy resin film is placed in an oven at 80° C. to cure for 10 minutes to complete the heat sink connection;
[0125] 9.2) Use debonding glue to remove the carrier wafer temporarily bonded on the device surface to complete the device manufacturing.
[0126] In the second embodiment, a Ga2O3 metal oxide semiconductor field effect transistor MOSFET with a heterojunction is manufactured in which the N-type thermoelectric material layer is Bi2(TeSe)3, the P-type thermoelectric material layer is (BiSb)2Te3, the thickness is 50μm, and the dielectric layer is NiO, the thickness is 120nm.
[0127] Step 1: heterogeneously bond the pre-prepared β-Ga2O3 wafer with the buffer layer 5 and the channel layer 6 to the substrate, thin the β-Ga2O3 wafer, and then smooth the channel layer 6, such as Figure 3 (a).
[0128] An AlN substrate 4 with a thickness of 600 μm was selected for organic ultrasonic cleaning with acetone, isopropanol, and deionized water in sequence. The cleaning time was 15 min, 10 min, and 5 min, respectively, and the ultrasonic power was 100 W. After the cleaning was completed, the surface of the AlN substrate 4 was blown dry with N2;
[0129] A pre-prepared β-Ga2O3 wafer is selected, which includes a 1.5 μm thick, unintentionally doped β-Ga2O3 buffer layer 5 and a 500 μm thick, doping concentration of 5×10 17 cm -3 β-Ga2O3 channel layer 6, H ion implantation is performed on one side of the buffer layer 5 of the β-Ga2O3 wafer, aiming to form defects in the β-Ga2O3 wafer at 2.5 μm from the surface of the buffer layer 5;
[0130] The front side of the AlN substrate 4 is bombarded with Ar ions for 2 minutes to form an amorphous layer, and then the front side of the AlN substrate 4 and one side of the β-Ga2O3 wafer buffer layer 5 are bonded by high-temperature annealing in vacuum at a temperature of 800°C for 1 minute.
[0131] The bonded wafers were placed in a N2 environment and subjected to secondary annealing at 760°C for 40 min to remove the β-Ga2O3 wafer from the defects, leaving a buffer layer 5 with a thickness of 1.5 μm and a channel layer 6 with a thickness of 1 μm on the AlN substrate;
[0132] The surface of the channel layer 6 is ground and polished by using a chemical mechanical polishing (CMP) technique to reduce the thickness of the channel layer 6 to 250 nm.
[0133] Step 2: epitaxially grow a dielectric layer 7 on the channel layer 6, and then deposit source S, drain D and gate G metals on the channel layer 6 and the dielectric layer 7 respectively, and perform ion implantation to isolate the device, such as Figure 3 (b).
[0134] The vacuum degree of the deposition chamber was set to 6 × 10 -4 Pa, a growth pressure of 3 Pa, and a sputtering power of 25 W. By magnetron sputtering technology, a p-type NiO dielectric layer 7 with a thickness of 120 nm and a doping concentration of 2×10 18 cm -3 .
[0135] The surface of the dielectric layer 7 is photolithographically processed, that is, a layer of photoresist is first coated on the dielectric layer 7, and then alignment, exposure, development, and pattern detection are sequentially performed to form an active region from the source S to the drain D of the device;
[0136] The dielectric layer 7 outside the active area is etched using an inductively coupled plasma etching (ICP) technique until the channel layer 6 is exposed, and then the wafer is placed in a photoresist stripping solution to remove the photoresist;
[0137] The surface of the channel layer 6 is photolithographically formed into source and drain regions, and the channel layer in the source and drain regions is ion-implanted to reduce the resistance of the source and drain regions. The doping element is Si, and the doping concentration is 1×10 19 cm -3 ;
[0138] The vacuum degree of the working chamber was set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 0.5A, and the evaporation time is 240s. Through electron beam evaporation E-Beam, Ti / Au with a thickness of 40 / 200nm is deposited in the source and drain regions as the source S and drain D, and then the wafer is placed in a photoresist stripping solution to remove the photoresist;
[0139] The wafer after the metal deposition of the source S and the drain D is placed in an annealing furnace and rapidly annealed in a N2 environment for 40 seconds at a temperature of 830° C. to form ohmic contacts at the contact surfaces of the source, drain and channel layer 6;
[0140] The surface of the dielectric layer 7 is again photolithographically formed into a gate region, and the vacuum degree of the working chamber is set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 0.5A, and the evaporation time is 240s. By electron beam evaporation E-Beam, Ni / Au with a thickness of 40 / 200nm is deposited in the gate area as the gate G, and then the wafer is placed in a photoresist stripping solution to remove the photoresist;
[0141] The implantation energy was set to 340 keV and the ion concentration was set to 5×10 14 cm -2 Under the process conditions, high-energy ions are implanted into the surface of the channel layer 6 outside the active area of the wafer through ion implantation technology to complete device isolation.
[0142] Step 3: Paste the upper surface of the device with electrode metal deposition to the external carrier wafer through bonding glue, and apply pressure to bond it, such as Figure 3 (c).
[0143] Step 4: Pre-treat the back side of the AlN substrate 4, such as Figure 3 (d).
[0144] The back side of the AlN substrate 4 of the device having the substrate 4, the buffer layer 5, the channel layer 6, the dielectric layer 7, the source electrode S, the drain electrode D, and the gate electrode G is thinned by grinding to reduce the thickness to 200 μm;
[0145] The back side of the thinned AlN substrate 4 is finely processed by polishing technology to improve the smoothness and flatness of the wafer surface.
[0146] Step 5: Deposit a substrate insulating layer 41 and an upper metal electrode layer 31 on the back of the pre-treated substrate 4 in sequence, such as Figure 3 (e).
[0147] Set the flow rates of SiH4 and N2O to 60 cm 3 / min、180cm 3 / min, temperature of 270°C, growth pressure of 90Pa, and RF power of 80W, a SiO2 substrate insulating layer 41 with a thickness of 0.4μm is deposited on the back of the AlN substrate 4 by plasma enhanced chemical vapor deposition PECVD technology;
[0148] The surface of the substrate insulating layer 41 is photolithographically processed, that is, a layer of photoresist is firstly coated on the substrate insulating layer 41, and then alignment, exposure, development, and pattern detection are sequentially performed to form an area for depositing a metal electrode;
[0149] Set the working chamber to evacuate to 2.5 × 10 -4Under the process conditions of 9 kV Pa, electron gun acceleration voltage, electron gun beam current of 0.7 A and evaporation time of 880 s, Cu / Au with a thickness of 800 / 80 nm is deposited in the area where the upper metal electrode is deposited as the upper metal electrode layer 31 by electron beam evaporation E-Beam, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0150] Step 6: Deposit the thermoelectric cooling module 3 on the upper metal electrode layer 31, such as Figure 3 (f).
[0151] The surface of the upper metal electrode layer 31 is photolithographically processed, that is, a layer of photoresist is first coated on the upper metal electrode layer 31, and then alignment, exposure, development, and pattern detection are sequentially performed to form a plurality of regions for depositing N-type thermoelectric materials, each region having a side length of 120 μm and a spacing of 155 μm;
[0152] The process conditions are set such that the flow rate ratio of DipTe and TMBi is 8, the flow rate ratio of DipTe and DESe is 3, the temperature is 500°C, and the growth pressure is 460 mbar. By using the metal organic chemical vapor deposition MOCVD technology, a 50 μm thick N-type Bi2(TeSe)3 layer is deposited in the area where the N-type thermoelectric material is deposited as the N-type thermoelectric material layer, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0153] The surface of the upper metal electrode layer 31 is again photolithographically processed to form a plurality of regions for depositing P-type thermoelectric material, each region having a side length of 120 μm and a distance of 15 μm from an adjacent N-type thermoelectric material layer and a distance of 20 μm from an adjacent N-type thermoelectric material layer;
[0154] The process conditions are set as follows: the flow rate ratio of DipTe and TMBi is 5, the flow rate ratio of TMBi and TDSb is 3, the temperature is 380°C, and the growth pressure is 420 mbar. Through the metal organic chemical vapor deposition MOCVD technology, a 50 μm thick P-type (BiSb)2Te3 is deposited in the area where the P-type thermoelectric material is deposited as a P-type thermoelectric material layer. The wafer is then placed in a photoresist stripping solution to remove the photoresist, completing the production of the thermoelectric cooling module 3.
