Preparation method of hot stamping part
Laser heating and air knife blowing flattening or blowing away the raised burrs on the surface of hot stamping parts, the problem of burrs affecting electroplating and electrophoresis during the molding process is solved, and the coating quality and corrosion resistance are improved.
Patent Information
- Application Number
- CN202410981602.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Hot stamping parts are prone to form protruding burrs during the molding process, resulting in uneven thickness of the electroplating coating and affecting corrosion resistance.
The protruding burrs on the surface of the hot stamping part are heated and blown flattened, or the slag produced by the heat is blown away, and then electroplating and electrophoresis are performed.
Effectively reduce the height of the raised burrs, improve the coating quality in the electroplating and electrophoresis steps, and optimize the corrosion resistance of hot stamping parts.
Smart Images

Figure CN118950792A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hot stamping surface treatment, and in particular relates to a method for preparing hot stamping parts. Background Art
[0002] At present, the hot stamping industry generally adopts several processes, including bare plate hot stamping, aluminum silicon coating hot stamping, galvanized plate hot stamping and bare plate hot stamping followed by electrogalvanizing. Among them, bare plates are prone to produce a large amount of oxide scale, and in the hot stamping process, due to the tensile deformation of the parts, they are also easy to adhere to the mold to form nodules. Nodules and oxide scales will cause serious damage to the bare plate, especially the side wall and R corner positions, and the raised burrs produced at the damaged position will affect the coating thickness of the hot stamping parts electrophoresis, which will then cause the corrosion resistance of the damaged position to be worse than that of the undamaged position. Summary of the invention
[0003] In view of the above-mentioned problems existing in the prior art, the main purpose of the present invention is to provide a method for preparing hot stamping parts, by heating and flattening the raised burrs on the surface of the hot stamping parts, or / and blowing away the slag generated by the heating of the raised burrs, thereby improving the quality of the surface coating of the hot stamping parts and optimizing the corrosion resistance of the hot stamping parts.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] The present invention provides a method for preparing a hot stamping part, and the method for preparing the hot stamping part comprises:
[0006] Hot stamping is performed on a bare plate blank to form it into a hot stamping part, wherein raised burrs are formed on the surface of the hot stamping part;
[0007] Heating the raised burrs on the surface of the hot stamping part, and flattening the raised burrs softened by the heat, or / and blowing off the slag generated by the raised burrs when heated;
[0008] After the raised burrs softened by heat are flattened, or / and the slag generated by the raised burrs being heated is blown off, the hot stamping parts are electroplated;
[0009] The electroplated hot stamped parts are subjected to electrophoresis treatment.
[0010] As a further description of the above technical solution, in the step of "heating the raised burrs on the surface of the hot stamping part, and flattening the raised burrs softened by heat, or / and blowing off the slag generated by the heating of the raised burrs", a laser heater is used to heat the raised burrs on the surface of the hot stamping part;
[0011] An air knife is used to flatten the raised burrs softened by heat, or / and to blow away the slag generated by the raised burrs when heated.
[0012] As a further description of the above technical solution, the power of the laser heater is less than 1.5KW, and the preferred power is 500W-1000W.
[0013] As a further description of the above technical solution, the scanning speed of the laser heater is less than 50 mm / s, and the preferred scanning speed is 3 mm / s-20 mm / s.
[0014] As a further description of the above technical solution, the laser heater scans the raised burrs on the surface of the hot stamping part at least once.
[0015] As a further description of the above technical solution, the laser line width emitted by the laser heater is less than 50 mm, and preferably the laser line width is 20 mm-50 mm.
[0016] As a further description of the above technical solution, the angle formed by the laser emitted by the laser heater and the hot stamping part is less than 90°, preferably less than 45°.
[0017] As a further description of the above technical solution, the air pressure of the wind knife is less than 20MPa, preferably 0.4MPa-16MPa.
[0018] As a further description of the above technical solution, in the extension direction of the laser emitted by the laser heater, the laser heater is located between the air knife and the hot stamping part;
[0019] The laser heater and the air knife move synchronously relative to the hot stamping part.
