Kaolin-based magnesium oxide carbon dioxide adsorbent and preparation method thereof
The liquid phase in-situ synthesis and impregnation method of kaolin-based magnesium oxide carbon dioxide adsorbent is prepared, and the problems of slow kinetics and poor cycle stability in high temperature environments are solved, thus achieving efficient CO2 capture and cost reduction, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202411315618.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
The existing MgO carbon dioxide adsorbents have slow kinetics and poor cycle stability under high temperature environments, and have high cost in preparation process, which affects the CO2 capture efficiency and economy.
Magnesium hydroxide carbon dioxide adsorbent is used to synthesize magnesium hydroxide through liquid phase in situ synthesis method, and magnesium oxide is uniformly grown on kaolin to control the heating rate to form pores. Sodium nitrate is loaded with a simple impregnation method to increase the adsorption rate of MgO and capacity, generate MgSiO3 to enhance cycle stability.
It achieves high carbon dioxide adsorption rate, high adsorption capacity and cycle stability, reduces adsorbent costs, simplifies the preparation process, and is suitable for industrial applications.
Smart Images

Figure CN118949911A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon dioxide adsorbents, and in particular to a kaolin-based magnesium oxide carbon dioxide adsorbent and a preparation method thereof. Background Art
[0002] The existing mature CO2 capture technology mainly uses chemical washing technology of liquid amine solution. The operating temperature of this technology is limited to low temperature environment (<100℃), the liquid amine solution used is extremely volatile, and liquid amine causes serious corrosion to equipment pipelines, which to a certain extent limits the application of this technology at higher temperatures and in more scenarios.
[0003] In recent years, environmentally friendly, low-cost and suitable for medium and high temperature (>200℃) solid adsorbents such as CaO, MgO, Li4SiO4, Li2ZrO3, Na4SiO4, etc. have been favored by researchers. Among them, MgO has attracted extensive attention from researchers due to its high theoretical adsorption capacity (24.8mmol / g), suitable regeneration temperature (<500℃) and good thermal stability. The adsorption of CO2 by MgO is a typical gas-solid reaction, and the contact area between MgO and CO2 affects the CO2 capture effect. Studies have found that commercial MgO has a small specific surface area and few alkaline sites, which directly affect its CO2 capture performance. Therefore, increasing the specific surface area and the number of alkaline sites of MgO is not only an important method to improve the CO2 adsorption performance, but also has important academic significance and engineering application value.
[0004] At present, the way to obtain highly active MgO is to first change the magnesium precursor and preparation method to increase the contact area and the number of alkaline sites between MgO and CO2. The adsorption capacity of pure MgO obtained in this way for CO2 is still not high, and it is easy to form a hardening during the adsorption process. After multiple adsorption-desorption, the adsorption performance is significantly reduced. The MgO composite adsorbent prepared by doping inert materials or carbon materials can improve the CO2 adsorption capacity and cycle stability to a certain extent. The MgO composite adsorbent prepared by doping inert materials or carbon materials has the advantages of large specific surface area and strong surface activity, but it does not solve the problem of Mg-O bond energy limitation during MgO adsorption of CO2, so it is still far from the theoretical adsorption capacity. In recent years, the technology of molten salt doping MgO has developed rapidly. This technology is to improve the CO2 capture performance of MgO from the perspective of reducing the lattice energy of MgO.
[0005] For example: Chinese patent application number 202410142857.0 discloses a magnesium oxide-based carbon dioxide adsorbent and a preparation method thereof, wherein basic magnesium carbonate is calcined to obtain magnesium oxide powder; magnesium oxide powder is immersed in an alkali metal salt solution and then dried to obtain alkali metal-loaded magnesium oxide powder; magnesium oxide powder loaded with alkali metal is immersed in a calcium nitrate solution and then dried, calcined, and refined to obtain a magnesium oxide-based carbon dioxide adsorbent. The adsorbent of the present invention effectively improves the adsorption capacity and cycle stability of the adsorbent for carbon dioxide through the synergistic effect of magnesium oxide, sodium ions, potassium ions, manganese ions, and calcium oxide, and controls the proportion and process parameters of each component, and the removal rate of carbon dioxide is high, and the adsorbent has excellent cyclic regeneration performance; magnesium oxide is immersed in an alkali metal salt solution, which can further increase the pores of the adsorbent, which is conducive to the diffusion of carbon dioxide inside the adsorbent.
