High-performance forming method for local stress plastification of difficult-to-deform material
By opening notches and setting mold features in the edges and stress concentration areas of high-strength steel and aluminum alloy materials, combined with the use of lubricants and adjustable presses, the problems of cracking and rebound during stamping are solved, and high precision and Uniformity forming effect.
Patent Information
- Application Number
- CN202411130217.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-15
AI Technical Summary
High-strength steel is prone to fracture and rebound during stamping, resulting in poor forming quality. Traditional cold stamping processes are difficult to meet the precision forming of complex structural parts. Hot stamping technology may lead to local thinning and tearing of the plate under high temperature environment. .
Open notches in the edge area and stress concentration area of the blank, set up hulls, grooves and type-based drawing ribs on the mold, and apply lubricant to the deformation concentration area and stamping wear area, and use an adjustable press to perform Stamping and shaping, adjust the stress and strain state of the material to reduce rebound and wrinkle.
Through local stress plasticization, the forming accuracy and surface smoothness are improved, rebound and wrinkle phenomena are reduced, and the thickness uniformity and forming quality of high-strength steel and aluminum alloy materials are ensured.
Smart Images

Figure CN118950797A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of stamping technology, and in particular to a high-performance forming method for local stress plasticization of difficult-to-deform materials. Background Art
[0002] High-strength steel is widely used in the automotive industry, shipbuilding industry, bridge construction, mining machinery and other fields due to its advantages of high specific strength, high specific stiffness, and good corrosion resistance. In particular, in the automotive manufacturing industry, high-strength steel has become an important basic material for manufacturing advanced car body structures.
[0003] However, as the strength of high-strength steel plates continues to increase, the traditional cold stamping process is very likely to produce negative effects such as cracking and springback during the forming process, making it impossible to meet the precision forming of complex structural parts. This has limited the large-scale application of high-strength steel to a certain extent. Although hot stamping technology can alleviate the cracking and springback of parts during the forming process, in a high-temperature forming environment, the hardening and softening effect caused by dislocation recovery will make the plate prone to local thinning and tearing, ultimately leading to uneven thickness of the formed parts.
[0004] Therefore, in the face of the forming quality problems of high-strength steel during the stamping process, it is of great significance to develop a high-performance forming method for local stress plasticization of difficult-to-deform materials. Summary of the invention
[0005] In view of this, it is necessary to provide a high-performance forming method for local stress plasticization of difficult-to-deform materials to solve the technical problems of defects such as cracking and springback that are easily generated in cold stamping forming in the prior art.
[0006] The present invention provides a high-performance forming method for local stress plasticization of difficult-to-deform materials, wherein the blank has a stress concentration area, a deformation concentration area and a stamping wear area, and the high-performance forming method for local stress plasticization of difficult-to-deform materials comprises the following steps: S1, a plurality of notches are formed in the edge area and / or the stress concentration area of the blank, and one or more of convex humps, grooves and conformal zone draw ribs are formed on the mold; S2, a lubricant is applied to the deformation concentration area and / or the stamping wear area of the blank; S3, a press is used to stamp the blank.
[0007] Furthermore, the material of the blank is steel or aluminum alloy.
[0008] Furthermore, the aluminum alloy grade is 2000 series, 6000 series or 7000 series.
[0009] Furthermore, the blank is a plate with a thickness of 1-4 mm.
[0010] Furthermore, in step S3, the blank holding force of the press is adjustable.
[0011] Further, in step S3, when the punching stroke is less than or equal to 20 mm, the blank holding force of the press is 2.8-3.2 MPa.
[0012] Further, in step S3, when the punching stroke is greater than 20 mm, the blank holding force of the press is 1-1.6 MPa.
[0013] Furthermore, in step S1, the shape of the notch is one or more of a semicircle, a semi-ellipse or a rounded rectangle.
[0014] Furthermore, in step S2, the lubricant is lubricating oil or lubricating grease.
[0015] Furthermore, the side of the blank coated with the lubricant faces the punch head of the press.
[0016] Compared with the prior art, the high-performance forming method for local stress plasticization of difficult-to-deform materials provided by the present invention opens a number of notches in the edge area and / or stress concentration area of the blank to obtain material replenishment from adjacent areas, changes the stress-strain state of the material, and sets local features such as convex humps, grooves, and conformal draw ribs on the mold to increase the feed resistance in different areas, increase the tensile stress of the blank, reduce rebound and wrinkling, and thus achieve stress plasticization. Lubricant is applied to the blank in the deformation concentration area and / or stamping wear area to reduce material flow during stamping. The components manufactured by this method have good surface smoothness while ensuring the forming accuracy.