[0155] Step 7: Deposit insulating support material 33 on the periphery of the thermoelectric cooling module 3, such as Figure 3 (g).
[0156] The surface of the substrate insulating layer 41 is again subjected to photolithography, that is, a layer of photoresist is first coated on the substrate insulating layer 41, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing insulating support material;
[0157] Set the flow rates of SiH4 and N2O to 80 cm 3 / min、200cm 3 / min, temperature of 280°C, growth pressure of 100Pa, and RF power of 90W, by plasma enhanced chemical vapor deposition (PECVD) technology, SiO2 is deposited as insulating support material 33 in the area where the insulating support material is deposited until the height is flush with the thermoelectric cooling module, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0158] Step 8: Deposit a metal electrode layer 32 on the thermoelectric cooling module 3 and the insulating support material 33, such as Figure 3 (h).
[0159] Photolithography is performed on the surfaces of the thermoelectric cooling module 3 and the insulating support material 33, that is, a layer of photoresist is first coated on the thermoelectric cooling module 3 and the insulating support material 33, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing a lower metal electrode layer;
[0160] Set the working chamber to evacuate to 2.5 × 10 -4 Under the process conditions of Pa, electron gun acceleration voltage of 9Kv, electron gun beam current of 0.7A, and evaporation time of 880s, Au / Cu with a thickness of 80 / 800nm is deposited in the area where the lower metal electrode is deposited as the lower metal electrode layer 32 by electron beam evaporation E-Beam, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0161] Step 9: Bond the heat sink layer 1 to the surface of the lower metal electrode layer 32 through the heat transfer interface layer 2, and remove the carrier wafer, such as Figure 3 (i).
[0162] By using a spin coating process, a silicone rubber film with a thickness of 5 μm is obtained as a heat transfer interface layer 2 after dropping silicone rubber on an aluminum-magnesium-silicon alloy heat sink 1 with a thickness of 1 mm and rotating it at a speed of 3500 r / s for 35 seconds. The surface of the lower metal electrode layer 32 is bonded to the silicone rubber film, and then placed in an oven at 120° C. to cure the silicone rubber film for 15 minutes to complete the heat sink connection.
[0163] The debonding glue is used to remove the carrier wafer temporarily bonded on the device surface, thereby completing the device fabrication.
[0164] Example 3: In the thermoelectric cooling module, the N-type thermoelectric material layer is PbTe, the P-type thermoelectric material layer is Bi2Te3, the thickness is 500 μm, and the dielectric layer is Al2O3 and Hf 0.5 Zr 0.5 O2, Ga2O3 metal oxide semiconductor field effect transistor MOSFET with ferroelectric storage gate with thickness of 15nm and 30nm respectively.
[0165] Step A: heterogeneously bond the pre-prepared β-Ga2O3 wafer with the buffer layer 5 and the channel layer 6 to the substrate 4, thin the β-Ga2O3 wafer, and then smooth the channel layer 6, as shown in FIG. Figure 3 (a).
[0166] A1) Selecting a SiC substrate 4 with a thickness of 600 μm, sequentially using acetone, isopropanol, and deionized water for organic ultrasonic cleaning, the cleaning time is 15 min, 10 min, and 5 min, respectively, the ultrasonic power is 100 W, and after the cleaning is completed, the surface of the SiC substrate 4 is blown dry with N2;
[0167] A2) A pre-prepared β-Ga2O3 wafer is selected, which includes a 2 μm thick, unintentionally doped β-Ga2O3 buffer layer 5 and a 500 μm thick, doping concentration of 8×10 17 cm -3 β-Ga2O3 channel layer 6, H ion implantation is performed on one side of the buffer layer 5 of the β-Ga2O3 wafer, aiming to form defects in the β-Ga2O3 wafer at 3 μm from the surface of the buffer layer 5;
[0168] A3) Ar ion bombardment is performed on the front side of the SiC substrate 4 for 2 minutes to form an amorphous layer, and then the front side of the SiC substrate 4 and one side of the β-Ga2O3 wafer buffer layer 5 are bonded by high-temperature annealing in vacuum at a temperature of 760° C. for 2 minutes;
[0169] A4) The bonded wafers are placed in a N2 environment and subjected to secondary annealing at 680°C for 2 hours to remove the β-Ga2O3 wafer from the defects, leaving a buffer layer 5 with a thickness of 2 μm and a channel layer 6 with a thickness of 1 μm on the SiC substrate.
[0170] A5) using chemical mechanical polishing (CMP) technology to grind and polish the surface of the channel layer 6 to reduce the thickness of the channel layer 6 to 400 nm;
[0171] Step B: epitaxially grow a dielectric layer 7 on the channel layer 6, and then deposit source S, drain D and gate G metals on the channel layer 6 and the dielectric layer 7, respectively, and perform ion implantation to isolate the device, such as Figure 3 (b).
[0172] B1) Using atomic layer deposition ALD technology, Al2O3 with a thickness of 15nm and Hf with a thickness of 30nm are deposited on the channel layer 6 in sequence. 0.5 Zr 0.5 O2 is used as the dielectric layer 7, wherein the process conditions of atomic layer deposition ALD for depositing Al2O3 are as follows:
[0173] The reaction chamber temperature is 360°C.
[0174] The reaction chamber pressure is 2 mbar.
[0175] Deposition of Hf 0.5 Zr 0.5 The process conditions of atomic layer deposition ALD of O2 are as follows:
[0176] The reaction chamber temperature is 280°C.
[0177] The reaction chamber pressure is 3.2 mbar;
[0178] B2) performing photolithography on the surface of the dielectric layer 7, that is, first coating a layer of photoresist on the dielectric layer 7, and then sequentially performing alignment, exposure, development, and pattern detection to form an active region from the source S to the drain D of the device;
[0179] B3) using inductively coupled plasma etching (ICP) technology to etch the dielectric layer 7 outside the active area until the channel layer 6 is exposed, and then placing the wafer in a photoresist stripping solution to remove the photoresist;
[0180] B4) Photolithography is performed on the surface of the channel layer 6 to form source and drain regions, and ion implantation technology is used to dope the channel layer in the source and drain regions to reduce the resistance of the source and drain regions, wherein the process conditions of the ion implantation are as follows:
[0181] The doping element is Si,
[0182] The doping concentration is 1×10 19 cm -3 ;
[0183] B5) Using electron beam evaporation E-Beam, Ti / Au with a thickness of 60 / 300 nm is deposited in the source and drain regions as the source S and drain D, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of electron beam evaporation E-Beam are as follows:
[0184] The vacuum degree of the working chamber was set to 2.0×10 -4 Pa,
[0185] The electron gun acceleration voltage is 10Kv.
[0186] The electron gun beam current is 0.1A.
[0187] The evaporation time is 360s;
[0188] B6) placing the wafer after the metal deposition of the source S and the drain D into an annealing furnace, and rapidly annealing for 45 seconds in a N2 environment at a temperature of 800° C. to form ohmic contacts at the contact surfaces of the source, drain and channel layer 6;
[0189] B7) The surface of the dielectric layer 7 is again photolithographically formed into a gate region, and Ni / Au with a thickness of 60 / 300 nm is deposited in the gate region as a gate G by electron beam evaporation E-Beam, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of the electron beam evaporation E-Beam are as follows:
[0190] The vacuum degree of the working chamber was set to 2.0×10 -4 Pa,
[0191] The electron gun acceleration voltage is 10Kv.
[0192] The electron gun beam current is 0.1A.
[0193] The evaporation time is 360s;
[0194] B8) Set the implantation energy to 320 keV and the ion concentration to 8×10 14 cm -2 Under the process conditions, ion implantation technology is used to implant high-energy ions into the surface of the channel layer 6 outside the active area of the wafer to complete device isolation.
[0195] Step C: The upper surface of the device on which the electrode metal deposition is completed is bonded to the external carrier wafer through bonding glue, and pressure is applied to bond them, such as Figure 3 (c).
[0196] Step D: Pre-treat the back side of the SiC substrate 4, such as Figure 3 (d).