[0020] As a further description of the above technical solution, the distance between the light spot of the laser heater and the wind knife is 0mm-50mm, preferably 20mm-30mm.
[0021] By means of the above technical solution, the outstanding effects of the present invention are:
[0022] Before the hot stamping parts obtained by hot stamping are subjected to electroplating and electrophoresis treatment, the raised burrs on the surface of the hot stamping parts are first heated to evaporate or soften them by the heat, and the raised burrs softened by the heat are blown flat, or / and the slag generated by the heat of the raised burrs is blown away, thereby effectively reducing the raised burrs on the surface of the hot stamping parts, and improving their surface quality before electroplating treatment, thereby ensuring the quality of the coating applied thereto in the subsequent electroplating and electrophoresis steps, thereby optimizing the overall corrosion resistance of the hot stamping parts. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a flow chart of a method for preparing a hot stamping part in an embodiment of the present invention;
[0024] Figure 2 This is a diagram of the untreated raised burr of the hot stamping part in the embodiment of the present invention;
[0025] Figure 3 This is a state diagram of the raised burrs of the hot stamping parts in an embodiment of the present invention after being heated and flattened or / and blowing away the slag generated by the raised burrs due to the heating. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] See also Figure 1 This embodiment discloses a method for preparing a hot stamping part, and the method for preparing a hot stamping part comprises:
[0028] Hot stamping is performed on a bare plate blank to form it into a hot stamping part, wherein raised burrs are formed on the surface of the hot stamping part;
[0029] Heating the raised burrs on the surface of the hot stamping part, and flattening the raised burrs softened by the heat, or / and blowing off the slag generated by the raised burrs when heated;
[0030] After the raised burrs softened by heat are flattened, or / and the slag generated by the raised burrs being heated is blown off, the hot stamping parts are electroplated;
[0031] The electroplated hot stamped parts are subjected to electrophoresis treatment.
[0032] By means of the above-mentioned preparation method, after the bare sheet blank is hot stamped into a hot stamped part, it is inevitable that raised burrs are formed on the surface of the hot stamped part. Before the hot stamped part is electroplated and electrophoretically treated, the raised burrs on the surface of the hot stamped part can be heated first so that they evaporate or soften due to the heat, and the raised burrs softened by the heat are blown flat, or / and the slag generated by the heating of the raised burrs is blown away, thereby effectively reducing the raised burrs on the surface of the hot stamped part, and improving its surface quality before electroplating, thereby ensuring the quality of the coating applied thereto in the subsequent electroplating and electrophoresis steps, thereby optimizing the overall corrosion resistance of the hot stamped part.
[0033] Specifically, in the step of "heating the raised burrs on the surface of the hot stamping part, and flattening the raised burrs softened by the heat, or / and blowing away the slag generated by the heating of the raised burrs", a laser heater is used to heat the raised burrs on the surface of the hot stamping part; an air knife is used to flatten the raised burrs softened by the heat, or / and blow away the slag generated by the heating of the raised burrs.
[0034] Specifically, the power of the laser heater is less than 1.5KW, preferably 500W-1000W, so that the raised burrs on the surface of the hot stamping part can be melted without causing deformation of the part. That is, when a laser heater with a lower power is used to scan and heat the raised burrs on the surface of the hot stamping part, the raised burrs on the surface of the hot stamping part cannot be melted, while a laser heater with a higher power can melt the raised burrs on the surface of the hot stamping part, but it is also easy to soften and deform the hot stamping part due to heat.
[0035] Specifically, the scanning speed of the laser heater is less than 50 mm / s. The reason is that if the scanning speed of the laser heater is too fast, the contact time between the light spot and the convex burr is short and the convex burr cannot be melted. If the scanning speed is too slow, the contact time between the light spot and the convex burr is long, and the heat concentration is large, which will cause the parts around the convex burr to soften. The preferred scanning speed is 3 mm / s-20 mm / s.
[0036] Specifically, the laser heater scans the raised burrs on the surface of the hot stamping part at least once.
