Zwitterionic modified fluorine-containing poly (ester) amide thin layer composite reverse osmosis membrane as well as preparation method and application thereof
By constructing a synergistic effect of fluoropoly (ester)amide thin layer and zwitterionic layer in reverse osmosis membrane, the problems of selectivity and permeability trade-offs and poor pollution resistance in reverse osmosis technology are solved, and the problem of existing membranes is poorly controlled by reverse osmosis technology, and the problem of poor anti-pollution ability in the existing membrane is achieved. Improved high-efficiency desalination and anti-biological pollution performance.
Patent Information
- Application Number
- CN202411231617.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-15
AI Technical Summary
The existing polyamide thin-layer composite membranes have a trade-off between selectivity and permeability in reverse osmosis technology and have poor anti-pollution ability, making it difficult to achieve efficient desalination and anti-biological pollution.
By forming a thin layer of fluoropoly (ester) amide on the porous ultrafiltration base membrane and building an zwitterionic layer on its surface, the synergistic effect of fluoro nanochannels and superhydrophilic zwitterionic layer is used to enhance the desalination of the reverse osmosis membrane by utilizing the synergistic effect of the fluoro-containing nanochannels and the superhydrophilic zwitterionic layer. Efficiency and anti-biological pollution performance.
The efficient desalination performance of the reverse osmosis membrane and excellent anti-biological pollution performance are achieved, which significantly improves the water flux and sodium chloride retention rate, and has good long-term stability.
Smart Images

Figure CN118949689A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane treatment, and in particular to a zwitterion-modified fluorine-containing poly(ester)amide thin-layer composite reverse osmosis membrane and a preparation method and application thereof. Background Art
[0002] Faced with the increasingly serious problem of freshwater resource shortage, seawater desalination technology represented by reverse osmosis technology provides an important solution. As the core component of reverse osmosis technology, the development of membrane materials has an important impact on the efficiency and sustainability of reverse osmosis technology. In the past 40 years, polyamide thin layer composite membrane (PATFC) prepared by interfacial polymerization has been regarded as the gold standard of reverse osmosis membrane, but it still has many limitations, such as the trade-off between selectivity and permeability, poor anti-fouling ability, etc. Therefore, further research and innovation are still needed to promote the continuous development and improvement of new high-performance anti-biofouling reverse osmosis membrane materials. Summary of the invention
[0003] The purpose of the present invention is to provide a zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane that solves the above technical problems and has high-efficiency desalination performance and anti-biological fouling performance.
[0004] The purpose of the present invention is to provide a method for preparing the above-mentioned zwitterion-modified fluorine-containing poly (ester) amide thin-layer composite reverse osmosis membrane.
[0005] The purpose of the present invention is to provide an application of the above-mentioned zwitterion-modified fluorine-containing poly (ester) amide thin-layer composite reverse osmosis membrane.
[0006] To this end, the technical solution of the present invention is as follows:
[0007] A zwitterion modified fluorinated poly(ester)amide thin layer composite reverse osmosis membrane comprises a porous ultrafiltration base membrane firstly composited with a fluorinated poly(ester)amide thin layer to form a fluorinated poly(ester)amide thin layer, and then based on the reaction of residual acyl chloride groups on the surface of the fluorinated poly(ester)amide thin layer with zwitterion monomers to form a zwitterion layer; the fluorinated poly(ester)amide thin layer is specifically formed by copolymerization and crosslinking of the fluorinated poly(ester)amide thin layer with polyamine monomers, fluorinated polyphenol monomers and acyl chloride monomers, or by copolymerization and crosslinking of polyamine monomers, fluorinated polyamine monomers and acyl chloride monomers.
[0008] In the present invention, by constructing fluorine-containing nanochannels in the separation membrane, rapid water transport of water molecules in the channels can be achieved. However, the inherent strong hydrophobicity of fluorine atoms will increase the energy barrier that water molecules have to cross to enter the channels. Based on this, a hydrophilic layer is further constructed on the surface of the separation layer with fluorine-containing channels to solve the above problem. Specifically, a hydrophilic zwitterionic layer is constructed based on the reaction of residual acyl chloride groups on the surface of the fluorine-containing poly (ester) amide thin layer with zwitterionic monomers. Considering that zwitterions have unique molecular structures and physical and chemical properties, their strong hydration ability is conducive to the formation of a hydration layer. The present application has found through a large number of experiments that trimethylamine N-oxides (abbreviated as TMAO) have a high hydrophilicity due to their The anions and cations are directly connected without a spacer in between, and have stronger hydration ability than PC, CB, and SB. They are used in the modification of reverse osmosis membranes, that is, the surface of the separation layer with fluorine-containing nanochannels is modified with a TMAO-type zwitterionic layer to provide traction for water molecules to enter the fluorine-containing nanochannels, so as to utilize the synergistic effect of the fluorine-containing nanochannels and the super-hydrophilic zwitterionic layer to improve the desalination efficiency of the reverse osmosis membrane while giving it excellent anti-biological fouling performance; in summary, the composite reverse osmosis membrane of the present invention synergizes the fluorine-containing structure of the fluorine-containing poly (ester) amide thin layer with the zwitterionic structure in the zwitterionic layer to improve the desalination efficiency of the reverse osmosis membrane and the anti-biological fouling effect.