[0006] A Chinese patent with application number 202311180121.4 discloses a method for preparing molten salt-modified magnesium oxide adsorbent particles for carbon dioxide capture and its application. Magnesium chloride is used as a magnesium source and reacted with sodium bicarbonate to prepare light basic magnesium carbonate. The light basic magnesium carbonate is calcined in stages to prepare a microporous magnesium oxide precursor. Then, the microporous magnesium oxide precursor is impregnated with a mixed salt composed of nitrate and carbonate, and an alkali metal molten salt-modified magnesium oxide powder is obtained after drying. A binder is added to the powder and extruded into a granular adsorbent.
[0007] In the above methods, the CO2 adsorption capacity of MgO modified by alkali metal salts and mixed molten salts is significantly improved, but its adsorption kinetics is slow and the cycle stability is poor. In addition, the complicated preparation process of MgO precursors and MgO composite materials is a burden on economic factors such as raw material costs, manufacturing process costs, process optimization costs, and energy consumption. Summary of the invention
[0008] The purpose of the present invention is to address the above-mentioned deficiencies in the prior art and to provide a kaolin-based magnesium oxide carbon dioxide adsorbent and a preparation method thereof, which has the characteristics of high carbon dioxide adsorption rate, high adsorption capacity, high cycle stability, etc.
[0009] The method for preparing a kaolin-based magnesium oxide carbon dioxide adsorbent of the present invention comprises the following steps:
[0010] S1, dissolving kaolin in magnesium chloride hexahydrate solution or magnesium acetate solution, then dropping sodium hydroxide solution thereinto, stirring, filtering, drying, grinding and calcining to obtain φZ-MgO;
[0011] S2. Add φZ-MgO into sodium nitrate solution and stir or ultrasonicate, dry and cool to room temperature, take out and grind to obtain kaolin-based magnesium oxide carbon dioxide adsorbent.
[0012] Furthermore, the molar ratio of magnesium chloride hexahydrate or magnesium acetate to sodium hydroxide is 1:2-4.
[0013] Further, the concentration of the sodium hydroxide solution is 3-25%.
[0014] Furthermore, in φZ-MgO, the mass ratio of kaolin to MgO is 2-1:1-4.
[0015] Further, the purity of kaolin is 85-99%.
[0016] Furthermore, in step S1, the stirring time is 30 min-12 h; in step S2, the stirring or ultrasonication is performed for 30 min-12 h.
[0017] Furthermore, in step S1, the temperature is raised to 350-395°C at a heating rate of 2-10°C / min and calcined for 1h-6h.
[0018] Furthermore, the molar ratio of MgO to NaNO3 is 1:0.05-0.4.
[0019] A kaolin-based magnesium oxide carbon dioxide adsorbent prepared by the above-mentioned preparation method.
[0020] The present invention utilizes the layered structure of kaolin, and synthesizes magnesium hydroxide on kaolin by liquid phase in-situ synthesis method, then decomposes it into kaolin-based magnesium oxide material at a certain temperature, controls the heating rate to form pores, and then uses a simple impregnation method to load a certain amount of sodium nitrate.
[0021] The present invention utilizes the unique layered structure of kaolin to make magnesium oxide grow uniformly thereon, thus preventing it from sintering into blocks, solving the problem of kinetic limitation of MgO in the CO2 adsorption process, improving the speed, capacity and cycle stability of MgO in adsorbing carbon dioxide, and generating a new phase MgSiO3 after multiple cycles, further improving its cycle stability.
