Manufacturing method of large-specification steel strand steel with uniform cleaning rod performance
By using high-line rolling and segmented Steyrmo air-cooled line cooling technology in steel strand production, the parameters of the air-cooling process are adjusted, and the problem of large fluctuations in the wire stranding performance is solved, and high The uniform performance production of large-scale steel strands with strength reduces production costs.
Patent Information
- Application Number
- CN202411166728.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-23
AI Technical Summary
When the prior art, when producing high-strength, large-size steel strands, the uneven cooling caused by the air-cooling and cooling process leads to large fluctuations in the structure and mechanical properties. How to reduce the fluctuations in the through-bar performance is a difficult problem.
Using high-line rolling and segmented Steyrmo air-cooled line cooling technology with lower production costs, the uniform cooling of wires is achieved by adjusting the fan air volume, roller speed, Jialing device opening angle and insulation cover switch, and the uniform cooling of wires is achieved and controlled. Temperature changes during air cooling.
It effectively reduces the fluctuations in the performance of the strip, meets the production of Φ21.8mm specification and strength of 1960MPa grade steel strands. The process operation is simple, the production cost is low, and it is easy to promote industrially.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of steel rolling, and in particular to a method for manufacturing steel for large-size steel strands with uniform pass rod performance. Background Art
[0002] High carbon steel wire is one of the typical steel grades among drawn materials. It has high strength and toughness. It is an important raw material for producing high-strength, large-size prestressed steel strands and high-strength, low-relaxation prestressed steel wires. It is widely used in public infrastructure, energy, marine engineering and other fields.
[0003] At present, some steel enterprises develop products with higher strength levels by upgrading equipment, such as adding lead bath, salt bath, water bath and other equipment, and developing ultra-fast cooling + isothermal troostitizing treatment technology to obtain products with high troostitizing rate, small performance fluctuation and good strength and toughness matching performance. However, the capital investment of these equipments is huge, and it also increases the production cost and the risk of environmental pollution. For now, most of the controlled cooling process of high-carbon steel wire rods adopts the Stelmor air-cooled line with low production cost. The control of organizational properties can fully meet the production of raw materials for 1860MPa grade steel strands with specifications of Φ21.8mm and below. Through chemical composition design and microalloying technology, it can also fully meet the production of raw materials for 1960MPa grade steel strands with specifications of Φ21.8mm and below. However, the disadvantage of the air-cooled controlled cooling process is that as the strength increases, the fluctuations in the organization and mechanical properties become more obvious due to the uneven cooling caused by the temperature difference between the head / middle / tail and the overlapping / non-overlapping positions of the rolled material. How to bring into play the "waste heat" of the Stelmor air-cooled line, reasonably control and reduce the fluctuations in the wire rod spinning temperature and the key process parameters of the air-cooled line, and reduce the fluctuations in the performance of the wire rod are issues that need to be resolved.
[0004] Therefore, there is a need in the prior art for improving large-size steel strands with uniform cleaning rod performance and a method for manufacturing the same. Summary of the invention
[0005] In view of this, the purpose of an embodiment of the present invention is to propose a method for manufacturing large-size steel strands with uniform wire rod performance, using high-wire rolling and Stelmor air-cooling line staged cooling control process with lower production costs, controlling the wire rod temperature during the air cooling process, and solving the problem of large fluctuations in wire rod performance.