[0009] Furthermore, the polyamine is o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, mesitylenetriamine or piperazine.
[0010] Furthermore, the fluorinated polyphenols are 4-fluororesorcinol, 5-fluororesorcinol, 2,3,5,6-tetrafluorohydroquinone, 5-(trifluoromethyl)benzene-1,3-diol, 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene, 9-(trifluoromethyl)-9-(3-(trifluoromethyl)phenyl)-9H-xanthene-3,6-diol, 9-(3,5-bis(trifluoromethyl)phenyl)-9-(trifluoromethyl) )-9H-xanthene-3,6-diol or 4,4'-(2,2,2-trifluoro-1-phenylethane-1,1-diyl)bis(benzene-1,2-diol); the fluorine-containing polyamine monomer is 5-fluorobenzene-1,3-diamine, 3,4-diaminofluorobenzene, 5-trifluoromethyl-1,3-phenylenediamine, 2-trifluoromethyl-1,4-phenylenediamine, 4-trifluoromethyl-o-phenylenediamine or 6-(trifluoromethyl)benzene-1,2,4-triamine.
[0011] Furthermore, the acyl chloride monomer is 1,3-phthaloyl chloride, 1,4-phthaloyl chloride, 1,3,5-benzenetricarboxylic acid chloride, 1,2,4-benzenetricarboxylic acid chloride or 1,2,4,5-benzenetetracarboxylic acid chloride.
[0012] Furthermore, the weight ratio of the polyamine monomer to the fluorine-containing polyphenol monomer, or the polyamine monomer to the fluorine-containing polyamine monomer is (9-1):(1-9), more preferably (4-1):(1-4).
[0013] Furthermore, the porous ultrafiltration base membrane is a polysulfone membrane, a polyethersulfone membrane, a polyimide membrane or a polyacrylonitrile membrane.
[0014] Further, the zwitterion is N-methyldiethanolamine N-oxide (MDEAO) or N-methylethylenediamine N-oxide (DNMAO); wherein N-methyldiethanolamine N-oxide is prepared by oxidizing N-methyldiethanolamine with a strong oxidant, and N,N-bis(3-aminopropyl)methylamine N-oxide monomer is prepared by oxidizing N,N-bis(3-aminopropyl)methylamine with a strong oxidant; the strong oxidant is preferably hydrogen peroxide (H 2 O 2 ).
[0015] In the present invention, the tertiary amine group in N-methyldiethanolamine (MDEA) is easily oxidized by a strong oxidant to synthesize N-methyldiethanolamine N-oxide monomer (MDEAO); the chemical reaction equation of the oxidation reaction process is:
[0016]
[0017] The tertiary amine group in N,N-bis(3-aminopropyl)methylamine (DNMA) is easily oxidized by a strong oxidant to synthesize N,N-bis(3-aminopropyl)methylamine N-oxide monomer (DNMAO); the chemical reaction equation of the oxidation reaction process is:
[0018]
[0019] Specifically, N-methyldiethanolamine N-oxide monomer and N,N-bis(3-aminopropyl)methylamine N-oxide monomer can be prepared by, but not limited to, the following method, wherein: 1) under ice bath conditions, a 30 wt.% aqueous hydrogen peroxide solution is added to a single-necked flask, and then N-methyldiethanolamine or N,N-bis(3-aminopropyl)methylamine is added dropwise, wherein the mass ratio of the N-methyldiethanolamine aqueous hydrogen peroxide solution or the mass ratio of N,N-bis(3-aminopropyl)methylamine to the aqueous hydrogen peroxide solution is 1:(1.5-2), to obtain a reaction mixture; ; 2) exposing the reaction mixture to air and stirring at room temperature for at least 48 hours to fully oxidize and obtain a reaction product liquid; 3) heating the reaction product liquid to 60°C to 65°C to decompose excess hydrogen peroxide, and detecting whether it is completely removed by starch potassium iodide test paper; 4) removing water by rotary evaporation at 60°C to 65°C, and washing with anhydrous ether precipitation; drying the precipitate obtained by washing in a 40°C oven to obtain a colorless viscous liquid, which is N-methyldiethanolamine N-oxide monomer or N,N-bis(3-aminopropyl)methylamine N-oxide monomer (yield ≥ 99%).
[0020] A method for preparing the above-mentioned zwitterion-modified fluorinated poly (ester) amide thin-layer composite reverse osmosis membrane comprises the following steps:
[0021] S1, dissolving a polyamine monomer and a fluorinated polyphenol monomer, or a polyamine monomer and a fluorinated polyphenol monomer in an alkaline solution to prepare an aqueous phase solution having a composite monomer concentration of 0.1 wt.% to 5.0 wt.%;
[0022] S2, dissolving the acyl chloride monomer in an organic solvent to prepare a mixed solution with an acyl chloride monomer concentration of 0.01 wt.% to 0.5 wt.%;
[0023] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 30s to 600s to obtain a membrane intermediate;
[0024] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 10s to 300s to obtain a primary membrane;
[0025] S5, placing the primary membrane in a blast drying oven at 60° C. to 80° C. for heat treatment for 5 min to 10 min to obtain a fluorine-containing poly(ester)amide thin-layer composite reverse osmosis membrane;
[0026] S6, dissolving the zwitterionic monomer and the catalyst in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 0.1 wt.% to 2.0 wt.%;
[0027] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 30s to 600s, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0028] Furthermore, in step S1, the alkaline solution is a sodium hydroxide aqueous solution or a triethylamine aqueous solution, and its pH is preferably 13; the concentration of the complex monomer in the aqueous phase solution is preferably 0.5 wt.% to 2.0 wt.%.