[0197] D1) grinding and thinning the back side of the SiC substrate 4 of the device having the substrate 4, the buffer layer 5, the channel layer 6, the dielectric layer 7, the source electrode S, the drain electrode D, and the gate electrode G, so that the thickness is reduced to 300 μm;
[0198] D2) Polishing technology is used to finely process the back side of the thinned SiC substrate 4 to improve the smoothness and flatness of the wafer surface.
[0199] Step E: Depositing a substrate insulating layer 41 and an upper metal electrode layer 31 on the back of the pre-treated substrate 4 in sequence, such as Figure 3 (e).
[0200] E1) Plasma enhanced chemical vapor deposition (PECVD) technology is used to deposit a SiO2 substrate insulating layer 41 with a thickness of 0.8 μm on the back side of the SiC substrate 4, wherein the process conditions of the plasma enhanced chemical vapor deposition (PECVD) are as follows:
[0201] The flow rates of SiH4 and N2O were 70 cm 3 / min、190cm 3 / min,
[0202] The temperature is 280℃,
[0203] The growth pressure is 90Pa.
[0204] The RF power is 90W;
[0205] E2) performing photolithography on the surface of the substrate insulating layer 41, that is, first coating a layer of photoresist on the substrate insulating layer 41, and then sequentially performing alignment, exposure, development, and pattern detection to form an area for depositing a metal electrode;
[0206] E3) Electron beam evaporation E-Beam is used to deposit Cu / Ni with a thickness of 2000 / 100 nm as the upper metal electrode layer 31 in the area where the upper metal electrode is deposited, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of electron beam evaporation E-Beam are as follows:
[0207] The working room was evacuated to 2.5×10 -4 Pa,
[0208] The electron gun acceleration voltage is 10Kv.
[0209] The electron gun beam current is 0.4A.
[0210] The evaporation time is 2100s.
[0211] Step F: Depositing the thermoelectric cooling module 3 on the upper metal electrode layer 31, such as Figure 3 (f).
[0212] F1) performing photolithography on the surface of the upper metal electrode layer 31, i.e., first coating a layer of photoresist on the upper metal electrode layer 31, and then sequentially performing alignment, exposure, development, and pattern detection to form a plurality of regions for depositing N-type thermoelectric materials, each region having a side length of 200 μm and a spacing of 250 μm;
[0213] F2) using metal organic chemical vapor deposition (MOCVD) technology, depositing N-type PbTe with a thickness of 500 μm as an N-type thermoelectric material layer in the area where the N-type thermoelectric material is deposited, and then placing the wafer in a photoresist stripping solution to remove the photoresist, wherein the process conditions of metal organic chemical vapor deposition (MOCVD) are as follows:
[0214] The flow rate ratio of DipTe and TEL is 3,
[0215] The temperature is 500℃,
[0216] The growth pressure is 450mbar;
[0217] F3) performing photolithography again on the surface of the upper metal electrode layer 31 to form a plurality of regions for depositing P-type thermoelectric material, each region having a side length of 200 μm and being 20 μm away from an adjacent N-type thermoelectric material layer and 30 μm away from an adjacent N-type thermoelectric material layer;
[0218] F4) Using metal organic chemical vapor deposition (MOCVD) technology, a 500 μm thick P-type Bi2Te3 layer is deposited as a P-type thermoelectric material layer in the area where the P-type thermoelectric material is deposited, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, thereby completing the production of the thermoelectric cooling module 3, wherein the process conditions of the metal organic chemical vapor deposition (MOCVD) are as follows:
[0219] The flow rate ratio of DipTe and TMBi is 8,
[0220] The temperature is 480℃,
[0221] The growth pressure is 560 mbar.
[0222] Step G: Deposit insulating support material 33 on the periphery of the thermoelectric cooling module 3, such as Figure 3 (g).
[0223] G1) The surface of the substrate insulating layer 41 is photolithographically processed, a layer of photoresist is first coated on the substrate insulating layer 41 by spin coating technology, and then alignment, exposure, development, and pattern detection are sequentially performed. In the area where the insulating support material needs to be deposited, the photoresist with a height flush with the thermoelectric cooling module is retained as the insulating support material 33, wherein the process conditions of the spin coating are as follows:
[0224] The speed is 2200r / s,
[0225] The spin coating time was 30 s;
[0226] G2) hard-baking the wafer on which the insulating support material is deposited so that the photoresist will not dissolve in the photoresist stripping solution or other etching solvents used subsequently, wherein the hard-baking process conditions are as follows:
[0227] The baking temperature is 280℃.
[0228] The baking time is 15 minutes.
[0229] Step H: depositing a metal electrode layer 32 on the thermoelectric cooling module 3 and the insulating support material 33, such as Figure 3 (h).
[0230] H1) performing photolithography on the surfaces of the thermoelectric cooling module 3 and the insulating support material 33, that is, first coating a layer of photoresist on the thermoelectric cooling module 3 and the insulating support material 33, and then sequentially performing alignment, exposure, development, and pattern detection to form an area for depositing a lower metal electrode layer;
[0231] H2) Depositing Ni / Cu with a thickness of 100 / 2000 nm as the lower metal electrode layer 32 in the area where the lower metal electrode is deposited by electron beam evaporation E-Beam, and then placing the wafer in a photoresist stripping solution to remove the photoresist, wherein the process conditions of electron beam evaporation E-Beam are as follows:
[0232] The working room was evacuated to 2.5×10 -4 Pa,
[0233] The electron gun acceleration voltage is 10Kv.
[0234] The electron gun beam current is 0.4A.
[0235] The evaporation time is 2100s.
[0236] Step I: Bond the heat sink layer 1 on the surface of the lower metal electrode layer through the heat transfer interface layer 2, and remove the carrier wafer, such as Figure 3 (i).
[0237] I1) using a spin coating process, dripping silicone grease on a SiC ceramic heat sink 1 with a thickness of 6 mm, and then rotating it at a speed of 1800 r / s for 50 seconds to obtain a silicone grease film with a thickness of 50 μm as a heat transfer interface layer 2, bonding the surface of the lower metal electrode layer 32 to the silicone grease film, and then putting it into an oven at 280° C. to cure the silicone grease film for 20 minutes to complete the heat sink connection;
[0238] I2) Use debonding glue to remove the carrier wafer temporarily bonded on the device surface to complete the device manufacturing.
[0239] Reference Figure 4 The present invention provides the following three embodiments for manufacturing a strong heat dissipation vertical Ga2O3 heterojunction diode HJD structure integrated with thermoelectric materials, but the embodiments of the present invention are not limited thereto.
[0240] Example 4: A vertical Ga2O3 heterojunction diode HJD with a thickness of 40 μm is manufactured in a thermoelectric cooling unit, wherein the N-type thermoelectric material layer is Bi2(TeSe)3, the P-type thermoelectric material layer is (BiSb)2Te3, and the thickness is 40 μm.
[0241] Operation 1: Clean the substrate f and then deposit n - β-Ga2O3 epitaxial layer g and p-type epitaxial layer h, such as Figure 4 (a).
[0242] 1-1) Select a thickness of 400 μm and a Si doping concentration of 2×10 18 cm -3 n +The β-Ga2O3 substrate f was cleaned with acetone, isopropanol, and deionized water in turn by organic ultrasonic cleaning. The cleaning time was 15 min, 10 min, and 5 min, respectively. The ultrasonic power was 80 W. After cleaning, the substrate surface was dried with N2.
[0243] 1-2) Metal organic chemical vapor deposition (MOCVD) technology was used, under the process conditions of O2 and TMGa flow rate ratio of 25, temperature of 620℃, and growth pressure of 60mbar. + The deposition thickness on the β-Ga2O3 substrate f is 15 μm, and the Si doping concentration is 2×10 16 cm -3 n - β-Ga2O3 epitaxial layer g.
[0244] 1-3) Using magnetron sputtering technology, the deposition chamber is evacuated to 6×10 -4 Pa, growth pressure of 2Pa, sputtering power of 25W, under the process conditions of n - The surface deposition thickness of β-Ga2O3 epitaxial layer g is 450nm and the doping concentration is 5×10 17 cm -3 p-NiO epitaxial layer h.
[0245] Operation 2: Make cathode electrode e, such as Figure 4 (b).