[0037] Specifically, the laser line width emitted by the laser heater is less than 50 mm, preferably the laser line width is 20 mm-50 mm, so as to ensure that the formed light spot covers the raised burr area during the scanning process.
[0038] Specifically, the angle formed by the laser emitted by the laser heater and the hot stamping part is less than 90°, preferably less than 45°. The smaller the angle formed by the laser emitted by the laser heater and the hot stamping part, the larger the spot area projected on the raised burr, so that the raised burr can be effectively heated.
[0039] Specifically, the air pressure of the air knife is less than 20 MPa, preferably 0.4 MPa-16 MPa, so as to quickly cool the hot stamping parts and blow away the slag generated by the melting of the raised burrs.
[0040] Specifically, in the extension direction of the laser emitted by the laser heater, the laser heater is located between the air knife and the hot stamping part; the laser heater and the air knife move synchronously relative to the hot stamping part to soften and flatten the raised burrs on its surface or soften the raised burrs and blow away the slag generated by the raised burrs when heated. Specifically, the distance between the spot of the laser heater and the air knife is 0mm-50mm, preferably 20mm-30mm.
[0041] The present invention is described in detail below through specific embodiments.
[0042] Embodiment 1:
[0043] First, place a 1.4mm thick hot stamping threshold on a fixture for fixing. The raised burrs are located on the side wall of the hot stamping threshold. The scanning path of the laser heater is set according to the position of the raised burrs. Turn on the laser heater and the wind knife to heat and blow the raised burrs. The power of the laser heater is 500W, the scanning speed is 5mm / s, the laser line width is 50mm, the wind knife is 20mm away from the spot of the laser heater, the gas pressure is 0.6MPa, and the raised burrs are scanned once.
[0044] The hot stamped door sill is then subjected to electrogalvanizing and electrophoresis treatment.
[0045] Embodiment 2:
[0046] First, place the 1.8mm thick hot stamping longitudinal beam on the fixture for fixing. The raised burrs are located on the side wall and R angle of the hot stamping longitudinal beam. The scanning path of the laser heater is set according to the position of the raised burrs. Turn on the laser heater and the wind knife to heat and blow the raised burrs. Among them, the power of the laser heater is 900W, the scanning speed is 20mm / s, the laser line width is 50mm, the wind knife is 30mm away from the spot of the laser heater, the gas pressure is 16Mpa, and the raised burrs are scanned twice.
[0047] Then, the hot stamped longitudinal beam is subjected to electrogalvanizing and electrophoresis treatment.
[0048] Embodiment 3:
[0049] First, place a 1.8mm thick hot stamping triangular reinforcement plate on a fixture for fixing. The raised burrs are located on the concave side wall and R angle of the hot stamping triangular reinforcement plate. The scanning path of the laser heater is set according to the position of the raised burrs (at the concave side wall, the laser line and the raised burrs are set to move in a vertical posture). Turn on the laser heater and the wind knife to heat and blow the raised burrs. Among them, the power of the laser heater is 500W, the scanning speed is 5mm / s, the laser line width is 30mm, the wind knife is 30mm away from the spot of the laser heater, the gas pressure is 16Mpa, and the raised burrs are scanned once.
[0050] Then, the hot stamped triangular reinforcement plate is subjected to electrogalvanizing and electrophoresis treatment.
[0051] As shown in Table 1 below, the heights of the raised burrs on the surfaces of the hot stamping parts of Examples 1-3 before and after the treatment were measured, and the measurement results are as follows:
[0052] Table 1 Height measurement results of raised burrs on the surface of hot stamping parts before and after treatment in Examples 1-3
[0053]
[0054] As can be seen from Table 1, the height of the raised burrs on the surface of the hot stamping parts in each embodiment decreased by about 10μm-30μm after being heated and blown by the laser heater and the air knife, and the surface quality of each hot stamping part was significantly improved before the electrogalvanizing step. It should be understood that the sampling positions in each embodiment are randomly selected.