[0029] Furthermore, in step S2, the organic solvent is n-hexane or isoparaffin Isopar G; and the concentration of the acyl chloride monomer is 0.01 wt.% to 0.1 wt.%.
[0030] Furthermore, in step S3, the contact time between the porous polysulfone ultrafiltration base membrane and water is preferably 120s to 300s.
[0031] Furthermore, in step S4, the contact time between the membrane intermediate and the oil phase solution is preferably 30 s to 300 s.
[0032] Further, in step S6, the catalyst is 4-dimethylaminopyridine catalyst, and the amount added is 0.5 times the molar amount of the zwitterionic monomer.
[0033] An application of the above zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane is specifically used as a desalination membrane in liquid separation treatment.
[0034] Compared with the existing technology, the zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane firstly adopts interfacial polymerization and post-treatment method to efficiently and quickly prepare a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane, and constructs a TMAO-type zwitterion layer with super hydration ability on the surface of the separation layer with fluorinated nanochannels. The synergistic effect of the two provides a strong boost for the rapid transport of water molecules through the membrane. Compared with traditional polyamide reverse osmosis membranes, this reverse osmosis membrane is used as a desalination membrane in liquid separation treatment, and has better water permeability and desalination rate, as well as good anti-biological contamination performance and long-term stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a comparison chart of the water flux and NaCl rejection of the zwitterion-modified fluorinated poly (ester) amide reverse osmosis membrane prepared in Example 1 of the present invention as the modification time of the zwitterion solution changes;
[0036] Figure 2 It is a comparison chart of the desalination performance test results of the composite reverse osmosis membranes prepared by Example 1 of the present invention and Comparative Examples 1 to 3;
[0037] Figure 3 This is a comparison chart of the antibacterial rates of the composite reverse osmosis membranes prepared by Example 1 of the present invention and Comparative Examples 1 to 3 against Escherichia coli and Staphylococcus aureus;
[0038] Figure 4 This is a SEM comparison diagram of the composite reverse osmosis membranes prepared by Example 1 of the present invention and Comparative Examples 1 to 3 after antibacterial experiments on Escherichia coli and Staphylococcus aureus. DETAILED DESCRIPTION
[0039] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the following embodiments are by no means intended to limit the present invention in any way.
[0040] Example 1
[0041] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0042] S1, dissolving 4.0 g of m-phenylenediamine and 1.0 g of 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene (the weight ratio of the two is 4:1) in a sodium hydroxide aqueous solution at pH=13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0 wt.%;
[0043] S2, preparing a n-hexane solution with a concentration of 0.1 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0044] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0045] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 30 seconds, removing the residual liquid, and obtaining a primary membrane;
[0046] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 5 minutes to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0047] S6, dissolving N-methyldiethanolamine N-oxide monomer and 4-dimethylaminopyridine catalyst in a molar amount of 0.5 times that of N-methyldiethanolamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 1.0 wt.%; wherein,
[0048] The preparation method of N-methyldiethanolamine N-oxide monomer is as follows: under ice bath conditions, 30wt.% hydrogen peroxide aqueous solution is added to a single-necked flask, and then N-methyldiethanolamine is added dropwise, the mass ratio of N-methyldiethanolamine to hydrogen peroxide aqueous solution is 1:1.5, to obtain a reaction mixture; the reaction mixture is exposed to air environment and stirred at room temperature for 48 hours to obtain a reaction product; then, under stirring conditions, the reaction product is heated to 60°C to decompose excess hydrogen peroxide, and starch potassium iodide test paper is used to detect whether it is completely removed; then, water is removed by rotary evaporation at 60°C, and anhydrous ether precipitation is washed; finally, the washed precipitate is dried, and the obtained colorless viscous liquid is N-methyldiethanolamine N-oxide monomer (yield 99%); the same as in the following examples;
[0049] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 300 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0050] Example 2
[0051] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0052] S1, dissolving 2.5 g of m-phenylenediamine and 2.5 g of 5-fluororesorcinol (the weight ratio of the two is 1:1) in a sodium hydroxide aqueous solution with a pH of 13 to prepare an aqueous phase solution with a composite monomer concentration of 2.0 wt.%;
[0053] S2, preparing a n-hexane solution with a concentration of 0.1 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0054] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0055] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 30 seconds, removing the residual liquid, and obtaining a primary membrane;
[0056] S5. The primary membrane is placed in a 60° C. forced air drying oven for heat treatment for 5 minutes to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0057] S6, dissolving N,N-bis(3-aminopropyl)methylamine N-oxide monomer and 4-dimethylaminopyridine catalyst in a molar amount of 0.5 times that of N-methyldiethanolamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 0.5 wt %; wherein,