[0022] The invention adopts appropriate kaolin, which can not only improve the performance of the adsorbent, but also effectively reduce the cost of the adsorbent. The preparation process of the invention is fast, efficient, simple and easy to industrialize. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 X-ray powder diffraction patterns of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared in Example 1 and MgO prepared in Comparative Example 1;
[0024] Figure 2 This is the SEM image of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared in Example 1;
[0025] Figure 3 This is a graph showing the change in carbon dioxide adsorption amount of the adsorbent prepared in Example 1 over time;
[0026] Figure 4 A bar graph showing the carbon dioxide adsorption capacity of the adsorbent prepared in Example 1;
[0027] Figure 5 This is a graph showing the change in carbon dioxide adsorption capacity of the adsorbent prepared in Example 2 over time;
[0028] Figure 6 The bar graph is a graph showing the carbon dioxide adsorption amount of the adsorbents prepared in Example 2 and Comparative Example 1;
[0029] Figure 7 This is the 20 cycle performance diagram of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared in Example 2;
[0030] Figure 8 X-ray powder diffraction patterns of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared in Example 2 and MgO prepared in Comparative Example 1 after 8 adsorption and desorption cycles;
[0031] Fig. 9 A bar graph showing the carbon dioxide adsorption capacity of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared in Example 2-4;
[0032] Fig.10 This is the SEM image of MgO prepared in Comparative Example 1;
[0033] Fig.11 This is a graph showing the 20 cycle performance of MgO prepared in Comparative Example 1. DETAILED DESCRIPTION
[0034] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0035] The kaolin-based magnesium oxide carbon dioxide adsorbent prepared by the present invention comprises the following steps:
[0036] 1. Choose kaolin with a purity of 85-99%;
[0037] 2. Take a certain amount of kaolin with a purity of 85-99% in step 1 and dissolve it in a certain amount of magnesium chloride hexahydrate / magnesium acetate solution to obtain solution 1. Prepare 3-25% sodium hydroxide solution to obtain solution 2, slowly add solution 2 to solution 1, and stir for 30min-12h. Vacuum filter to obtain filter residue. The molar ratio of magnesium chloride hexahydrate / magnesium acetate to sodium hydroxide is 1:2-1:4, and the mass ratio of kaolin to theoretically prepared MgO is 2:1-1:4.
[0038] 3. Dry the filter residue from step 2 in an oven at 60-80°C, grind it into powder, and calcine it in a muffle furnace at a heating rate of 2-10°C / min to 350-395°C for 1h-6h. Record it as φZ-MgO (X:Y, mass ratio of kaolin to MgO). (φZ kaolin type number)
[0039] 4. Take a certain amount of sodium nitrate and put it into water / ethanol to prepare a sodium nitrate solution. The amount of sodium nitrate added is based on the molar ratio of MgO:NaNO3 of 1:0.05-1:0.4. Then add the φZ-MgO (X:Y) obtained in step 3 to the sodium nitrate solution and stir / ultrasound for 30min-12h, dry at 60-80℃ and cool to room temperature. After taking it out and grinding it thoroughly, a powder sample is obtained, which is recorded as φZ-MgO (X:Y, mass ratio of kaolin to MgO)-NaNO3 (A:B, molar ratio of MgO to NaNO3).
[0040] Embodiment 1:
[0041] This example prepares φ250-MgO(1:4)-NaNO3(1:0.05)-φ250-MgO(1:4)-NaNO3(1:0.05)-(1:0.4).
[0042] Take 14.2g of magnesium acetate and dissolve it in 80mL of deionized water. Select kaolin numbered φ250, take 1g of kaolin and dissolve it in the magnesium acetate solution to obtain solution 1. Then add 8g of NaOH to deionized water to 32g to obtain 25% sodium hydroxide solution 2. Slowly add solution 2 to solution 2 and stir for 6h. Vacuum filter to obtain the filter residue. Put the filter residue into an oven at 80℃ and dry it for 12h, grind it into powder, put it into a muffle furnace heated to 390℃ at a heating rate of 2℃ / min and calcine it for 3h, cool it to room temperature and take it out and record it as φ250-MgO (1:4). Take sodium nitrate with a molar ratio of MgO:NaNO3 of 1:0.05, 1:0.1, 1:0.2, 1:0.3 and 1:0.4 and put it into ethanol to prepare sodium nitrate solution. Then φ250-MgO (1:4) was added to sodium nitrate solution and ultrasonically treated for 2 hours, dried at 80°C and cooled to room temperature. After being taken out and fully ground, powdered samples were obtained, which were recorded as φ250-MgO (1:4)-NaNO3 (1:0.05), φ250-MgO (1:4)-NaNO3 (1:0.1), φ250-MgO (1:4)-NaNO3 (1:0.2), φ250-MgO (1:4)-NaNO3 (1:0.3), and φ250-MgO (1:4)-NaNO3 (1:0.4).