[0017] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows with reference to the accompanying drawings. The specific implementation of the present invention is given in detail by the following embodiments and their accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings: Figure 1 A flowchart of another preferred embodiment of the high-performance forming method for local stress plasticization of difficult-to-deform materials provided by the present invention.
[0019] Figure 2 A schematic flow chart of a preferred embodiment of a high-performance forming method for local stress plasticization of difficult-to-deform materials provided by the present invention; Figure 3 A three-dimensional model diagram of a high-strength steel lower control arm provided by the present invention; Figure 4 Schematic diagram of the structure of the conventional cold stamped aluminum alloy automobile tool box cover provided by the present invention Figure 5 This is a schematic diagram of the structure of the local stress plasticized cold stamping aluminum alloy automobile tool box cover provided by the present invention. DETAILED DESCRIPTION
[0020] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0021] See also Figure 1 and Figure 2 The present invention provides a high-performance forming method for local stress plasticization of difficult-to-deform materials. The blank has a stress concentration area, a deformation concentration area and a stamping wear area. The method comprises the following steps: S1. A plurality of notches 11 are provided in the edge area and / or the stress concentration area of the blank 1. The notches 11 are provided according to the complexity of the geometric shape of the formed parts. For parts with regular shapes, the opening parts are provided along the edges of the blank 1. For parts with complex geometric shapes, the notches 11 are provided as far as possible in the areas with large stress concentration and easy wrinkling, i.e., stress concentration areas. The stress plasticization is achieved by changing the stress distribution state of the blank 1 during the forming process through the notches 11.
[0022] S2. Apply lubricant to the deformation concentration area and / or stamping wear area of the blank 1. The deformation concentration area and stamping wear area are determined based on the wear condition of the blank 1 during the trial stamping process.
[0023] S3. Use a press machine 2 to punch the blank 1.
[0024] In some embodiments, the material of the blank 1 is steel, specifically HDT780C or a steel plate with a yield strength of 210MPa-550MPa and a tensile strength of 270MPa-700MPa. In other embodiments, in addition to steel, the material of the blank 1 can also be aluminum alloy. Specifically, the material of the blank 1 can be 2000 series, 6000 series or 7000 series aluminum alloy.
[0025] In some embodiments, the blank 1 is a plate with a thickness of 1-4 mm.
[0026] In step S1 of some embodiments, the shape of the notch 11 is one or more of a semicircle, a semi-ellipse or a rounded rectangle.
[0027] In step S2 of some embodiments, the lubricant 12 is lubricating oil or lubricating grease.
[0028] In some embodiments, the side of the blank 1 coated with the lubricant 12 faces the punching head of the press 2 .
[0029] In step S3 of some embodiments, the press 2 is a servo press with adjustable blank holding force.
[0030] In step S3 of some embodiments, when the punching stroke is less than or equal to 20 mm, the blank holding force of the press is 2.8-3.2 MPa. When the punching stroke is greater than 20 mm, the blank holding force of the press is 1-1.6 MPa. That is, when the punching stroke is larger, the blank holding force is smaller, and when the punching stroke is smaller, the blank holding force is larger.
[0031] Example 1 The local stress plasticized high-strength steel lower control arm stamping forming method, the forming material is 490mm×307mm×3.2mm HDT780C high-strength steel, specifically comprising the following steps: (1) According to the problem that the front and rear ends of the high-strength steel lower control arm components are prone to springback during cold stamping, which in turn affects the forming accuracy, the front and rear ends of the high-strength steel billet are opened to change the stress-strain state of the material. The opening part consists of an arc part and a straight-line connecting part, with a specific size of 8 mm × 8 mm. The distance between the straight-line segments is 4 mm, and the arc part of R2 borders the straight-line segment.
[0032] (2) Lubricate the pre-opened high-strength steel sheet in different areas. Figure 3 It is clear that the front convex surface 31, the left side 32, the right side 33, and the rear concave surface 34 of the blank are relatively severely worn during the forming process, so lubricant is applied to the above-mentioned areas.
[0033] (3) Place the processed blank in the lower mold cavity of the forming mold, start the press, and the slider of the press moves downward to drive the upper forming mold downward, so that the blank placed in the mold is formed by the variable pressure force. The initial pressure force is set to 500-700kN, and the punching speed is 50-100mm / s-1. As the forming stroke increases, when it reaches 10-20mm, the pressure force gradually decreases to 200-400kN.