[0058] The preparation method of N,N-bis(3-aminopropyl)methylamine N-oxide monomer is as follows: under ice bath conditions, 30wt.% hydrogen peroxide aqueous solution is added to a single-necked flask, and then N,N-bis(3-aminopropyl)methylamine is added dropwise, the mass ratio of N,N-bis(3-aminopropyl)methylamine to hydrogen peroxide aqueous solution is 1:2, to obtain a reaction mixture; the reaction mixture is exposed to air environment and stirred at room temperature for 48 hours to obtain a reaction product; then, under stirring conditions, the reaction product is heated to 65°C to decompose excess hydrogen peroxide, and starch potassium iodide test paper is used to detect whether it is completely removed; then, water is removed by rotary evaporation at 60°C, and the precipitation is washed with anhydrous ether; finally, the washed precipitate is dried, and the obtained colorless viscous liquid is N,N-bis(3-aminopropyl)methylamine N-oxide monomer (yield 99%); the following examples are the same;
[0059] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 120 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0060] Example 3
[0061] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0062] S1, 3.0 g of m-phenylenediamine and 2.0 g of 4,4'-(2,2,2-trifluoro-1-phenylethane-1,1-diyl)bis(benzene-1,2-diol) (the weight ratio of the two is 3:2) are dissolved in a triethylamine aqueous solution at pH=13 to prepare an aqueous phase solution with a composite monomer concentration of 0.5 wt.%;
[0063] S2, preparing a n-hexane solution with a concentration of 0.01 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0064] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 180 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0065] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 120 seconds, removing the residual liquid, and obtaining a primary membrane;
[0066] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 10 min to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0067] S6, dissolving N,N-bis(3-aminopropyl)methylamine N-oxide monomer and 4-dimethylaminopyridine catalyst in a molar amount of 0.5 times that of N-methyldiethanolamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 2.0 wt %;
[0068] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 600 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0069] Example 4
[0070] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0071] S1, dissolving 2.0 g of m-phenylenediamine and 3.0 g of 5-fluorobenzene-1,3-diamine (the weight ratio of the two is 2:3) in a triethylamine aqueous solution at pH = 13 to prepare an aqueous phase solution with a composite monomer concentration of 2.0 wt.%;
[0072] S2, preparing an isoparaffin Isopar G solution with a concentration of 0.1 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0073] S3, contacting the porous polyethersulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0074] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 60 seconds, removing the residual liquid, and obtaining a primary membrane;
[0075] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 10 min to obtain a fluorine-containing polyamide thin-layer composite reverse osmosis membrane.
[0076] S6, dissolving N-methyldiethanolamine N-oxide monomer and 4-dimethylaminopyridine catalyst in a molar amount of 0.5 times that of N-methyldiethanolamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 0.1 wt %;
[0077] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 480 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0078] Example 5
[0079] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0080] S1, dissolving 1.0 g of m-phenylenediamine and 4.0 g of 5-trifluoromethyl-1,3-phenylenediamine (the weight ratio of the two is 1:4) in a sodium hydroxide aqueous solution at pH=13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0 wt.%;
[0081] S2, preparing an isoparaffin Isopar G solution with a concentration of 0.05 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0082] S3, contacting the porous polyacrylonitrile ultrafiltration base membrane with the aqueous solution prepared in step S1 for 120 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0083] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 60 seconds, removing the residual liquid, and obtaining a primary membrane;
[0084] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 10 min to obtain a fluorine-containing polyamide thin-layer composite reverse osmosis membrane.
[0085] S6, dissolving N-methyldiethanolamine N-oxide monomer and 4-dimethylaminopyridine catalyst in a molar amount of 0.5 times that of N-methyldiethanolamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 1.5 wt %;
[0086] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 60 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0087] Example 6
[0088] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0089] S1, 3.0 g of m-phenylenediamine and 2.0 g of 6-(trifluoromethyl)benzene-1,2,4-triamine (the weight ratio of the two is 3:2) are dissolved in a sodium hydroxide aqueous solution with a pH of 13 to prepare an aqueous phase solution with a composite monomer concentration of 2.0 wt.%;
[0090] S2, preparing an isoparaffin Isopar G solution with a 1,3-phthaloyl chloride concentration of 0.05 wt.% as the oil phase solution;
[0091] S3, contacting the porous polyimide ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0092] S4, contacting the membrane obtained in step S3 with the oil phase solution prepared in step S2 for 60 seconds, removing the residual liquid, and obtaining a primary membrane;
[0093] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 10 min to obtain a fluorine-containing polyamide thin-layer composite reverse osmosis membrane.