[0006] Based on the above purpose, the embodiment of the present invention provides a method for manufacturing large-size steel strand with uniform performance, and the production process is: heating of wire billet → high-pressure water dephosphorization → rough rolling, intermediate rolling, finishing rolling and water tank controlled cooling → wire laying → Stelmor air-cooled line controlled cooling → coiling → PF chain transportation → finishing, wherein the segmented Stelmor air-cooled line controlled cooling is adopted, including: The first stage of controlled cooling temperature changes from 890±10℃ to 650±10℃, the initial roller speed is 0.56~0.58m / s, and increases by 0.04m / s step by step. The maximum air volume of the fan is 200,000m 3 / h, opening degree 100%, wire overlap / non-overlap cooling rate is 8-10℃ / s, Jialing device opening angle is 3-5 degrees, and the insulation cover is opened; The second stage of controlled cooling temperature changes from 650±10℃ to 590±10℃, the roller speed increases by 0.02m / s step by step, and the maximum air volume of the fan is 155,000m 3 / h, the opening degree is 90% to 95%, the wire overlap / non-overlap cooling rate is 3 to 5°C / s, the opening angle of the Jialing device is 0 to 2 degrees, and the insulation cover is opened; In the third stage, the controlled cooling temperature changes from 590±10℃ to 450±10℃, the roller speed increases by 0.01m / s step by step, the fan is turned off, the insulation cover is all closed, and the wire overlap / non-overlap cooling speed is 1-2℃ / s; The fourth stage of controlled cooling temperature is changed from 450±10℃ to room temperature, and cooled naturally.
[0007] In some embodiments, the chemical composition of the wire for steel strand includes, by weight percentage: C 0.84% to 0.87%, Si 0.50% to 0.60%, Mn 0.60% to 0.80%, P≤0.015%, S≤0.010%, Cr 0.25% to 0.35%, Cu≤0.20%, Ni≤0.10%, and the rest is Fe and unavoidable impurities.
[0008] In some embodiments, the carbon segregation degree at the center of the billet used for the wire is ≤1.10.
[0009] In some embodiments, during the wire billet heating stage, the soaking temperature is 1080-1150° C., and the heating time t=(0.7-1.2)H, wherein H is the billet thickness in mm, and the heating time t is in min.
[0010] In some embodiments, in the high-pressure water dephosphorization stage, the dephosphorization water pressure is 15-20 MPa.
[0011] In some embodiments, during the rolling and water tank controlled cooling stages, the temperature difference of the rolled piece after the fourth stand of rough rolling is controlled at ≤20°C throughout the length, and the temperature before final rolling is 870±10°C.
[0012] In some embodiments, the water tank opening degree before final rolling is ≥25%, and the water volume in the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, water tank opening degree after final rolling ≤5%.
[0013] In some embodiments, the spinning temperature is controlled to be 890±10°C, and the temperature difference along the length of the wire is ≤10°C.
[0014] In some embodiments, the spinning machine has an inclination angle of 20°, a vibration value of the spinning machine ≤ 0.5 mm / s, and a spinning speed of 29-31 m / s.
[0015] In some embodiments, a walking beam furnace is used to heat the blank.
[0016] The present invention has at least the following beneficial technical effects: The high-wire rolling + Stelmor air-cooling wire controlled cooling process with lower production cost is adopted, and the air volume of the fan, roller speed, opening angle of the Jialing device and opening / closing of the insulation cover are adjusted to realize staggered segmented cooling. The problem of large fluctuations in wire rod performance is solved through chemical composition design and temperature control of wire rods in the rolling and air-cooling processes. The high-carbon steel wire can meet the production of Φ21.8mm specification and 1960MPa strength steel strand. The process operation is simple, the production cost is low, and it is easy to promote and apply industrially. DETAILED DESCRIPTION
[0017] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in conjunction with specific embodiments.
[0018] The terms "including" and "having" and any variations thereof in the specification and claims of the present invention are intended to cover non-exclusive inclusions; the terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish different objects rather than to describe a specific order. "Multiple" means two or more, unless otherwise clearly and specifically defined.