[0043] See attached Figure 1, is the X-ray powder diffraction spectrum of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared according to the technical scheme of this embodiment, and the results show kaolin, NaNO3 and Mg(OH)2, and no other impurity peaks appear. MgO is easily converted into Mg(OH)2 by absorbing water, and a pre-calcination process is performed before adsorbing carbon dioxide to decompose it into MgO.
[0044] See attached Figure 2 , is a SEM (scanning electron microscope) image of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared according to the technical scheme of this embodiment. It can be seen that the sample morphology is multi-layer petal-shaped, with structure, which increases the contact area between MgO and carbon dioxide, which plays an important role in improving the carbon fixation performance of MgO.
[0045] See attached Figure 3 , is the change of carbon dioxide adsorption amount over time of φ250-MgO(1:4)-NaNO3(1:0.05), φ250-MgO(1:4)-NaNO3(1:0.1), φ250-MgO(1:4)-NaNO3(1:0.2), φ250-MgO(1:4)-NaNO3(1:0.3), and φ250-MgO(1:4)-NaNO3(1:0.4) prepared according to the technical scheme of this embodiment. The adsorption rate of φ250-MgO(1:4)-NaNO3(1:0.2) is the fastest.
[0046] See attached Figure 4 , are the carbon dioxide adsorption amounts of φ250-MgO(1:4)-NaNO3(1:0.05), φ250-MgO(1:4)-NaNO3(1:0.1), φ250-MgO(1:4)-NaNO3(1:0.2), φ250-MgO(1:4)-NaNO3(1:0.3), and φ250-MgO(1:4)-NaNO3(1:0.4) prepared according to the technical scheme of this embodiment. The adsorption amount of φ250-MgO(1:4)-NaNO3(1:0.2) is the highest.
[0047] The kaolin-based magnesium oxide adsorbent provided by the present invention has excellent carbon dioxide adsorption performance, and the molar ratio of MgO:NaNO3 of the best material is 1:0.2.
[0048] Embodiment 2:
[0049] In this example, φ250-MgO(2:1)-NaNO3(1:0.2)-φ250-MgO(1:4)-NaNO3(1:0.2) is prepared.
[0050] Take 1.775g-14.2g of magnesium acetate and dissolve it in 80mL of deionized water. Select kaolin numbered φ250, take 1g of kaolin and dissolve it in the magnesium acetate solution to obtain solution 1. Then add 1-8g of NaOH to deionized water to 32g to obtain 3%-25% sodium hydroxide solution 2. Slowly add solution 2 to solution 2 and stir for 6h. Vacuum filtration to obtain the filter residue. Put the filter residue into an oven at 80℃ and dry it for 12h, grind it into powder, put it into a muffle furnace heated to 390℃ at a heating rate of 2℃ / min and calcine it for 3h, cool it to room temperature and take it out and record it as φ250-MgO (2:1), φ250-MgO (1:1), φ250-MgO (1:2), φ250-MgO (1:3) and φ250-MgO (1:4). Take the molar ratio of MgO:NaNO3 as 1:0.2 and put it into ethanol to prepare sodium nitrate solution. Then φ250-MgO(2:1), φ250-MgO(1:1), φ250-MgO(1:2), φ250-MgO(1:3) and φ250-MgO(1:4) were added to sodium nitrate solution and ultrasonicated for 2 hours, dried at 80°C and cooled to room temperature. After being taken out and fully ground, powdered samples were obtained, which were recorded as φ250-MgO(2:1)-NaNO3(1:0.2), φ250-MgO(1:1)-NaNO3(1:0.2), φ250-MgO(1:2)-NaNO3(1:0.2), φ250-MgO(1:3)-NaNO3(1:0.2), and φ250-MgO(1:4)-NaNO3(1:0.2).