[0094] S6, dissolving N,N-bis(3-aminopropyl)methylamine N-oxide monomer and 0.5 times the molar amount of 4-dimethylaminopyridine catalyst as that of N,N-bis(3-aminopropyl)methylamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 0.5 wt %;
[0095] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 360 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0096] Example 7
[0097] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0098] S1, taking 3.5g of mesitylenetriamine and 1.5g of 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene (the weight ratio of the two is 7:3) and dissolving them in a sodium hydroxide aqueous solution with a pH of 13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0wt.%;
[0099] S2, preparing a n-hexane solution with a concentration of 0.1 wt.% of 1,2,4,5-benzenetracarboxylic acid chloride as an oil phase solution;
[0100] S3, contacting the porous polyacrylonitrile ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0101] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 90 seconds, removing the residual liquid, and obtaining a primary membrane;
[0102] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 5 minutes to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0103] S6, dissolving N-methyldiethanolamine N-oxide monomer and 4-dimethylaminopyridine catalyst in a molar amount of 0.5 times that of N,N-bis(3-aminopropyl)methylamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 2.0 wt %;
[0104] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 30 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0105] Example 8
[0106] A method for preparing a zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane that resists biological contamination is prepared by the following steps:
[0107] S1, taking 2.5g of piperazine and 2.5g of 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene (the weight ratio of the two is 1:1) and dissolving them in a sodium hydroxide aqueous solution with a pH of 13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0wt.%;
[0108] S2, preparing a n-hexane solution with a 1,3-phthaloyl chloride concentration of 0.1 wt.% as an oil phase solution;
[0109] S3, contacting the porous polyacrylonitrile ultrafiltration base membrane with the aqueous solution prepared in step S1 for 180 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0110] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 300 seconds, removing the residual liquid, and obtaining a primary membrane;
[0111] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 10 min to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0112] S6, dissolving N,N-bis(3-aminopropyl)methylamine N-oxide monomer and 0.5 times the molar amount of 4-dimethylaminopyridine catalyst as that of N,N-bis(3-aminopropyl)methylamine N-oxide monomer in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 1.0 wt%;
[0113] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 180 seconds, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0114] Comparative Example 1
[0115] A polyamide reverse osmosis composite membrane is prepared by the following steps:
[0116] S1, contacting the porous polysulfone ultrafiltration base membrane with an alkaline aqueous solution of metaphenylenediamine (MPD) with a concentration of 1.0 wt.% (sodium hydroxide solution with a pH of 13) for 300 s to remove the residual liquid;
[0117] S2. The membrane obtained in step S1 is contacted with a 0.1 wt. % n-hexane solution of 1,3,5-benzenetricarboxylic acid chloride for 60 seconds, the residual liquid is removed, and the membrane is heat treated at 80° C. for 5 minutes to obtain a polyamide reverse osmosis composite membrane.
[0118] Comparative Example 2
[0119] An unmodified fluorine-containing polyester amide reverse osmosis composite membrane is prepared by the following steps:
[0120] S1, dissolving 4.0 g of m-phenylenediamine and 1.0 g of 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene (the weight ratio of the two is 4:1) in a sodium hydroxide aqueous solution at pH=13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0 wt.%;
[0121] S2, preparing a n-hexane solution with a concentration of 0.1 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0122] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0123] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 30 seconds, removing the residual liquid, and obtaining a primary membrane;
[0124] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 5 minutes to obtain a fluorine-containing polyester amide thin layer composite reverse osmosis membrane that is not modified by zwitterions.
[0125] Comparative Example 3
[0126] A non-zwitterion-modified polyesteramide reverse osmosis composite membrane is prepared by the following steps:
[0127] S1, dissolving 4.0 g of m-phenylenediamine and 1.0 g of 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene (the weight ratio of the two is 4:1) in a sodium hydroxide aqueous solution at pH=13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0 wt.%;
[0128] S2, preparing a n-hexane solution with a concentration of 0.1 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0129] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0130] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 30 seconds, removing the residual liquid, and obtaining a primary membrane;
[0131] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 5 minutes to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0132] S6, dissolving non-zwitterionized N-methyldiethanolamine (MDEA) monomer and 0.5 times the molar amount of 4-dimethylaminopyridine catalyst as that of non-zwitterionized N-methyldiethanolamine (MDEA) monomer in deionized water to prepare a modified solution having a zwitterion monomer concentration of 1.0 wt %;
[0133] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 300 seconds, and rinsing to obtain a non-zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0134] Comparative Example 4
[0135] A non-TMAO derivative zwitterion-modified polyester amide reverse osmosis composite membrane is prepared by the following steps:
[0136] S1, dissolving 4.0 g of m-phenylenediamine and 1.0 g of 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene (the weight ratio of the two is 4:1) in a sodium hydroxide aqueous solution at pH=13 to prepare an aqueous phase solution with a composite monomer concentration of 1.0 wt.%;
[0137] S2, preparing a n-hexane solution with a concentration of 0.1 wt.% of 1,3,5-benzenetricarboxylic acid chloride as an oil phase solution;
[0138] S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 300 seconds, removing the residual liquid, and obtaining a membrane intermediate;
[0139] S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 30 seconds, removing the residual liquid, and obtaining a primary membrane;
[0140] S5. The primary membrane is placed in a forced air drying oven at 80° C. for heat treatment for 5 minutes to obtain a fluorine-containing polyester amide thin-layer composite reverse osmosis membrane.