[0246] 2-1) Through electron beam evaporation E-beam, the vacuum in the working room is evacuated to 2.0×10 -4 Pa, electron gun acceleration voltage of 8Kv, electron gun beam current of 0.5A, evaporation time of 250s, under the process conditions of n + A Ti / Au cathode electrode e with a thickness of 50 / 200 nm is deposited on the back of the β-Ga2O3 substrate f;
[0247] 2-2) Place the wafer after cathode electrode deposition in an annealing furnace and perform rapid annealing in a N2 environment at a furnace temperature of 840°C for 35 seconds to form a bond between the cathode electrode and the n + The contact surface of the β-Ga2O3 substrate forms a good ohmic contact.
[0248] Operation 3: Make an anode electrode i, such as Figure 4 (c).
[0249] 3-1) performing photolithography on the surface of the p-NiO epitaxial layer h, that is, first coating a layer of photoresist on the p-NiO epitaxial layer, and then sequentially performing alignment, exposure, development, and pattern detection to form the device anode region;
[0250] 3-2) Through electron beam evaporation E-beam, the vacuum in the working room is evacuated to 2.0×10 -4 Under the process conditions of 300 Pa, electron gun acceleration voltage of 8 Kv, electron gun beam current of 0.5 A and evaporation time of 250 s, a Ni / Au anode electrode i with a thickness of 50 / 200 nm is deposited in the anode region to form a Schottky contact at the contact surface of the anode electrode and the p-NiO epitaxial layer, and finally the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0251] Operation 4: The upper surface of the device with electrode metal deposition completed is bonded to the external carrier wafer through bonding glue, and pressure is applied to bond them, such as Figure 4 (d).
[0252] Operation 5: Make the isolation layer d and the upper electrode layer c1, such as Figure 4 (e).
[0253] 5-1) Plasma enhanced chemical vapor deposition (PECVD) was used with SiH4 and NH3 flow rates of 25 cm 3 / min、15cm 3 / min, temperature of 320°C, growth pressure of 110Pa, and RF power of 360W, a Si3N4 isolation layer d with a thickness of 0.6μm is deposited on the back of the cathode electrode e;
[0254] 5-2) photolithography is performed on the surface of the isolation layer d, that is, a layer of photoresist is first coated on the isolation layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing the upper electrode;
[0255] 5-3) Through electron beam evaporation E-Beam, the vacuum degree in the working chamber is 2.5×10 -4 Under the process conditions of Pa, electron gun acceleration voltage of 9Kv, electron gun beam current of 0.7A, and evaporation time of 1000s, Cu / Ni with a thickness of 900 / 100nm is deposited in the area where the upper electrode is deposited as the upper electrode layer c1, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0256] Operation 6: Make a thermoelectric cooling unit c, such as Figure 4 (f).
[0257] 6-1) Photolithography is performed on the surface of the upper electrode layer c1, that is, a layer of photoresist is first coated on the upper metal electrode layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form multiple areas for depositing N-type thermoelectric materials, each area having a side length of 120 μm and a spacing of 155 μm;
[0258] 6-2) using metal organic chemical vapor deposition (MOCVD) technology, under the process conditions of a flow rate ratio of DipTe to TMBi of 4, a flow rate ratio of DipTe to DESe of 1, a temperature of 480° C., and a growth pressure of 420 mbar, depositing a 40 μm thick N-type Bi2(TeSe)3 layer as an N-type thermoelectric material layer in the area where the N-type thermoelectric material is deposited, and then placing the wafer in a photoresist stripping solution to remove the photoresist;
[0259] 6-3) The surface of the upper electrode layer c1 is again photolithographically processed to form a plurality of regions for depositing P-type thermoelectric material, each region having a side length of 120 μm and a distance of 15 μm from an adjacent N-type thermoelectric material layer and a distance of 20 μm from an adjacent N-type thermoelectric material layer;
[0260] 6-4) Using metal organic chemical vapor deposition (MOCVD) technology, under the process conditions of a flow rate ratio of DipTe to TMBi of 3, a flow rate ratio of TMBi to TDSb of 3, a temperature of 360°C, and a growth pressure of 420 mbar, a P-type (BiSb)2Te3 layer with a thickness of 40 μm was deposited in the area where the P-type thermoelectric material was deposited as a P-type thermoelectric material layer, and then the wafer was placed in a photoresist stripping solution to remove the photoresist, completing the production of the thermoelectric cooling unit c.
[0261] Operation 7: Depositing insulating filling material c3, such as Figure 4 (g).
[0262] 7-1) Photolithography is performed again on the surface of the isolation layer d, that is, a layer of photoresist is first coated on the isolation layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing insulating filling material;
[0263] 7-2) Using plasma enhanced chemical vapor deposition (PECVD) technology, the flow rates of SiH4 and NH3 were 30 cm 3 / min、20cm 3 / min, temperature of 400°C, growth pressure of 150Pa, and RF power of 500W, Si3N4 is deposited as insulating filling material c3 in the area where the insulating filling material is deposited until the height is flush with the thermoelectric cooling unit, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0264] Operation 8: Make the lower electrode layer c2, such as Figure 4 (h).
[0265] 8-1) Photolithography is performed on the surfaces of the thermoelectric cooling unit c and the insulating filling material c3, that is, a layer of photoresist is first coated on the thermoelectric cooling unit and the insulating filling material, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing the lower electrode layer;
[0266] 8-2) Through electron beam evaporation E-Beam, the vacuum degree in the working chamber is 2.5×10 -4 Under the process conditions of Pa, electron gun acceleration voltage of 9Kv, electron gun beam current of 0.7A, and evaporation time of 1000s, Ni / Cu with a thickness of 100 / 900nm is deposited in the area where the lower electrode layer is deposited as the lower electrode layer c2, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0267] Operation 9: Connect the heat dissipation layer a through the thermal interface layer b and remove the carrier wafer, such as Figure 4 (i).
[0268] 9-1) After dropping silica gel on the surface of the copper-tungsten alloy heat dissipation layer a, rotate it at a speed of 3200r / s for 35s to obtain a silica gel film with a thickness of 5μm as the thermal interface layer b, bond the surface of the lower electrode layer and the silica gel film, and then put it into an oven at 180℃ to cure the silica gel film for 15min to complete the heat dissipation layer connection;
[0269] 9-2) Use debonding glue to remove the carrier wafer temporarily bonded on the device surface, and finally complete the device production.
[0270] Example 5: A vertical Ga2O3 heterojunction diode with a thickness of 400 μm is manufactured in a thermoelectric cooling unit, in which the N-type thermoelectric material layer is PbTe, the P-type thermoelectric material layer is Bi2Te3, and the thickness is 400 μm.
[0271] §1: After cleaning the substrate f, deposit n - β-Ga2O3 epitaxial layer g and p-type epitaxial layer h, such as Figure 4 (a).
[0272] The thickness is 500 μm and the Sn doping concentration is 1×10 19 cm -3 n + β-Ga2O3 substrate f, cleaned with acetone, isopropanol, and deionized water for 15 min, 10 min, and 5 min, respectively, at 80 W organic ultrasonic power, and then dried with N2;
[0273] The process conditions were set at a flow rate ratio of O2 and TMGa of 40, a temperature of 700°C, and a growth pressure of 65 mbar. Metal organic chemical vapor deposition (MOCVD) technology was used. + The surface growth thickness of β-Ga2O3 substrate f is 30μm, and the Sn doping concentration is 1×10 17 cm -3 n - β-Ga2O3 epitaxial layer g;
[0274] The vacuum degree of the deposition chamber was set to 6 × 10 -4 Pa, growth pressure of 5Pa, sputtering power of 30W, magnetron sputtering technology was used, and the - The surface growth thickness of the β-Ga2O3 epitaxial layer g is 600nm and the doping concentration is 1×10 19 cm -3 p-NiO epitaxial layer h.
[0275] §2: Make cathode electrode e, such as Figure 4 (b).
[0276] The vacuum degree of the working chamber was set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 6Kv, the electron gun beam current is 1A, and the evaporation time is 360s. By electron beam evaporation E-beam, + A Ti / Au cathode electrode e with a thickness of 60 / 300 nm is deposited on the back of the β-Ga2O3 substrate f;
[0277] Then, the wafer after cathode electrode deposition is placed in an annealing furnace and rapidly annealed for 40 seconds in a N2 environment at 820°C to form a bond between the cathode electrode and n + The contact surface of the β-Ga2O3 substrate forms a good ohmic contact.