[0034] After forming, the mold is opened to obtain the formed component. The springback values of the left side 32 and the right side 33 of the formed high-strength steel lower control arm are shown in the following table, which ensures that the forming is not cracked or wrinkled while synergistically improving the forming accuracy of the high-strength steel lower control arm.
[0035]
[0036] Example 2 The local stress plasticized aluminum alloy automobile tool box cover stamping forming method, the forming material is 6061 aluminum alloy of 1100mm×900mm×1mm, specifically comprising the following steps: (1) According to numerical simulation and component test results, the main problem of aluminum alloy automotive tool box cover in the cold forming process is wrinkling, and the wrinkling position is distributed around the edges of the component. Figure 4 Based on the above phenomenon, the 6061 aluminum alloy automobile tool box cover blank is opened and the punch is set with drawbeads and other local features, such as Figure 5 As shown, the feeding resistance in different areas is increased, the tensile stress of the blank is increased, and the wrinkling phenomenon is reduced.
[0037] (2) Apply lubricant to the deformation concentrated area and / or stamping wear area of the sheet metal for zoned lubrication. According to the numerical simulation and the test stamping results of the parts, it is clear that the convex parts of the corners of the 6061 aluminum alloy billet are relatively severely worn during the forming process, so lubricant is applied to the above-mentioned areas.
[0038] (3) Place the processed blank in the lower mold cavity of the forming mold, start the press, and the slider of the press moves downward to drive the upper forming mold downward, so that the blank placed in the mold is formed by the variable pressure force. The initial pressure force is set to 150-300kN, and the punching speed is 80-120mm / s-1. As the forming stroke increases, when it reaches 15-20mm, the pressure force gradually decreases by 50-150kN.
[0039] After forming, the mold is opened to obtain the formed component. The wrinkle phenomenon on the surface of the formed automobile tool box cover is significantly reduced, the precision of the part is improved, and the surface is smooth without visible cracks.
[0040] Compared with the prior art, the high-performance forming method for local stress plasticization of difficult-to-deform materials provided by the present invention opens a number of notches in the edge area and / or stress concentration area of the blank to obtain material replenishment from adjacent areas, changes the stress-strain state of the material, and sets local features such as convex humps, grooves, and conformal draw ribs on the mold to increase the feed resistance in different areas, increase the tensile stress of the blank, reduce rebound and wrinkling, and thus achieve stress plasticization. Lubricant is applied to the blank in the deformation concentration area and / or stamping wear area to reduce material flow during stamping. The components manufactured by this method have good surface smoothness while ensuring the forming accuracy.
[0041] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A high-performance forming method for local stress plasticization of difficult-to-deform materials, wherein the blank has a stress concentration area, a deformation concentration area and a stamping wear area, characterized in that: It includes the following steps: S1. A plurality of notches are formed in the edge area of the blank and / or the stress concentration area, and one or more of convex humps, concave grooves, and contour-based draw ribs are formed on the mold; S2, applying lubricant to the blank in the deformation concentrated area and / or the stamping wear area; S3, using a press to stamp the blank.
2. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 1, characterized in that: The material of the blank is steel or aluminum alloy.
3. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 2, characterized in that: The aluminum alloy grade is 2000 series, 6000 series or 7000 series.
4. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 1, characterized in that: The blank is a plate with a thickness of 1-4 mm.
5. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 1, characterized in that: In step S3, the blank holding force of the press is adjustable.
6. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 5, characterized in that: In step S3, when the punching stroke is less than or equal to 20 mm, the blank holding force of the press is 2.8-3.2 MPa.
7. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 5, characterized in that: In step S3, when the punching stroke is greater than 20 mm, the blank holding force of the press is 1-1.6 MPa.
8. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 1, characterized in that: In step S1, the shape of the notch is one or more of a semicircle, a semi-ellipse or a rounded rectangle.
9. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 1, characterized in that: In step S2, the lubricant is lubricating oil or lubricating grease.
10. The high-performance forming method of local stress plasticization of difficult-to-deform materials according to claim 1, characterized in that: The side of the blank coated with lubricant faces the punch head of the press.
Citation Information
Patent Citations
Deep drawing process of austenitic stainless steel plate
CN102029314A
Variable speed and variable blank holder force linked sheet drawing process
CN102950185A
Automobile side body roof rail shaping die
CN110479796A
METHOD FOR MANUFACTURING MOLDED MATERIAL, BLANK MATERIAL, AND Square TUBE
CN116940423A