[0019] In addition, reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0020] The present invention provides a method for manufacturing large-size steel strands with uniform performance. The production process is as follows: heating of wire billets → high-pressure water dephosphorization → rough rolling, intermediate rolling, finishing rolling and water tank controlled cooling → spinning → Stelmore air-cooled line controlled cooling → coiling → PF chain transportation → finishing. Among them, the Stelmore air-cooled line has segmented controlled cooling: by adjusting the roller speed before and after the drop section, the opening angle of the Jialing device, the opening degree of the fan, and the opening / closing of the insulation cover, the wire is uniformly cooled and its structure and performance are reasonably controlled. Specifically, it includes the following stages: The first stage of controlled cooling temperature changes from 890±10℃ to 650±10℃, the initial roller speed is 0.56~0.58m / s, and increases by 0.04m / s step by step. The maximum air volume of the fan is 20.0m 3 / h, opening degree 100%, wire overlap / non-overlap cooling rate is 8-10℃ / s, Jialing device opening angle is 3-5 degrees, and the insulation cover is opened; The second stage of controlled cooling temperature changes from 650±10℃ to 590±10℃, the roller speed increases by 0.02m / s step by step, and the maximum air volume of the fan is 155,000m 3 / h, the opening degree is 90% to 95%, the wire overlap / non-overlap cooling rate is 3 to 5°C / s, the opening angle of the Jialing device is 0 to 2 degrees, and the insulation cover is opened; In the third stage, the controlled cooling temperature changes from 590±10℃ to 450±10℃, the roller speed increases by 0.01m / s step by step, the fan is turned off, the insulation cover is all closed, and the wire overlap / non-overlap cooling speed is 1-2℃ / s; The fourth stage of controlled cooling temperature is changed from 450±10℃ to room temperature, and cooled naturally.
[0021] Furthermore, the chemical composition of the steel strand wire is as follows by weight: C 0.84% to 0.87%, Si 0.50% to 0.60%, Mn 0.60% to 0.80%, P≤0.015%, S≤0.010%, Cr 0.25% to 0.35%, Cu≤0.20%, Ni≤0.10%; the rest is Fe and unavoidable impurities.
[0022] Furthermore, the rolled billet: the central carbon segregation degree of the billet used for the steel strand wire is ≤1.10.
[0023] Further, the billet is heated: the soaking temperature is 1080-1150°C, and the heating time is t= (0.7-1.2)H, wherein H is the billet thickness in mm, and the heating time t is in min.
[0024] Furthermore, high-pressure water dephosphorization: the dephosphorization water pressure is 15-20MPa, and there shall be no residual iron oxide scale visible to the naked eye on the surface of the blank after dephosphorization.
[0025] Furthermore, in the rough, medium and finish rolling and water tank controlled cooling process, the temperature difference of the rolled piece after the fourth rough rolling stand is controlled at ≤20℃; the water tank opening degree before final rolling is ≥25%, and the water inlet volume of the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, temperature before final rolling is 870±10℃; water tank opening degree after final rolling is ≤5%.
[0026] Furthermore, in the spinning process, the spinning temperature is controlled to be 890±10°C, and the temperature difference of the wire along its entire length is ≤10°C; the spinning machine has an inclination angle of 20°, a vibration value of ≤0.5mm / s, and a spinning speed of 29-31m / s to ensure the stability of the coil shape.
[0027] The high carbon steel wire produced by the above method is cut into 8 sections in the same circle, the tensile strength range of the same circle is ≤30MPa, the tensile strength range of the wire rod is ≤40MPa, the troostitizing rate is ≥90%, the core network cementite is ≤1.0 level, there is no core martensite quenching structure, and the strength of the finished steel strand is 1990-2050MPa.
[0028] The present invention will be further explained below in conjunction with specific embodiments.
[0029] Example 1 A metal products company adopts the technology of the present invention to prepare Φ14.0mm high-carbon steel strand steel, and its production process is: billet heating → high-pressure water dephosphorization → rough, medium and fine rolling and water tank controlled cooling → wire laying → Stelmor air-cooled wire controlled cooling → coiling → PF chain transportation → finishing.
[0030] The chemical composition of steel strand wire by weight percentage is: C 0.84%, Si 0.60%, Mn 0.71%, P 0.012%, S0.008%, Cr 0.28%, Cu 0.04%, Ni 0.03%, and the rest is Fe and unavoidable impurities.
[0031] The central carbon segregation degree of the billet used for steel strand wire is 1.08.
[0032] The raw materials were placed in a walking beam heating furnace for heating, the soaking section temperature was 1130°C, the ingot thickness was 200 mm, and the heating time was 210 min.
[0033] After being taken out of the furnace, the hot billets are subjected to high-pressure water dephosphorization. The dephosphorization water pressure is 18MPa. After dephosphorization, no iron oxide scale remains on the surface with the naked eye.