[0055] Moreover, Figure 2 and Figure 3 As shown, the raised burrs on the surface of the hot stamping parts appear sharp before being processed by the laser heater and the air knife, while after being processed by the laser heater and the air knife, the surface appears arc-shaped, which is obviously more conducive to ensuring the quality of the coating applied in the subsequent electroplating and electrophoresis steps.
[0056] Before and after the raised burrs on the surface of the hot stamping door sill in Example 1 were processed by the laser heater and the air knife, the mechanical properties of the hot stamping door sill were tested. The test results are shown in Table 2 below:
[0057]
[0058] It can be seen from Table 2 above that after the raised burrs on the surface of the hot stamped door sill are processed, the mechanical properties of the hot stamped door sill are still within the qualified range.
[0059] In addition, cyclic corrosion tests were performed on the hot stamping threshold after electrophoresis treatment in Example 1 and the hot stamping threshold of the same batch without burr treatment. The test results showed that the cyclic corrosion result of the hot stamping threshold after electrophoresis treatment in Example 1 was qualified, while the cyclic corrosion result of the hot stamping threshold of the same batch without burr treatment by laser heater and air knife was unqualified.
[0060] In summary, by preparing hot stamping parts using the method for preparing hot stamping parts disclosed in the present invention, the height of the raised burrs can be effectively reduced and their shape can be changed, thereby improving the quality of the electroplating layer and the electrophoretic layer applied thereon, thereby improving the corrosion resistance of the hot stamping parts.
[0061] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any changes, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a hot stamping part, characterized in that: include: Hot stamping is performed on a bare plate blank to form it into a hot stamping part, wherein raised burrs are formed on the surface of the hot stamping part; Heating the raised burrs on the surface of the hot stamping part, and flattening the raised burrs softened by the heat, or / and blowing off the slag generated by the raised burrs when heated; After the raised burrs softened by heat are flattened, or / and the slag generated by the raised burrs being heated is blown off, the hot stamping parts are electroplated; The electroplated hot stamped parts are subjected to electrophoresis treatment.
2. The method for preparing hot stamping parts according to claim 1, characterized in that: In the step of "heating the raised burrs on the surface of the hot stamping part, and flattening the raised burrs softened by the heat, or / and blowing off the slag generated by the heating of the raised burrs", the raised burrs on the surface of the hot stamping part are heated by a laser heater; An air knife is used to flatten the raised burrs softened by heat, or / and to blow away the slag generated by the raised burrs when heated.
3. The method for preparing hot stamping parts according to claim 2, characterized in that: The power of the laser heater is less than 1.5KW, preferably 500W-1000W.
4. The method for preparing hot stamping parts according to claim 2, characterized in that: The scanning speed of the laser heater is less than 50 mm / s, and preferably the scanning speed is 3 mm / s-20 mm / s.
5. The method for preparing hot stamping parts according to claim 2, characterized in that: The laser heater scans the raised burrs on the surface of the hot stamping part at least once.
6. The method for preparing hot stamping parts according to claim 2, characterized in that: The laser line width emitted by the laser heater is less than 50 mm, and preferably the laser line width is 20 mm-50 mm.
7. The method for preparing hot stamping parts according to claim 2, characterized in that: The angle formed by the laser emitted by the laser heater and the hot stamping part is less than 90°, preferably less than 45°.
8. The method for preparing hot stamping parts according to claim 2, characterized in that: The air pressure of the air knife is less than 20 MPa, preferably 0.4 MPa-16 MPa.
9. The method for preparing a hot stamping part according to claim 2, characterized in that: In the extension direction of the laser emitted by the laser heater, the laser heater is located between the air knife and the hot stamping part; The laser heater and the air knife move synchronously relative to the hot stamping part.
10. The method for preparing a hot stamping part according to claim 9, characterized in that: The distance between the light spot of the laser heater and the wind knife is 0mm-50mm, preferably 20mm-30mm.
Citation Information
Patent Citations
Machining method of engine left suspension bracket
CN104551567A
Sheet metal part machining technology
CN105196003A
Preparation method of hot stamping forming part
CN114790561A
Welding method for aluminum shell and cover plate
CN116174898A
Deburring device
CN217290878U