[0051] See attached Figure 5 , is the change of carbon dioxide adsorption amount over time of φ250-MgO(2:1)-NaNO3(1:0.2), φ250-MgO(1:1)-NaNO3(1:0.2), φ250-MgO(1:2)-NaNO3(1:0.2), φ250-MgO(1:3)-NaNO3(1:0.2), and φ250-MgO(1:4)-NaNO3(1:0.2) prepared according to the technical scheme of this embodiment. The adsorption rate of φ250-MgO(1:4)-NaNO3(1:0.2) is still the fastest.
[0052] See attached Figure 6, are the carbon dioxide adsorption capacities of φ250-MgO(2:1)-NaNO3(1:0.2), φ250-MgO(1:1)-NaNO3(1:0.2), φ250-MgO(1:2)-NaNO3(1:0.2), φ250-MgO(1:3)-NaNO3(1:0.2), and φ250-MgO(1:4)-NaNO3(1:0.2) prepared according to the technical scheme of this embodiment. The adsorption capacity of φ250-MgO(1:4)-NaNO3(1:0.2) is the highest, exceeding 0.4g / g CO2 .
[0053] See attached Figure 7 , is the 20-cycle performance of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared according to the technical scheme of this embodiment. After 20 cycles of carbon dioxide adsorption and desorption, the carbon dioxide adsorption capacity of φ250-MgO (1:4)-NaNO3 (1:0.2) still remains at 0.2g / g CO2 .
[0054] See attached Figure 8 , is the X-ray powder diffraction pattern of φ250-MgO(1:4)-NaNO3(1:0.2) prepared according to the technical scheme of this embodiment after 8 cycles of adsorption and desorption. After 8 cycles of carbon dioxide adsorption and desorption, φ250-MgO(1:4)-NaNO3(1:0.2) generates a new phase MgSiO3. The inert carrier MgSiO3 is conducive to multiple cycles of kaolin-based magnesium oxide carbon dioxide adsorbent.
[0055] See attached Fig. 9 , 1 is the carbon dioxide adsorption capacity of φ250-MgO(1:4)-NaNO3(1:0.2) prepared repeatedly according to the technical scheme of this embodiment. The adsorption capacity of φ250-MgO(1:4)-NaNO3(1:0.2) is the highest, still exceeding 0.4g / g CO2 , specifically 0.42g / g CO2 .
[0056] The kaolin-based magnesium oxide adsorbent provided by the present invention has excellent carbon dioxide adsorption performance, and the mass ratio of Kaol:MgO of the best material is 1:4. However, the mass ratio of Kaol:MgO from 2:1 to 1:4 has a higher carbon dioxide adsorption capacity. The addition of kaolin is conducive to improving the carbon dioxide adsorption rate. Controlling the amount of kaolin added can control the balance between performance and cost.
[0057] Embodiment 3:
[0058] This example expands the experimental preparation of φ250-MgO(1:4)-NaNO3(1:0.2) by 8 times.
[0059] Take 113.6g of magnesium acetate and dissolve it in 160mL of deionized water. Select kaolin numbered φ250, take 8g of kaolin and dissolve it in the magnesium acetate solution to obtain solution 1. Then add 64g of NaOH to deionized water to 256g to obtain 25% sodium hydroxide solution 2. Slowly add solution 2 to solution 2 and stir for 6h. Vacuum filter to obtain the filter residue. Put the filter residue into an oven at 80℃ and dry it for 12h, grind it into powder, put it into a muffle furnace at a heating rate of 2℃ / min to 390℃ and calcine it for 3h, cool it to room temperature and take it out and record it as φ250-MgO (1:4). Take the molar ratio of MgO:NaNO3 as 1:0.2 and put it into ethanol to prepare sodium nitrate solution. Then, φ250-MgO (1:4) was added to sodium nitrate solution and ultrasonicated for 2 hours, dried at 80°C and cooled to room temperature. After being taken out and fully ground, a powder sample was obtained, which was recorded as K-φ250-MgO (1:4)-NaNO3 (1:0.2).