[0278] §3: Make the anode electrode i, such as Figure 4 (c).
[0279] The surface of the p-NiO epitaxial layer h is subjected to photolithography, that is, a layer of photoresist is first coated on the p-NiO epitaxial layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form the device anode region;
[0280] The vacuum degree of the working chamber was set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 6Kv, the electron gun beam current is 1A, and the evaporation time is 360s. By electron beam evaporation E-beam, a Ni / Au anode electrode i with a thickness of 60 / 300nm is deposited in the anode area to form a Schottky contact at the contact surface of the anode electrode and the p-NiO epitaxial layer, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0281] §4: The upper surface of the device with electrode metal deposition is bonded to the external carrier wafer through bonding glue, and pressure is applied to bond them, such as Figure 4 (d).
[0282] §5: Make the isolation layer d and the upper electrode layer c1, such as Figure 4 (e).
[0283] Set the flow rates of SiH4 and N2O to 80 cm3 / min、200cm 3 / min, temperature of 300°C, growth pressure of 100Pa, and RF power of 100W, a SiO2 isolation layer d with a thickness of 1μm is deposited on the back of the cathode electrode e by plasma enhanced chemical vapor deposition PECVD;
[0284] The surface of the isolation layer d is photolithographically processed, that is, a layer of photoresist is first coated on the isolation layer, and then alignment, exposure, development, and pattern detection are sequentially performed to form an area for depositing the upper electrode;
[0285] The vacuum degree of the working chamber was set to 2.5×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 1A, and the evaporation time is 2100s. Through electron beam evaporation E-Beam, Cu / Au with a thickness of 2000 / 100nm is deposited in the area where the upper electrode is deposited as the upper electrode layer c1, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0286] §6: Make a thermoelectric cooling unit c, such as Figure 4 (f).
[0287] The surface of the upper electrode layer c1 is photolithographically processed, that is, a layer of photoresist is first coated on the upper metal electrode layer, and then alignment, exposure, development, and pattern detection are sequentially performed to form multiple areas for depositing N-type thermoelectric materials, each area having a side length of 200 μm and a spacing of 250 μm;
[0288] The process conditions of setting the flow rate ratio of DipTe and TEL to 3, the temperature to 500°C, and the growth pressure to 450 mbar, using metal organic chemical vapor deposition MOCVD technology, depositing N-type PbTe with a thickness of 400 μm as the N-type thermoelectric material layer in the area where the N-type thermoelectric material is deposited, and then placing the wafer in a photoresist stripping solution to remove the photoresist;
[0289] The surface of the upper electrode layer c1 is again photolithographically processed to form a plurality of regions for depositing P-type thermoelectric material, each region having a side length of 200 μm and a distance of 20 μm from an adjacent N-type thermoelectric material layer and a distance of 30 μm from an adjacent N-type thermoelectric material layer;
[0290] The process conditions are set at a flow rate ratio of DipTe and TMBi of 10, a temperature of 500°C, and a growth pressure of 600 mbar. Through the metal organic chemical vapor deposition (MOCVD) technology, a 400 μm thick P-type Bi2Te3 is deposited as a P-type thermoelectric material layer in the area where the P-type thermoelectric material is deposited. The wafer is then placed in a photoresist stripping solution to remove the photoresist, completing the production of the thermoelectric cooling unit c.
[0291] §7: Deposit insulating filling material c3, such as Figure 4 (g).
[0292] The process conditions of the rotation speed of 2500r / s and the spin coating time of 40s are set, and the surface of the isolation layer d is photolithographically processed. A layer of photoresist is first coated on the isolation layer by spin coating technology, and then alignment, exposure, development, and pattern detection are sequentially performed. In the area where the insulating filling material needs to be deposited, the photoresist with a height flush with the thermoelectric cooling unit is retained as the insulating filling material c3;
[0293] The baking temperature was set to 260° C. and the baking time was set to 8 min. The wafer on which the insulating filling material was deposited was hard-baked to prevent the photoresist from being dissolved in the photoresist stripping solution or other etching solvents used subsequently.
[0294] §8: Make the lower electrode layer c2, such as Figure 4 (h).
[0295] Photolithography is performed on the surfaces of the thermoelectric cooling unit c and the insulating filling material c3, that is, a layer of photoresist is first coated on the thermoelectric cooling unit and the insulating filling material, and then alignment, exposure, development, and pattern detection are performed in sequence to form an area for depositing the lower electrode layer;
[0296] The vacuum degree of the working chamber was set to 2.5×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 1A, and the evaporation time is 2100s. Through electron beam evaporation E-Beam, Au / Cu with a thickness of 100 / 2100nm is deposited in the area where the lower electrode layer is deposited as the lower electrode layer c2, and then the wafer is placed in a photoresist stripping solution to remove the photoresist.
[0297] §9: Connect the heat dissipation layer a through the thermal interface layer b and remove the carrier wafer, such as Figure 4 (i).
[0298] After dripping silicone grease on the surface of the aluminum-silicon-carbon alloy heat dissipation layer a, the layer was rotated at a speed of 2200 r / s for 40 seconds to obtain a silicone grease film with a thickness of 10 μm as the thermal interface layer b. The surface of the lower electrode layer and the silicone grease film were bonded, and then placed in an oven at 220° C. to cure the silicone grease film for 15 minutes to complete the heat dissipation layer connection;
[0299] Use debonding glue to remove the carrier wafer temporarily bonded on the device surface to complete device fabrication.
[0300] Example 6: A vertical Ga2O3 heterojunction diode with a thickness of 50 nm is manufactured in a thermoelectric cooling unit, in which the N-type thermoelectric material layer is Bi2Te3, the P-type thermoelectric material layer is Sb2Te3, and the thickness is 50 nm.
[0301] Step 1: Clean the substrate f and then deposit n- β-Ga2O3 epitaxial layer g and p-type epitaxial layer h, such as Figure 4 (a).
[0302] A-1) The thickness is 300 μm and the Si doping concentration is 5×10 17 cm -3 n + β-Ga2O3 substrate f, organic ultrasonic cleaning was carried out with acetone, isopropanol and deionized water in sequence, the cleaning time was 15min, 10min and 5min respectively, the ultrasonic power was 80W, and after the cleaning was completed, the substrate surface was blown dry with N2;
[0303] A-2) Using metal organic chemical vapor deposition MOCVD technology, in n + The deposition thickness on the β-Ga2O3 substrate f is 5 μm, and the Sn doping concentration is 5×10 15 cm -3 n - β-Ga2O3 epitaxial layer g, wherein the process conditions of metal organic chemical vapor deposition MOCVD are as follows:
[0304] The flow rate ratio of O2 and TMGa is 10,
[0305] The temperature is 550℃,
[0306] The growth pressure is 55mbar;
[0307] A-3) Using magnetron sputtering technology, - The surface growth thickness of the β-Ga2O3 epitaxial layer g is 300nm and the doping concentration is 1×10 16 cm -3 The p-NiO epitaxial layer h, wherein the process conditions of magnetron sputtering are as follows:
[0308] The vacuum degree of the deposition chamber is 6×10 -4 Pa,
[0309] The growth pressure is 1Pa,
[0310] The sputtering power is 20W.
[0311] Step 2: Make the cathode electrode e, such as Figure 4 (b).
[0312] B-1) Using electron beam evaporation E-beam, + A Ti / Au cathode electrode e with a thickness of 20 / 60 nm is deposited on the back of the β-Ga2O3 substrate f, wherein the process conditions of the electron beam evaporation E-beam are as follows:
[0313] The vacuum degree of the working chamber is 2.0×10-4 Pa,
[0314] The electron gun acceleration voltage is 10Kv.
[0315] The electron gun beam current is 0.1A.
[0316] The evaporation time is 80s;
[0317] B-2) Place the wafer after cathode electrode deposition in an annealing furnace, set the furnace temperature to 860°C in a N2 environment, and perform annealing for 30 seconds to form a gap between the cathode electrode and the n + The contact surface of the β-Ga2O3 substrate forms a good ohmic contact.
[0318] Step 3: Make the anode electrode i, such as Figure 4 (c).