[0034] The temperature difference of the rolled piece after the 4th rough rolling stand is 18℃. The opening degree of the 1#~4# water tanks before final rolling is 25%, 28%, 28% and 30% respectively, and the water inflow of the water tank is 50, 55, 55 and 55m3 respectively. 3 / h, the outlet water pressure is 3.5, 3.8, 3.8, 4.0bar; the temperature before final rolling is 873℃; after final rolling, the opening degree of 5# water tank is 3%, the wire drawing temperature is 887℃, and the temperature difference of the wire along its length is 8℃.
[0035] The hot rolled wire is continuously and evenly laid on the moving roller table through the laying machine. The laying machine has an inclination angle of 20°, a vibration value of 0.4mm / s, a laying speed of 29m / s, a coil diameter of 1075mm, and a stable coil shape.
[0036] The total length of the air-cooled line is 105 meters, and the air-cooled roller is divided into 13 sections. The first section of the roller is shorter and there is no fan underneath it. There are two fans under each of the remaining sections. Each fan has a Jialing device for adjusting the air volume ratio between the overlapping and non-overlapping positions of the wire. There are a total of 8 sections of drops after sections 3, 4, 5, 6, 7, 9, 11, and 12 of the air-cooled roller.
[0037] The controlled cooling process of hot rolled wire adopts Stelmor air cooling and segmented cooling: (1) 887℃-649℃, beginning of the first stage to the end of the third stage, the initial roller speed is 0.56m / s, the roller speed increases by 0.04m / s step by step, and the maximum air volume of the fan is 200,000m 3 / h, the Jialing device under the fan is opened at an angle of 3°, the opening degree of 1#-4# fans is 100%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling speeds of the wires are 8℃ / s and 10℃ / s respectively; (2) 649℃-588℃, the roller speed at the beginning of the 4th stage to the middle of the 5th stage and the end of the 3rd stage is 0.68m / s, and the roller speed increases by 0.02m / s in each stage. The maximum air volume of the 5#-6# fans is 200,000m3 / h, and the maximum air volume of the 7# fan is 155,000m3 / h. 3 / h, the opening angle of the Jialing device under the fan is 2°, the opening degree of 5#-6# fans is 95%, the opening degree of 7# fan is 90%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling speed of the wire is 3℃ / s and 4℃ / s respectively; (3) 588℃-450℃, from the middle of the 5th stage to the end of the 13th stage, the roller speed at the end of the 5th stage is 0.7m / s, and the roller speed increases by 0.01m / s in each stage. All fans are turned off, all insulation covers are turned off, and the overlapping / non-overlapping cooling speed of the wire is 1℃ / s; (4) Then roll up and let cool naturally.
[0038] The high carbon steel wire produced by the above method was analyzed by taking the head / middle / tail circle, and each circle of wire was cut into 8 uniform equal parts. The range of tensile strength of the same circle was 25MPa, the range of tensile strength of the wire rod was 38MPa, the troostitization rate was 92%, the network cementite was level 1.0, and the core martensite was level 0.5. The tensile strength of the finished Φ21.8mm steel strand produced by this furnace ranged from 1190 to 2025MPa, and the performance fluctuation of the steel strand was small.
[0039] Example 2 A metal products company adopts the technology of the present invention to prepare Φ14.0mm high-carbon steel strand steel, and its production process is: billet heating → high-pressure water dephosphorization → rough, medium and fine rolling and water tank controlled cooling → wire laying → Stelmor air-cooled wire controlled cooling → coiling → PF chain transportation → finishing.
[0040] The chemical composition of steel strand wire by weight percentage is: C 0.87%, Si 0.50%, Mn 0.60%, P 0.015%, S0.010%, Cr 0.25%, Cu 0.04%, Ni 0.03%, and the rest is Fe and unavoidable impurities.
[0041] The carbon segregation degree at the center of the billet used for steel strand wire is 1.05.
[0042] The raw materials were placed in a walking beam heating furnace for heating, the soaking section temperature was 1150°C, the ingot thickness was 200 mm, and the heating time was 240 min.