[0141] S6, dissolving a zwitterionic aminoethylpiperazine propane sulfonate (AEPPS) monomer and a 4-dimethylaminopyridine catalyst having a molar amount of 0.5 times that of the zwitterionic aminoethylpiperazine propane sulfonate in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 1.0 wt %;
[0142] S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 300 seconds, and rinsing to obtain a non-zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
[0143] Comparative Example 5
[0144] A zwitterion-modified fluorine-free polyesteramide reverse osmosis composite membrane is prepared by the following steps:
[0145] S1, contacting the porous polysulfone ultrafiltration base membrane with an alkaline aqueous solution (sodium hydroxide solution with pH=13) of m-phenylenediamine and resorcinol with a concentration of 0.5wt.% and a weight ratio of 4:1 for 300s, and removing the residual liquid;
[0146] S2. The membrane obtained in step 1 is contacted with a 0.05 wt. % 1,3,5-benzenetricarboxylic acid chloride n-hexane solution for 60 seconds, the residual liquid is removed, and the membrane is heat treated at 60° C. for 5 minutes to obtain a fluorine-free polyester amide reverse osmosis composite membrane.
[0147] S3, dissolving the non-zwitterionized N-methyldiethanolamine monomer and 0.5 times the molar amount of 4-dimethylaminopyridine catalyst as that of the non-zwitterionized N-methyldiethanolamine monomer in deionized water to prepare a modified solution having a zwitterion monomer concentration of 1.0 wt%;
[0148] S4, contacting the fluorine-free polyester amide thin layer composite reverse osmosis membrane prepared in step S2 with the modified solution prepared in step S3 for 300 seconds, and rinsing to obtain a zwitterion-modified fluorine-free polyester amide thin layer composite reverse osmosis membrane.
[0149] Performance Test:
[0150] (I) Water flux and sodium chloride retention rate test:
[0151] Water flux and retention rate are two important parameters for evaluating the desalination performance of reverse osmosis membranes. In this test, the desalination performance of reverse osmosis membranes is evaluated through a cross-flow filtration device. Among them, water flux (water flux, J) is defined as: the volume of water that permeates through a unit area per unit time under certain operating conditions, with the unit of L m -2 h -1 The rejection rate (R) is defined as: under certain operating conditions, the difference between the salt concentration of the feed solution and the salt concentration of the permeate divided by the salt concentration of the feed solution. The specific test results are shown in Table 1 below.
[0152] Table 1:
[0153]
[0154] From the test results in Table 1, we can see that:
[0155] The sodium chloride rejection rate of the TMAO-type zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane (FPEA-MDEAO) prepared in Examples 1 to 8 of the present invention is 97.3% to 99.1%, and has excellent desalination performance;
[0156] Comparative Example 1 prepared a polyamide reverse osmosis membrane (PA), which differed from Example 1 in that, on the one hand, the comparative example used a functional layer that was not modified with fluorine on a porous polysulfone ultrafiltration base membrane, and on the other hand, the ion layer was not modified with zwitterionic monomers. Therefore, the water flux of Comparative Example 1 was 15.5 Lm -2 h -1 The sodium chloride rejection rate was 96.2%, which was much lower than the water flux of 54.1 Lm in Example 1. -2 h -1 and sodium chloride rejection rate 99.1%;
[0157] Comparative Example 2 prepared a fluorinated polyester amide reverse osmosis membrane (FPEA), which was different from Example 1 in that, although the functional layer of the comparative example was modified with fluorine like Example 1, the ionic layer was not modified with zwitterionic monomers. Therefore, the water flux of Comparative Example 2 was 33.6 Lm -2 h -1 The sodium chloride rejection rate was 97.1%, which was still lower than the water flux of Example 1 (54.1 Lm). -2 h -1 and sodium chloride rejection rate 99.1%;
[0158] It can be seen that Example 1 achieves a significant improvement in the water flux and sodium chloride rejection rate of the reverse osmosis membrane by sequentially modifying the fluorine-containing modification of the functional layer and the modification of the ion layer, and the performance is more excellent.
[0159] also,
[0160] Comparative Example 3 prepared a non-zwitterionic (MDEA) modified fluoropolyester membrane (FPEA-MDEA), which showed a slightly higher water flux (38.3 Lm -2 h -1 ) and salt rejection rate (98.3%), but the performance in these two aspects is still slightly worse than that of Example 1;
[0161] Comparative Example 4 prepared a zwitterion (AEPPS) modified fluorinated polyester amide membrane (FPEA-AEPPS), which showed a slightly higher water flux (47.2 Lm -2 h -1 ) and salt rejection rate (98.8%), but the performance in these two aspects is still slightly worse than that of Example 1;
[0162] It can be seen that although in Comparative Examples 3 and 4, the ionic layer was also modified based on the fluorine-containing modification of the functional layer, they were not as good as the fluorine-containing polyester amide reverse osmosis membrane modified with TMAO-type zwitterions in Example 1, which highlights the important role of TMAO-type zwitterions in improving the desalination efficiency.