[0319] C-1) first coating a layer of photoresist on the p-NiO epitaxial layer h, and then sequentially performing alignment, exposure, development, and pattern detection to photoetch out the device anode region on the surface of the p-NiO epitaxial layer;
[0320] C-2) using electron beam evaporation E-Beam to deposit a Ni / Au anode electrode I with a thickness of 20 / 60 nm in the anode region to form a Schottky contact, wherein the process conditions of the electron beam evaporation E-Beam are as follows:
[0321] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0322] The electron gun acceleration voltage is 10Kv.
[0323] The electron gun beam current is 0.1A.
[0324] The evaporation time is 80s;
[0325] C-3) placing the wafer with the anode electrode deposited thereon into a photoresist stripping solution to remove the photoresist.
[0326] Step 4: Paste the upper surface of the device with electrode metal deposition to the external carrier wafer through bonding glue, and apply pressure to it for bonding, such as Figure 4 (d).
[0327] Step 5: Make the isolation layer d and the upper electrode layer c1, such as Figure 4 (e).
[0328] D-1) Plasma enhanced chemical vapor deposition (PECVD) is used to deposit a Si3N4 isolation layer d with a thickness of 0.1 μm on the back of the cathode electrode e, wherein the process conditions of the plasma enhanced chemical vapor deposition (PECVD) are as follows:
[0329] The flow rates of SiH4 and NH3 were 10 cm 3 / min、5cm 3 / min,
[0330] The temperature is 200°C,
[0331] The growth pressure is 100Pa.
[0332] The RF power is 50W;
[0333] D-2) performing photolithography on the surface of the isolation layer d, that is, first coating a layer of photoresist on the isolation layer, and then sequentially performing alignment, exposure, development, and pattern detection to form an area for depositing the upper electrode;
[0334] D-3) Electron beam evaporation E-Beam is used to deposit Ni / Au with a thickness of 200 / 40 nm as the upper electrode layer c1 in the area where the upper electrode is deposited, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of electron beam evaporation E-Beam are as follows:
[0335] The working room was evacuated to 2.5×10 -4 Pa,
[0336] The electron gun acceleration voltage is 8Kv.
[0337] The electron gun beam current is 0.9A.
[0338] The evaporation time is 240s.
[0339] Step 6: Make a thermoelectric cooling unit c, such as Figure 4 (f).
[0340] E-1) performing photolithography on the surface of the upper electrode layer c1, i.e., first coating a layer of photoresist on the upper electrode layer, and then sequentially performing alignment, exposure, development, and pattern detection to form a plurality of regions for depositing N-type thermoelectric materials, each region having a side length of 60 μm and a spacing of 80 μm;
[0341] E-2) Using metal organic chemical vapor deposition (MOCVD) technology, a 50 nm thick N-type Bi2Te3 layer is deposited as an N-type thermoelectric material layer in the area where the N-type thermoelectric material is deposited, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the metal organic chemical vapor deposition (MOCVD) process conditions are as follows:
[0342] The flow rate ratio of DipTe and TMBi is 6,
[0343] The temperature is 260℃,
[0344] The growth pressure is 380mbar;
[0345] E-3) performing photolithography again on the surface of the upper electrode layer c1 to form a plurality of regions for depositing P-type thermoelectric material, each region having a side length of 60 μm and being 10 μm away from an adjacent N-type thermoelectric material layer;
[0346] E-4) Using metal organic chemical vapor deposition MOCVD technology, a P-type Sb2Te3 layer with a thickness of 50nm is deposited as a P-type thermoelectric material layer in the area where the P-type thermoelectric material is deposited, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, thereby completing the production of the thermoelectric cooling unit c, wherein the process conditions of the metal organic chemical vapor deposition MOCVD are as follows:
[0347] The flow rate ratio of DipTe to TDSb is 1,
[0348] The temperature is 320℃,
[0349] The growth pressure is 360 mbar.
[0350] Step 7: Deposit insulating filling material c3, such as Figure 4 (g).
[0351] F-1) performing photolithography again on the surface of the isolation layer d, that is, first coating a layer of photoresist on the isolation layer, and then sequentially performing alignment, exposure, development, and pattern detection to form an area for depositing insulating filling material;
[0352] F-2) Plasma enhanced chemical vapor deposition (PECVD) technology is used to deposit Si3N4 as the insulating filling material c3 in the area where the insulating filling material is deposited until the height is flush with the thermoelectric cooling unit, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of the plasma enhanced chemical vapor deposition (PECVD) technology are as follows:
[0353] The flow rates of SiH4 and NH3 were 25 cm 3 / min、15cm 3 / min,
[0354] The temperature is 380℃,
[0355] The growth pressure is 120Pa.
[0356] The RF power is 460W.
[0357] Step 8: Make the lower electrode layer c2, such as Figure 4 (h).
[0358] G-1) performing photolithography on the surfaces of the thermoelectric cooling unit c and the insulating filling material c3, i.e., first coating a layer of photoresist on the thermoelectric cooling unit and the insulating filling material, and then sequentially performing alignment, exposure, development, and pattern detection to form an area for depositing the lower electrode layer;
[0359] G-2) Using electron beam evaporation E-Beam, Au / Ni with a thickness of 40 / 200 nm is deposited in the area where the lower electrode is deposited as the upper electrode layer c2, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of electron beam evaporation E-Beam are as follows:
[0360] The working room was evacuated to 2.5×10 -4 Pa,
[0361] The electron gun acceleration voltage is 8Kv.
[0362] The electron gun beam current is 0.9A.
[0363] The evaporation time is 240s.
[0364] Step 9: Connect the heat dissipation layer a through the thermal interface layer b and remove the carrier wafer, such as Figure 4 (i).
[0365] H-1) dripping epoxy resin on the surface of the copper-molybdenum alloy heat dissipation layer a and rotating it at a speed of 4000 r / s for 30 seconds to obtain an epoxy resin film with a thickness of 1 μm as a thermal interface layer b, bonding the surface of the lower electrode layer and the epoxy resin film, and then placing it in an oven at 100° C. to cure the epoxy resin film for 5 minutes to complete the heat dissipation layer connection;
[0366] H-2) Use debonding glue to remove the carrier wafer temporarily bonded on the device surface to complete the final device production.
[0367] The above descriptions are only six specific examples of the present invention, and do not constitute any limitation to the present invention. Obviously, for professionals in this field, after understanding the content and principle of the present invention, various modifications and changes in form and details may be made without deviating from the principle and result of the present invention. For example, in addition to copper alloy and aluminum alloy, SiC ceramics can also use AlN ceramics for heat sink layer and heat dissipation layer; in addition to Bi2Te3 / Sb2Te3, Bi2(TeSe)3 / (BiSb)2Te3, PbTe / Bi2Te3, thermoelectric cooling module and thermoelectric cooling unit can also use other materials with thermoelectric effect; in addition to Au / Cu, Ni / Cu, Ni / Au, upper and lower metal electrode layers can also use other metals that match thermoelectric materials, but these modifications and changes based on the idea of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A strong heat dissipation Ga integrated with thermoelectric materials 2 O 3 A metal oxide semiconductor field effect transistor MOSFET comprises, from bottom to top: a heat sink layer (1), a heat transfer interface layer (2), a substrate (4), a buffer layer (5), a channel layer (6), a dielectric layer (7) and metal electrodes located on the channel layer and the dielectric layer. Features: A plurality of sequentially arranged thermoelectric cooling modules (3) are provided between the substrate (1) and the heat transfer interface layer (2), each thermoelectric cooling module comprising a symmetrical N-type thermoelectric material layer and a P-type thermoelectric material layer, and a patterned upper metal electrode layer (31) and a lower metal electrode layer (32) are provided on the upper and lower surfaces thereof, respectively; A substrate insulating layer (41) is provided between the upper surface of the upper metal electrode layer (31) and the lower surface of the substrate (4) to achieve electrical isolation between the thermoelectric cooling module and the substrate; Each of the thermoelectric cooling modules (3) is wrapped with an insulating support material (33) on its periphery to support the deposition and patterning of the lower metal electrode layer and to achieve mutual isolation between each of the thermoelectric cooling modules.