[0060] See attached Fig. 9 , K is the carbon dioxide adsorption capacity of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared by expanding the experiment by 8 times. The carbon dioxide adsorption capacity is 0.42g / g CO2 , and the adsorption capacity of the reduced preparation experiment was 0.42g / g CO2 Not much difference.
[0061] The preparation method of the kaolin-based magnesium oxide adsorbent provided by the present invention can be expanded and has industrial potential. The adsorption performance of the adsorbent remains basically unchanged.
[0062] Embodiment 4:
[0063] φ250-MgO(1:4)-NaNO3(1:0.2)-2 prepared in this example.
[0064] Take 5.08g of magnesium chloride hexahydrate and dissolve it in 80mL of deionized water. Select kaolin numbered φ250, take 1g of kaolin and dissolve it in magnesium chloride hexahydrate solution to obtain solution 1. Then add 8g of NaOH to deionized water to 32g to obtain 25% sodium hydroxide solution 2. Slowly add solution 2 to solution 2 and stir for 1h. Vacuum filter to obtain the filter residue. Put the filter residue into an oven at 80℃ and dry it for 12h, grind it into powder, put it into a muffle furnace at a heating rate of 2℃ / min to 390℃ and calcine it for 1h, cool it to room temperature and take it out and record it as φ250-MgO (1:4). Take the molar ratio of MgO:NaNO3 as 1:0.2 and put it into deionized water to prepare sodium nitrate solution. Then, φ250-MgO (1:4) was added to sodium nitrate solution and ultrasonicated for 30 minutes, dried at 80°C and cooled to room temperature. After being taken out and fully ground, a powder sample was obtained, which was recorded as K-φ250-MgO (1:4)-NaNO3 (1:0.2).
[0065] See attached Fig. 9 , 2 is the carbon dioxide adsorption capacity of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared by replacing raw materials and shortening the process. The carbon dioxide adsorption capacity is 0.37g / g CO2 The carbon dioxide adsorption capacity of φ250-MgO (1:4)-NaNO3 (1:0.2) prepared by the original process is not much different.
[0066] The preparation method of the kaolin-based magnesium oxide adsorbent provided by the present invention can replace raw materials, shorten the process, realize low cost and simplify the process, and has industrialization potential. The adsorption performance of the adsorbent remains basically unchanged.
[0067] Comparative Example 1:
[0068] MgO prepared in this example.
[0069] Take 14.2g of magnesium acetate and dissolve it in 80mL of deionized water to dissolve into solution 1. Then add 8g of NaOH to deionized water to 32g to obtain 25% sodium hydroxide solution 2. Slowly add solution 2 to solution 2 and stir for 6h. Vacuum filter to obtain the filter residue. Put the filter residue into an oven and dry it at 80℃ for 12h, grind it into powder, put it into a muffle furnace heated to 390℃ at a heating rate of 2℃ / min and calcine it for 3h, cool it to room temperature and take it out and record it as MgO. Take the molar ratio of MgO:NaNO3 as 1:0.2 and put it into ethanol to prepare a sodium nitrate solution. Then add MgO to the sodium nitrate solution and ultrasonicate it for 2h, dry it at 80℃ and cool it to room temperature, take it out and grind it thoroughly to obtain a powder sample, recorded as MgO-NaNO3 (1:0.2), referred to as MgO.
[0070] See attached Figure 1, is the X-ray powder diffraction spectrum of MgO prepared according to the technical scheme of this comparative example, the result shows NaNO3 and Mg(OH)2, and no other impurity peaks appear. MgO is easily converted into Mg(OH)2 by absorbing water, and a pre-calcination process is performed before adsorbing carbon dioxide to decompose it into MgO.