[0043] After being taken out of the furnace, the hot billet is subjected to high-pressure water dephosphorization. The dephosphorization water pressure is 20MPa. After dephosphorization, no iron oxide scale is left on the surface with the naked eye.
[0044] The temperature difference of the rolled piece after the 4th rough rolling stand is 10℃. The opening degree of the 1#~4# water tanks before final rolling is 25%, 28%, 28% and 30% respectively, and the water inflow of the water tank is 50, 55, 55 and 55m3 respectively. 3 / h, the outlet water pressure is 3.5, 3.8, 3.8, 4.0bar; the temperature before final rolling is 860℃; after final rolling, the opening degree of 5# water tank is 1%, the wire drawing temperature is 888℃, and the temperature difference of the wire along its length is 10℃.
[0045] The hot rolled wire is continuously and evenly laid on the moving roller table through the laying machine. The laying machine has an inclination angle of 20°, a vibration value of 0.2mm / s, a laying speed of 30m / s, a coil diameter of 1075mm, and a stable coil shape.
[0046] The total length of the air-cooled line is 105 meters, and the air-cooled roller is divided into 13 sections. The first section of the roller is shorter and there is no fan underneath it. There are two fans under each of the remaining sections. Each fan has a Jialing device for adjusting the air volume ratio between the overlapping and non-overlapping positions of the wire. There are a total of 8 sections of drops after sections 3, 4, 5, 6, 7, 9, 11, and 12 of the air-cooled roller.
[0047] The controlled cooling process of hot rolled wire adopts Stelmor air cooling and segmented cooling: (1) 888℃-650℃, from the beginning of the first stage to the end of the third stage, the initial roller speed is 0.56m / s, the roller speed increases by 0.04m / s stage by stage, the maximum air volume of the fan is 200,000m3 / h, the opening angle of the Jialing device under the fan is 5°, the opening degree of 1#-4# fans is 100%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling rates of the wire are 8℃ / s and 9℃ / s respectively; (2) 650℃-591℃, the roller speed at the beginning of the 4th section to the middle of the 5th section and the end of the 3rd section is 0.68m / s, and the roller speed increases by 0.02m / s in each section. The maximum air volume of the 5#-6# fans is 200,000m3 / h, and the maximum air volume of the 7# fan is 155,000m3 / h. The opening angle of the Jialing device under the fan is 2°, the opening degree of the 5#-6# fans is 95%, and the opening degree of the 7# fan is 90%. The insulation cover is fully opened, and the overlapping / non-overlapping cooling rates of the wire are 3℃ / s and 3℃ / s respectively; (3) 591℃-440℃, from the middle of the 5th stage to the end of the 13th stage, the roller speed at the end of the 5th stage is 0.7m / s, and the roller speed increases by 0.01m / s in each stage. All fans are turned off, all insulation covers are turned off, and the overlapping / non-overlapping cooling speed of the wire is 2℃ / s; (4) Then roll up and let cool naturally.
[0048] The high carbon steel wire produced by the above method was analyzed by taking the head / middle / tail circle, and each circle of wire was cut into 8 uniform equal parts. The range of tensile strength of the same circle was 30MPa, the range of tensile strength of the wire rod was 40MPa, the troostitization rate was 95%, the network cementite was level 1.0, and the core martensite was level 0. The tensile strength of the finished Φ21.8mm steel strand produced by the furnace ranged from 2019 to 2050MPa, and the performance fluctuation of the steel strand was small.
[0049] Example 3 A metal products company adopts the technology of the present invention to prepare Φ14.0mm high-carbon steel strand steel, and its production process is: billet heating → high-pressure water dephosphorization → rough, medium and fine rolling and water tank controlled cooling → wire laying → Stelmor air-cooled wire controlled cooling → coiling → PF chain transportation → finishing.
[0050] The chemical composition of steel strand wire by weight percentage is: C 0.85%, Si 0.55%, Mn 0.80%, P 0.008%, S0.008%, Cr 0.35%, Cu 0.05%, Ni 0.03%, and the rest is Fe and unavoidable impurities.