2. The device according to claim 1, Features: The N-type thermoelectric material layer and the P-type thermoelectric material layer in each thermoelectric cooling module (3) are symmetrically distributed at a spacing of 10 μm to 20 μm, and two adjacent thermoelectric cooling modules are distributed at an equal spacing of 10 μm to 30 μm.
3. The device according to claim 1, Features: The N-type thermoelectric material layer in the thermoelectric cooling module (3) is made of Bi 2 Te 3 、Bi 2 (TeSe) 3 , PbTe or any other N-type material with thermoelectric effect, with a thickness of 0.03μm to 3000μm and a side length of 60μm to 200μm; The P-type thermoelectric material layer in the thermoelectric cooling module (3) is made of Sb 2 Te 3 、(BiSb) 2 Te 3 、Bi 2 Te 3 Or any other P-type material with thermoelectric effect, its thickness and side length are the same as those of the N-type thermoelectric material layer.
4. The device according to claim 1, Features: The patterned upper metal electrode layer (31) and the lower metal electrode layer (32) are both made of Ni / Au, Au / Cu, Ni / Cu or other metals matching the thermoelectric material, and have a thickness of 240 to 2100 nm. They are connected in series with each thermoelectric cooling module so that a voltage is applied thereto to form a current, thereby forming a temperature difference between the upper and lower surfaces of the thermoelectric cooling module and improving the heat dissipation capacity of the device. The substrate insulating layer (41) is made of SiO 2 or Si 3 N 4 , the thickness is 0.1μm~1μm; The insulating support material (33) is made of SiO 2 、Si 3 N 4 Or any one of the photoresists, the thickness of which is the sum of the thickness of the upper metal electrode layer and the thermoelectric cooling module.
5. The device according to claim 1, Features: The heat transfer interface layer (2) is made of any one of silica gel, silicone grease or epoxy resin, and has a thickness of 1 to 50 μm; The heat sink layer (1) is made of any one of copper alloy, aluminum alloy or high thermal conductivity ceramic material, and has a thickness of 0.1 to 10 mm. The copper alloy includes copper-tungsten alloy and copper-molybdenum alloy. The aluminum alloy includes aluminum-magnesium-silicon alloy and aluminum-silicon-carbon alloy. The high thermal conductivity ceramic material includes SiC ceramic and AlN ceramic.
6. The device according to claim 1, Features: The substrate (4) is made of SiC or AlN and has a thickness of 100 to 400 μm; The buffer layer (5) is made of β-Ga 2 O 3 , its thickness is 0.3~3μm; The channel layer (6) is made of β-Ga 2 O 3 , its thickness is 10~500nm; The dielectric layer (7) is made of Al 2 O 3 or NiO or Al 2 O 3 and Hf 0.5 Zr 0.5 O 2 , and its thickness is 20 to 100 nm.
7. A strong heat dissipation vertical Ga integrated with thermoelectric materials 2 O 3 Heterojunction diode HJD, from bottom to top: heat dissipation layer (a), thermal interface layer (b), cathode electrode (e), n + β-Ga 2 O 3 Substrate (f), n - β-Ga 2 O 3 Epitaxial layer (g), p-type epitaxial layer (h), anode electrode (i), Features: A plurality of sequentially arranged thermoelectric cooling units (c) are provided between the cathode electrode (e) and the thermal interface layer (b), each thermoelectric cooling unit comprising a symmetrically distributed N-type thermoelectric material layer and a P-type thermoelectric material layer, and a patterned upper electrode layer (c1) and a lower electrode layer (c2) are provided on the upper and lower surfaces thereof, respectively; An isolation layer (d) is provided between the upper surface of the upper electrode layer (c1) and the lower surface of the cathode electrode (e) to achieve electrical isolation between the thermoelectric cooling unit (c) and the cathode electrode (e); The periphery of each thermoelectric cooling unit (c) is wrapped with an insulating filling material (c3) to support the deposition and patterning of the lower electrode layer (c2) and to achieve electrical isolation between each thermoelectric cooling unit (c).
8. The device according to claim 7, Features: The N-type thermoelectric material layer in the thermoelectric cooling unit (c) is made of Bi 2 Te 3 、Bi 2 (TeSe) 3 , PbTe or any other N-type material with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm; The P-type thermoelectric material layer in the thermoelectric cooling unit (c) is made of Sb 2 Te 3 、(BiSb) 2 Te 3 、Bi 2 Te 3 Or any one of other P-type materials with thermoelectric effect, with a thickness of 0.03 to 3000 μm and a side length of 60 to 200 μm; The spacing between the N-type thermoelectric material layer and the P-type thermoelectric material layer in the single thermoelectric cooling unit (c) is 10 to 20 μm, and the spacing between two adjacent thermoelectric cooling units is 10 to 30 μm; The patterned upper electrode layer (c1) and lower electrode layer (c2) are both made of Ni / Au, Au / Cu, Ni / Cu or other metals matching the thermoelectric material, and have a thickness of 240 to 2100 nm, and are used to connect each thermoelectric cooling unit in series, and apply voltage to form current, so that a temperature difference is formed between the upper and lower surfaces of the thermoelectric cooling unit, thereby improving the heat dissipation capacity of the device; The isolation layer (d) is made of SiO 2 or Si 3 N 4 , its thickness is 0.1~1μm; The insulating filling material (c3) is SiO 2 、Si 3 N 4 Or any one of the photoresists, the thickness of which is the sum of the thickness of the upper electrode layer and the thermoelectric cooling unit.
9. The device according to claim 7, Features: The thermal interface layer (b) is made of any one of silica gel, silicone grease or epoxy resin, and has a thickness of 1 to 50 μm; The heat dissipation layer (a) is made of any one of copper alloy, aluminum alloy or high thermal conductivity ceramic material, and its thickness is 0.1 to 10 mm, wherein the copper alloy includes copper-tungsten alloy and copper-molybdenum alloy, the aluminum alloy includes aluminum-magnesium-silicon alloy and aluminum-silicon-carbon alloy, and the high thermal conductivity ceramic material includes SiC ceramic and AlN ceramic.
10. The device according to claim 7, Features: The + β-Ga 2 O 3 Substrate (f), with a thickness of 300-500 μm, doped with Si or Sn at a doping concentration of 5×10 17 ~1×10 19 cm -3 ; The - β-Ga 2 O 3 The epitaxial layer (g) has a thickness of 5 to 30 μm, and is doped with Si or Sn at a doping concentration of 5×10 15 ~1×10 17 cm -3 ; The p-type epitaxial layer (h) is made of NiO, has a thickness of 300-600 nm, is doped with B, and has a doping concentration of 1×10 16 ~1×10 19 cm -3 .
11. A method for preparing the field effect transistor of claim 1, It is characterized in that The following steps are involved: S1) high temperature annealing is used to prepare the β-Ga with buffer layer and channel layer 2 O 3 The wafer is heterogeneously bonded to the substrate and the β-Ga is thinned by ion cutting. 2 O 3 Wafer, smoothing the surface of the channel layer; S2) epitaxially growing a dielectric layer on the channel layer, then depositing electrode metal by electron beam evaporation E-Beam, and performing ion implantation isolation; S3) connecting the upper surface of the electrode deposition sample to an external carrier wafer through a bonding process; S4) pre-processing the back side of the substrate by thinning the substrate and polishing the surface; S5) depositing a substrate insulating layer and an upper metal electrode layer on the lower surface of the pretreated substrate by plasma enhanced chemical vapor deposition (PECVD) and electron beam evaporation (E-Beam); S6) defining N-type thermoelectric material and P-type thermoelectric material deposition regions and depositing N-type thermoelectric material layers and P-type thermoelectric material layers on the upper metal electrode layer by photolithography and metal organic chemical vapor deposition (MOCVD) to form a thermoelectric cooling module; S7) depositing an insulating support material on the periphery of the thermoelectric cooling module by plasma enhanced chemical vapor deposition (PECVD) or spin coating; S8) depositing a metal electrode layer on the thermoelectric cooling module and the insulating support material by electron beam evaporation (E-Beam); S9) Bonding the heat sink material to the surface of the lower metal electrode layer through the heat transfer interface material, and removing the carrier wafer to complete the device manufacturing.