[0071] See attached Fig.10 , is a SEM (scanning electron microscope) image of MgO prepared according to the technical scheme of this comparative example. It can be seen that the sample morphology is blocky, which is significantly different from the multi-layer petal shape of φ250-MgO (1:4)-NaNO3 (1:0.2) and has no structure.
[0072] See attached Figure 5 , is the change of carbon dioxide adsorption amount of MgO prepared according to the technical scheme of this comparative example over time. The adsorption rate of MgO is not good, which is lower than that of most kaolin-based magnesium oxide carbon dioxide adsorbents.
[0073] See attached Figure 6 , is the carbon dioxide adsorption capacity of MgO prepared according to the comparative technical scheme. The adsorption capacity of MgO is not much different from that of φ250-MgO (1:4)-NaNO3 (1:0.2).
[0074] See attached Fig.11 , is the 20-cycle performance of MgO prepared according to the technical scheme of this comparative example. After 20 cycles of carbon dioxide adsorption and desorption, the carbon dioxide adsorption capacity of MgO is only 0.16g / g CO2 .
[0075] See attached Figure 8 , is the X-ray powder diffraction pattern of MgO prepared according to the comparative technical solution after 8 adsorption and desorption cycles. After 8 cycles of carbon dioxide adsorption and desorption, no new phase is generated on MgO.
[0076] Compared with the kaolin-based magnesium oxide adsorbent provided by the present invention, the comparative example MgO has a low adsorption rate and poor cycle performance. With similar adsorption performance, the kaolin-based magnesium oxide adsorbent provided by the present invention has a lower cost.
[0077] For matters not mentioned above, the prior art applies.
[0078] Although some specific embodiments of the present invention have been described in detail through examples, those skilled in the art should understand that the above examples are for illustration only and are not intended to limit the scope of the present invention. Those skilled in the art to which the present invention belongs may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but they will not deviate from the direction of the present invention or exceed the scope defined by the attached claims. Those skilled in the art should understand that any modifications, equivalent substitutions, improvements, etc. made to the above embodiments based on the technical essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a kaolin-based magnesium oxide carbon dioxide adsorbent, characterized in that: The following steps are involved: S1, dissolving kaolin in magnesium chloride hexahydrate solution or magnesium acetate solution, then dropping sodium hydroxide solution thereinto, stirring, filtering, drying, grinding and calcining to obtain φZ-MgO; S2. Add φZ-MgO into sodium nitrate solution and stir or ultrasonicate, dry and cool to room temperature, take out and grind to obtain kaolin-based magnesium oxide carbon dioxide adsorbent.
2. The preparation method according to claim 1, characterized in that: The molar ratio of magnesium chloride hexahydrate or magnesium acetate to sodium hydroxide is 1:2-4.
3. The preparation method according to claim 1, characterized in that: The concentration of the sodium hydroxide solution is 3-25%.
4. The preparation method according to claim 1, characterized in that: In φZ-MgO, the mass ratio of kaolin to MgO is 2-1:1-4.
5. The preparation method according to claim 1, characterized in that: The purity of kaolin is 85-99%.
6. The preparation method according to claim 1, characterized in that: In step S1, the stirring time is 30 min-12 h; in step S2, the stirring or ultrasonication is performed for 30 min-12 h.
7. The preparation method according to claim 1, characterized in that: In step S1, the temperature is raised to 350-395°C at a heating rate of 2-10°C / min and calcined for 1h-6h.
8. The preparation method according to claim 1, characterized in that: The molar ratio of MgO and NaNO3 is 1:0.05-0.
4.
9. A kaolin-based magnesium oxide carbon dioxide adsorbent prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Method for preparing modified attapulgite clay adsorbing material
CN102019166A
CO2 absorbent as well as preparation method and application method thereof
CN105664708A
Preparation method of calcium-based carbon dioxide adsorbent
CN113856617A
Synthesis of co2-one adsorbent for co2 removal
US20150209758A1
Carbon dioxide absorbent, and preparation method thereof
WO2013048191A2