[0051] The central carbon segregation degree of the billet used for steel strand wire is 1.10.
[0052] The raw materials were placed in a walking beam heating furnace for heating, the soaking section temperature was 1100°C, the ingot thickness was 200 mm, and the heating time was 180 min.
[0053] After being taken out of the furnace, the hot billets are subjected to high-pressure water dephosphorization. The dephosphorization water pressure is 15MPa. After dephosphorization, no iron oxide scale is visible on the surface with the naked eye.
[0054] The temperature difference of the rolled piece after the 4th rough rolling stand is 15℃. The opening degree of the 1#~4# water tanks before final rolling is 25%, 28%, 28% and 30% respectively, and the water inflow of the water tank is 50, 55, 55 and 55m3 respectively. 3 / h, the outlet water pressure is 3.5, 3.8, 3.8, 4.0bar; the temperature before final rolling is 880℃; after final rolling, the opening degree of 5# water tank is 5%, the wire drawing temperature is 892℃, and the temperature difference of the wire along its length is 8℃.
[0055] The hot rolled wire is continuously and evenly laid on the moving roller table through the laying machine. The laying machine has an inclination angle of 20°, a vibration value of 0.4mm / s, a laying speed of 29m / s, a coil diameter of 1075mm, and a stable coil shape.
[0056] The total length of the air-cooled line is 105 meters, and the air-cooled roller is divided into 13 sections. The first section of the roller is shorter and there is no fan underneath it. There are two fans under each of the remaining sections. Each fan has a Jialing device for adjusting the air volume ratio between the overlapping and non-overlapping positions of the wire. There are a total of 8 sections of drops after sections 3, 4, 5, 6, 7, 9, 11, and 12 of the air-cooled roller.
[0057] The controlled cooling process of hot rolled wire adopts Stelmor air cooling and segmented cooling: (1) 892℃-655℃, beginning of the first stage to the end of the third stage, the initial roller speed is 0.56m / s, the roller speed increases by 0.04m / s step by step, and the maximum air volume of the fan is 200,000m 3 / h, the Jialing device under the fan is opened at an angle of 4°, the opening degree of 1#-4# fans is 100%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling speeds of the wires are 9℃ / s and 9℃ / s respectively; (2) 655℃-578℃, the roller speed at the beginning of the 4th stage to the middle of the 5th stage, and the end of the 3rd stage is 0.68m / s, and the roller speed increases by 0.02m / s in each stage. The maximum air volume of the 5#-6# fan is 200,000m 3 / h, the maximum air volume of 7# fan is 155,000 m3 / h, the opening angle of the Jialing device under the fan is 1°, the opening degree of 5#-6# fans is 95%, the opening degree of 7# fan is 90%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling speeds of the wire are 3℃ / s and 4℃ / s respectively; (3) 578℃-451℃, from the middle of the 5th stage to the end of the 13th stage, the roller speed at the end of the 5th stage is 0.7m / s, and the roller speed increases by 0.01m / s in each stage. All fans are turned off, all insulation covers are turned off, the overlapping cooling speed of the wire is 1℃ / s, and the non-overlap cooling speed is 2℃ / s; (4) Then roll up and let cool naturally.
[0058] The high carbon steel wire produced by the above method was analyzed by taking the head / middle / tail circle, and each circle of wire was cut into 8 uniform equal parts. The range of tensile strength of the same circle was 20MPa, the range of tensile strength of the wire rod was 39MPa, the troostitization rate was 93%, the network cementite was level 0, and the core martensite was level 0.5. The tensile strength of the finished Φ21.8mm steel strand produced by the furnace ranged from 2002 to 2038MPa, and the performance fluctuation of the steel strand was small.
[0059] Example 4 A metal products company adopts the technology of the present invention to prepare Φ14.0mm high-carbon steel strand steel, and its production process is: billet heating → high-pressure water dephosphorization → rough, medium and fine rolling and water tank controlled cooling → wire laying → Stelmor air-cooled wire controlled cooling → coiling → PF chain transportation → finishing.