[0163] Comparative Example 5 prepared a fluorine-free polyester amide reverse osmosis membrane (PEA-MDEAO) modified by MDEAO zwitterion. The difference between it and Example 1 is that the functional layer is not modified with fluorine, and the same ion layer modification as in Example 1 is performed. Correspondingly, the water flux of the reverse osmosis membrane prepared in this comparative example (36.1 Lm -2 h -1 ) and salt retention rate (98.4%), both properties are still slightly worse than those of Example 1;
[0164] It can be seen that in the TMAO-type zwitterion-modified fluorinated polyester amide membrane of the present invention, the fluorinated structure of the fluorinated poly (ester) amide thin layer and the zwitterion structure in the zwitterion layer work synergistically to jointly improve the water flux and salt retention rate of the reverse osmosis membrane, that is, the importance of fluorinated nanochannels.
[0165] like Figure 1 The figure shows a comparison of the water flux and NaCl rejection of the zwitterion-modified fluorinated poly(ester)amide reverse osmosis membrane prepared in Example 1 of the present invention as the modification time of the zwitterion solution changes; Figure 2 The figure shows a comparison of the desalination performance test results of the composite reverse osmosis membranes prepared by Example 1 of the present invention and Comparative Examples 1 to 3; the test results in the figure clearly show the unique advantages of the zwitterion-modified fluorinated polyester amide membrane prepared by the present invention; it can be seen that the present invention successfully constructs a fluorinated nanochannel that is conducive to rapid water transmission and excludes salt in the separation layer by introducing a fluorinated polyphenol monomer or a fluorinated polyamine monomer into the aqueous phase monomer to participate in the interfacial polymerization reaction, and then constructs a TMAO-type zwitterion layer on the surface of the separation layer with the fluorinated nanochannel, and the synergistic effect of the two effectively improves the water flux and desalination performance of the reverse osmosis membrane.
[0166] (II) Anti-biological contamination performance test
[0167] The anti-biological fouling performance of the reverse osmosis membrane prepared in the embodiment and the control example was investigated by the plate count method. Cut each composite membrane into pieces, take 0.3g and put it into a 100mL conical flask, add 2mL 105CFU / mL bacterial solution and 28mL PBS buffer (pH=7.4) respectively, place the conical flask in a constant temperature shaking shaker, and shake at 120r / min and 25℃ for 24 hours. Take 300μL of the cultured bacterial solution, dilute it with sterile water, and spread it on the agar solid culture medium, and culture it in a constant temperature incubator at 37℃ for 24 hours. After the culture is completed, record the number of colonies and calculate the antibacterial rate. The antibacterial rate calculation formula is as follows:
[0168] N=Z×R,
[0169] K=(1-N m / N 0 )×100%,
[0170] Where R is the dilution factor; N (CFU / mL) is the concentration of bacteria in each conical flask; Z (CFU / mL) is the average value of the number of colonies in the agar solid medium corresponding to each membrane sample; K is the inhibition rate; N m (CFU / mL) is the bacterial concentration corresponding to the membrane sample; N 0 (CFU / mL) is the bacterial concentration of the blank control group.
[0171] like Figure 3 The figure shows the comparison of the antibacterial rates of the composite reverse osmosis membranes prepared by Example 1 of the present invention and Comparative Examples 1 to 3 against Escherichia coli and Staphylococcus aureus. The test results shown in the figure show that the MDEAO zwitterion-modified fluorinated polyester amide (FPEA-MDEAO) reverse osmosis membrane prepared by Example 1 of the present invention has a strong bactericidal ability against Gram-positive bacteria represented by Staphylococcus aureus and Gram-negative bacteria represented by Escherichia coli.
[0172] like Figure 4 The SEM comparison diagram of the composite reverse osmosis membranes prepared by Example 1 of the present invention and Comparative Examples 1 to 3 after the antibacterial test on Escherichia coli (E. coli) and Staphylococcus aureus (S. aureus) is shown. The test results shown in the figure show that there are no residual Escherichia coli and Staphylococcus aureus on the surface of the FPEA-MDEAO membrane, and the membrane surface morphology is basically the same as that before the antibacterial test (see Figure 4 a3 and b3 in the figure), indicating that it has excellent anti-adhesion performance; while a large number of Escherichia coli and Staphylococcus aureus with intact morphology remain on the surface of the PA film (see Figure 4 a1 and b1 in the figure), indicating that the PA membrane has a poor anti-adhesion effect on bacteria and has almost no bactericidal ability; the bacteria on the surface of the FPEA membrane are damaged in morphology, but the dead bacteria are aggregated and contaminated on the membrane surface (see Figure 4 a2 and b2 in ), indicating that the FPEA membrane has good bactericidal properties, but poor anti-adhesion properties; a small amount of Escherichia coli and Staphylococcus aureus were present on the surface of the FPEA-MDEA membrane (see Figure 4 a4 and b4 in the figure), and some bacteria were damaged, indicating that it has good bactericidal and anti-adhesion properties; it can be seen that the MDEAO zwitterion-modified fluorinated polyester amide (FPEA-MDEAO) reverse osmosis membrane prepared in Example 1 of the present invention has excellent anti-biological adhesion properties.