12. The method according to claim 11, Features: The process conditions of the electron beam evaporation E-Beam in step S2) are as follows: The working room is evacuated to 2.0×10 -4 Pa, the electron gun acceleration voltage is 6-10Kv, the electron gun beam current is 0.1-1A, and the evaporation time is 80-360s; The process conditions of the electron beam evaporation E-Beam in step S5) are as follows: The working room was evacuated to 2.5×10 -4 Pa, the electron gun acceleration voltage is 8-10Kv, the electron gun beam current is 0.4-1A, and the evaporation time is 240-2100s; In the step S5), the plasma enhanced chemical vapor deposition PECVD process conditions are as follows: Deposition of SiO 2 SiH 4 and N 2 O is the precursor gas, and the flow rate is maintained at 50-80 cm 3 / min, 160~200cm 3 / min, the temperature was maintained at 250-300°C, the growth pressure was maintained at 80-100Pa, and the RF power was set to 60-100W; Deposition of Si 3 N 4 SiH 4 and NH 3 The precursor gas is maintained at a flow rate of 10 to 30 cm 3 / min, 5~20cm 3 / min, the temperature is maintained at 200-400°C, the growth pressure is maintained at 100-150Pa, and the RF power is set to 50-500W; The process conditions of the metal organic chemical vapor deposition MOCVD in step S6 are as follows: TMBi was used as a precursor of Bi, TDSb as a precursor of Sb, DipTe as a precursor of Te, TEL as a precursor of Pb, DESe as a precursor of Se, and high-purity H 2 As carrier gas; Deposition Bi 2 Te 3 The flow rate ratio of DipTe and TMBi is 2-10, the temperature is maintained at 200-500°C, and the growth pressure is maintained at 300-600 mbar; Deposition Sb 2 Te 3 The flow rate ratio of DipTe and TDSb is 1 to 6, the temperature is maintained at 250 to 450 °C, and the growth pressure is maintained at 200 to 500 mbar; The flow rate ratio of DipTe and TEL for depositing PbTe is 1 to 3, the temperature is maintained at 300 to 500 °C, and the growth pressure is maintained at 200 to 450 mbar; Deposition Bi 2 (TeSe) 3 The flow rate ratio of DipTe and TMBi is 1 to 8, the flow rate ratio of DipTe and DESe is 1 to 3, the temperature is maintained at 220 to 600 °C, and the growth pressure is maintained at 200 to 600 mbar; Deposition (BiSb) 2 Te 3 The flow rate ratio of DipTe and TMBi is 1 to 5, the flow rate ratio of TMBi and TDSb is 2 to 4, the temperature is maintained at 200 to 550° C., and the growth pressure is maintained at 300 to 500 mbar.
13. A method for preparing the Ga as claimed in claim 7 2 O 3 The two-stage method It is characterized in that The following steps are involved: 1) For n + β-Ga 2 O 3 The substrate surface is first cleaned by organic ultrasonic cleaning, and then epitaxially deposited by metal organic chemical vapor deposition (MOCVD) and magnetron sputtering. - β-Ga 2 O 3 epitaxial layer and p-type epitaxial layer; 2) In n + β-Ga 2 O 3 The cathode electrode is deposited on the back of the substrate by electron beam evaporation E-beam, followed by rapid thermal annealing; 3) Firstly, an anode electrode region is formed on the p-type epitaxial layer by photolithography, and then an anode electrode is deposited by electron beam evaporation (E-beam); 4) connecting the upper surface of the anode electrode deposition device to an external carrier wafer through a bonding process; 5) Depositing an isolation layer and an upper electrode layer on the lower surface of the cathode electrode by plasma enhanced chemical vapor deposition (PECVD) and electron beam evaporation (E-Beam); 6) defining N-type thermoelectric material and P-type thermoelectric material deposition regions and depositing N-type thermoelectric material layers and P-type thermoelectric material layers on the upper electrode layer by photolithography and metal organic chemical vapor deposition (MOCVD) to form a thermoelectric cooling unit; 7) depositing insulating filling material on the periphery of the thermoelectric cooling unit by plasma enhanced chemical vapor deposition (PECVD) or spin coating; 8) depositing a lower electrode layer on the thermoelectric cooling unit and the insulating filling material by electron beam evaporation E-Beam; 9) Bonding the heat sink material to the surface of the lower electrode layer through the heat transfer interface material, and removing the carrier wafer to complete the device manufacturing.
14. The method according to claim 13, Features: The process conditions of metal organic chemical vapor deposition (MOCVD) in step 1) are: TMGa is used as Ga precursor, O 2 As an oxygen source, N 2 As carrier gas, O 2 The flow rate ratio of TMGa is 10-40, the temperature is maintained at 550-700°C, and the growth pressure is maintained at 55-65 mbar; The process conditions of magnetron sputtering in step 1) are as follows: the deposition chamber is evacuated to 6×10 -4 Pa, the growth pressure is maintained at 1-5 Pa, and the sputtering power is set to 20-30 W; The process conditions of electron beam evaporation (E-Beam) in step 2) and step 3) are as follows: the working room is evacuated to 2.0×10 -4 Pa, the electron gun acceleration voltage is 6-10Kv, the electron gun beam current is 0.1-1A, and the evaporation time is 80-360s; The process conditions of electron beam evaporation E-Beam in step 5) and step 8) are as follows: the working room is evacuated to 2.5×10 -4 Pa, the electron gun acceleration voltage is 8-10Kv, the electron gun beam current is 0.4-1A, and the evaporation time is 240-2100s; In the step 5) and the step 7), the plasma enhanced chemical vapor deposition PECVD process conditions are as follows: Deposition of SiO 2 SiH 4 and N 2 O is the precursor gas, and the flow rate is maintained at 50-80 cm 3 / min, 160~200cm 3 / min, the temperature was maintained at 250-300°C, the growth pressure was maintained at 80-100Pa, and the RF power was set to 60-100W; Deposition of Si 3 N 4 SiH 4 and NH 3 The precursor gas is maintained at a flow rate of 10 to 30 cm 3 / min, 5~20cm 3 / min, the temperature is maintained at 200-400°C, the growth pressure is maintained at 100-150Pa, and the RF power is set to 50-500W; The process conditions of metal organic chemical vapor deposition MOCVD in step 6) are as follows: TMBi was used as a precursor of Bi, TDSb as a precursor of Sb, DipTe as a precursor of Te, TEL as a precursor of Pb, DESe as a precursor of Se, and high-purity H 2 As carrier gas; Deposition Bi 2 Te 3 The flow rate ratio of DipTe and TMBi is 2-10, the temperature is maintained at 200-500°C, and the growth pressure is maintained at 300-600 mbar; Deposition Sb 2 Te 3 The flow rate ratio of DipTe and TDSb is 1 to 6, the temperature is maintained at 250 to 450 °C, and the growth pressure is maintained at 200 to 500 mbar; The flow rate ratio of DipTe and TEL for depositing PbTe is 1 to 3, the temperature is maintained at 300 to 500 °C, and the growth pressure is maintained at 200 to 450 mbar; Deposition Bi 2 (TeSe) 3 The flow rate ratio of DipTe and TMBi is 1 to 8, the flow rate ratio of DipTe and DESe is 1 to 3, the temperature is maintained at 220 to 600 °C, and the growth pressure is maintained at 200 to 600 mbar; Deposition (BiSb) 2 Te 3 The flow rate ratio of DipTe and TMBi is 1 to 5, the flow rate ratio of TMBi and TDSb is 2 to 4, the temperature is maintained at 200 to 550° C., and the growth pressure is maintained at 300 to 500 mbar.
Citation Information
Patent Citations
Full-vertical type Si-based GaN UMOSFET power device and preparation method thereof
CN112018177A
Gallium oxide device for enhancing heat dissipation through electrocaloric refrigeration and preparation method
CN117855166A
High-thermal-conductivity gallium oxide transistor and preparation method thereof
CN118039701A
Method of performing AI deep learning-based OTC drug prescription service
KR1020230066858A
Structure for monolithic and heterogeneous integration of passive cavity-type single-crystal FBAR and active GAN HEMT
WO2022116395A1
Cited By
Sensor chip metal electrode thermal protection structure and preparation method thereof
CN119935197A
Preparation method of passive heat dissipation device of integrated circuit chip
CN120432453A
Semiconductor structure, manufacturing method and electronic device
CN120749093A
A semiconductor structure, fabrication method and electronic device
CN120749093B