[0060] The chemical composition of wire steel for steel strands is as follows by weight: C 0.86%, Si 0.52%, Mn 0.75%, P0.011%, S 0.009%, Cr 0.30%, Cu 0.04%, Ni 0.03%, and the rest is Fe and unavoidable impurities.
[0061] The central carbon segregation degree of the billet used for steel strand wire is 1.09.
[0062] The raw materials were placed in a walking beam heating furnace for heating, the soaking section temperature was 1080°C, the ingot thickness was 200 mm, and the heating time was 140 min.
[0063] After being taken out of the furnace, the hot billets are subjected to high-pressure water dephosphorization. The dephosphorization water pressure is 16MPa. After dephosphorization, no iron oxide scale remains on the surface with the naked eye.
[0064] The temperature difference of the rolled piece after the 4th rough rolling stand is 20℃. The opening degree of the 1#~4# water tanks before final rolling is 25%, 28%, 28% and 30% respectively, and the water inflow of the water tank is 50, 55, 55 and 55m3 respectively. 3 / h, the outlet water pressure is 3.5, 3.8, 3.8, 4.0bar; the temperature before final rolling is 870℃; after final rolling, the opening degree of 5# water tank is 0%, the wire drawing temperature is 900℃, and the temperature difference of the wire along its length is 10℃.
[0065] The hot rolled wire is continuously and evenly laid on the moving roller table through the laying machine. The laying machine has an inclination angle of 20°, a vibration value of 0.5mm / s, a laying speed of 31m / s, a coil diameter of 1075mm, and a stable coil shape.
[0066] The total length of the air-cooled line is 105 meters, and the air-cooled roller is divided into 13 sections. The first section of the roller is shorter and there is no fan underneath it. There are two fans under each of the remaining sections. Each fan has a Jialing device for adjusting the air volume ratio between the overlapping and non-overlapping positions of the wire. There are a total of 8 sections of drops after sections 3, 4, 5, 6, 7, 9, 11, and 12 of the air-cooled roller.
[0067] The controlled cooling process of hot rolled wire adopts Stelmor air cooling and segmented cooling: (1) 900℃-660℃, beginning of the first stage to the end of the third stage, the initial roller speed is 0.56m / s, the roller speed increases by 0.04m / s step by step, and the maximum air volume of the fan is 200,000m 3 / h, the Jialing device under the fan is opened at an angle of 3°, the opening degree of 1#-4# fans is 100%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling speeds of the wires are 9℃ / s and 10℃ / s respectively; (2) 660℃-600℃, the roller speed at the beginning of the 4th stage to the middle of the 5th stage, and the end of the 3rd stage is 0.68m / s, and the roller speed increases by 0.02m / s in each stage. The maximum air volume of the 5#-6# fan is 200,000m 3 / h, maximum air volume of 7# fan is 155,000 m 3 / h, the opening angle of the Jialing device under the fan is 0°, the opening degree of 5#-6# fans is 95%, the opening degree of 7# fan is 90%, the insulation cover is fully opened, and the overlapping / non-overlapping cooling speed of the wire is 4℃ / s and 5℃ / s respectively; (3) 600℃-460℃, from the middle of the 5th stage to the end of the 13th stage, the roller speed at the end of the 5th stage is 0.7m / s, and the roller speed increases by 0.01m / s in each stage. All fans are turned off, all insulation covers are turned off, and the overlapping / non-overlapping cooling speed of the wire is 1℃ / s; (4) Then roll up and let cool naturally.
[0068] The high carbon steel wire produced by the above method was analyzed by taking the head / middle / tail circle, and each circle of wire was cut into 8 uniform equal parts. The range of tensile strength of the same circle was 30MPa, the range of tensile strength of the wire rod was 39MPa, the troostitization rate was 90%, the network cementite was level 1.0, and the core martensite was level 0.5. The tensile strength of the finished Φ21.8mm steel strand produced by this furnace ranged from 2012 to 2046MPa, and the performance fluctuation of the steel strand was small.
[0069] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope disclosed in the embodiments of the present invention as defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0070] It should be understood that, as used herein, the singular forms "a", "an" are intended to include the plural forms as well, unless the context clearly supports an exception. It should also be understood that, as used herein, "and / or" refers to any and all possible combinations including one or more of the associated listed items.