[0173] In summary, the zwitterion-modified fluorinated polyester amide reverse osmosis membrane of the present invention has excellent water flux and sodium chloride rejection rate, as well as strong anti-biological fouling performance.
Claims
1. A zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane, characterized in that: The method comprises a porous ultrafiltration base membrane firstly compounded with a fluorine-containing poly(ester)amide thin layer to form a fluorine-containing poly(ester)amide thin layer, and then the residual acyl chloride groups on the surface of the fluorine-containing poly(ester)amide thin layer react with zwitterionic monomers to form a zwitterionic layer; wherein the fluorine-containing poly(ester)amide thin layer is formed by copolymerization and cross-linking of polyamine monomers, fluorine-containing polyphenol monomers and acyl chloride monomers, or by copolymerization and cross-linking of polyamine monomers, fluorine-containing polyamine monomers and acyl chloride monomers.
2. The zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to claim 1, characterized in that: The polyamine is o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, mesitylenetriamine or piperazine.
3. The zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to claim 1, characterized in that: Fluorinated polyphenols include 4-fluororesorcinol, 5-fluororesorcinol, 2,3,5,6-tetrafluorohydroquinone, 5-(trifluoromethyl)benzene-1,3-diol, 3,6-dihydroxy-9-trifluoromethyl-9-phenylxanthene, 9-(trifluoromethyl)-9-(3-(trifluoromethyl)phenyl)-9H-xanthene-3,6-diol, 9-(3,5-bis(trifluoromethyl)phenyl)-9-(trifluoromethyl)-9 H-xanthene-3,6-diol or 4,4'-(2,2,2-trifluoro-1-phenylethane-1,1-diyl)bis(benzene-1,2-diol); the fluorine-containing polyamine monomer is 5-fluorobenzene-1,3-diamine, 3,4-diaminofluorobenzene, 5-trifluoromethyl-1,3-phenylenediamine, 2-trifluoromethyl-1,4-phenylenediamine, 4-trifluoromethyl-o-phenylenediamine or 6-(trifluoromethyl)benzene-1,2,4-triamine.
4. The zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to claim 1, characterized in that: The acyl chloride monomer is 1,3-phthaloyl chloride, 1,4-phthaloyl chloride, 1,3,5-benzenetricarboxylic acid chloride, 1,2,4-benzenetricarboxylic acid chloride or 1,2,4,5-benzenetetracarboxylic acid chloride.
5. The zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to claim 1, characterized in that: The weight ratio of the polyamine monomer to the fluorine-containing polyphenol monomer, or the polyamine monomer to the fluorine-containing polyamine monomer is (9-1): (1-9).
6. The zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to claim 1, characterized in that: The porous ultrafiltration base membrane is a polysulfone membrane, a polyethersulfone membrane, a polyimide membrane or a polyacrylonitrile membrane.
7. The zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to claim 1, characterized in that: The zwitterion is N-methyldiethanolamine N-oxide or N-methylethylenediamine N-oxide.
8. A method for preparing a zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane according to any one of claims 1 to 7, characterized in that: Here are the steps: S1, dissolving a polyamine monomer and a fluorinated polyphenol monomer, or a polyamine monomer and a fluorinated polyphenol monomer in an alkaline solution to prepare an aqueous phase solution having a composite monomer concentration of 0.1 wt.% to 5.0 wt.%; S2, dissolving the acyl chloride monomer in an organic solvent to prepare a mixed solution with an acyl chloride monomer concentration of 0.01 wt.% to 0.5 wt.%; S3, contacting the porous polysulfone ultrafiltration base membrane with the aqueous solution prepared in step S1 for 30s to 600s to obtain a membrane intermediate; S4, contacting the membrane intermediate obtained in step S3 with the oil phase solution prepared in step S2 for 10s to 300s to obtain a primary membrane; S5, placing the primary membrane in a blast drying oven at 60° C. to 80° C. for heat treatment for 5 min to 10 min to obtain a fluorine-containing poly(ester)amide thin-layer composite reverse osmosis membrane; S6, dissolving the zwitterionic monomer and the catalyst in deionized water to prepare a modified solution having a zwitterionic monomer concentration of 0.1 wt.% to 2.0 wt.%; S7, contacting the fluorinated poly (ester) amide thin layer composite reverse osmosis membrane with the modified solution prepared in step S6 for 30s to 600s, and rinsing to obtain a zwitterion-modified fluorinated poly (ester) amide thin layer composite reverse osmosis membrane.
9. The preparation method according to claim 8, characterized in that: In step S1, the alkaline solution is a sodium hydroxide aqueous solution or a triethylamine aqueous solution; in step S2, the organic solvent is n-hexane or isoparaffin Isopar G.
10. An application of the zwitterion-modified fluorinated poly(ester)amide thin-layer composite reverse osmosis membrane as claimed in any one of claims 1 to 7, characterized in that: Used as a desalination membrane in liquid separation processing.
Citation Information
Cited By
Synergistic enhancement type desalination membrane as well as preparation method and application thereof
CN121490591A
A synergistically enhanced desalination membrane and its preparation method and application
CN121490591B