[0071] The serial numbers of the embodiments disclosed in the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0072] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for manufacturing large-size steel strand with uniform performance of wire rods, the production process is: heating of wire billet → high-pressure water dephosphorization → rough rolling, intermediate rolling, finishing rolling and water tank controlled cooling → spinning → Stelmor air-cooled wire controlled cooling → coiling → PF chain transportation → finishing, characterized in that: Adopt segmented Stelmore air-cooled line-controlled cooling, including: The first stage of controlled cooling temperature changes from 890±10℃ to 650±10℃, the initial roller speed is 0.56~0.58m / s, and increases by 0.04m / s step by step. The maximum air volume of the fan is 200,000m 3 / h, opening degree 100%, cooling rate of wire overlap / non-overlap position is 8-10℃ / s, opening angle of Jialing device is 3-5 degrees, and insulation cover is opened; The second stage of controlled cooling temperature changes from 650±10℃ to 590±10℃, the roller speed increases by 0.02m / s step by step, and the maximum air volume of the fan is 155,000m 3 / h, the opening degree is 90% to 95%, the cooling rate of the wire overlap / non-overlap position is 3 to 5°C / s, the opening angle of the Jialing device is 0 to 2 degrees, and the insulation cover is opened; In the third stage, the controlled cooling temperature changes from 590±10℃ to 450±10℃, the roller speed increases by 0.01m / s step by step, the fan is turned off, the insulation cover is all closed, and the cooling speed of the wire overlap / non-overlap position is 1-2℃ / s; The fourth stage of controlled cooling temperature is changed from 450±10℃ to room temperature, and cooled naturally.
2. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: Calculated by weight percentage, the chemical composition of steel strand wire includes: C: 0.84% ~ 0.87%, Si: 0.50% ~ 0.60%, Mn: 0.60% ~ 0.80%, P ≤ 0.015%, S ≤ 0.010%, Cr 0.25% ~ 0.35%, Cu ≤ 0.20%, Ni ≤ 0.10%, and the rest is Fe and unavoidable impurities.
3. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: The central carbon segregation degree of the blank used for the wire rod is ≤1.
10.
4. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: In the wire billet heating stage, the soaking temperature is 1080-1150° C., and the heating time t=(0.7-1.2)H, wherein H is the billet thickness in mm, and the heating time t is in min.
5. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: In the high-pressure water dephosphorization stage, the dephosphorization water pressure is 15-20MPa.
6. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: During the rolling and water tank controlled cooling stage, the temperature difference of the rolled piece after the 4th stand of rough rolling is controlled at ≤20℃, and the temperature before final rolling is 870±10℃.
7. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: The opening degree of the water tank before final rolling is ≥25%, and the water volume in the water tank is ≥50m 3 / h, outlet water pressure ≥3.5bar, water tank opening degree after final rolling ≤5%.
8. The method for manufacturing large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: The spinning temperature is controlled at 890±10℃, and the temperature difference along the entire length of the wire is ≤10℃.
9. The method for manufacturing a large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: The inclination angle of the spinning machine is 20°, the vibration value of the spinning machine is ≤0.5mm / s, and the spinning speed is 29-31m / s.
10. The method for manufacturing large-size steel strand with uniform cleaning rod performance according to claim 1, characterized in that: The billet is heated by a walking beam heating furnace.
Citation Information
Patent Citations
Stelmor air cooling and line-controlled cooling production method for HRB400(E) deformed steel bar with yield strength larger than or equal to 420 MPa
CN111893279A
Method for controlling martensite and grain boundary cementite at center of 82B hot-rolled wire rod
CN112080618A
Preparation method of aging-free 82B hot-rolled wire rod
CN112126760A
Large-specification high-strength SWRH82B wire rod multi-section controlled cooling process method based on multi-target regulation and control
CN117286416A
Production process of steel DL75 hot-rolled wire rod for cable steel strand
CN118326233A
Cited By
5500MPa-grade diamond wire bus steel wire and production method thereof
CN121732601A