Simple moulding bed forging method for large gear machining
Patent Information
- Application Number
- CN202411298361.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
AI Technical Summary
[0008]针对现有技术的不足,本发明提供了一种用于大型齿轮加工的简易胎模锻造方法,解决了现有技术存在生产效率低、材料浪费、热处理不均匀、精度差的问题
本发明通过整合先进的金属3D打印技术、智能温度控制系统、多轴锻造设备、液氮快速冷却技术及精确的热处理流程,显著提高了胎模的生产效率和质量。能够优化胎模的耐用性和结构完整性,减少材料消耗,缩短生产周期,并提升最终产品的精度和表面光洁度。通过实现更精确的加工控制和增强的性能参数,本发明有效地降低了制造成本,同时确保了胎模能够满足更高负载和更苛刻工况的需求,为高性能齿轮制造提供了一种经济高效的解决方案。
Smart Images

Figure CN118950924A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of large gear processing, in particular to a simple die forging method for large gear processing. Background Art
[0002] In the field of large gear manufacturing, the design and manufacture of the die (mold) is crucial to the quality and performance of the final product. Traditional die forging methods usually involve multiple steps, including complex machining and heat treatment processes, which are often time-consuming, costly, and have limitations on material utilization and production efficiency. In addition, due to the limitations of traditional methods in temperature control and the accuracy of the forging process, it is often difficult to ensure the uniformity and accuracy of the die, which directly affects the quality and durability of the gear.
[0003] Disadvantages of existing technology Precision and consistency issues: In traditional forging processes, temperature control and pressure application are often not precise enough, resulting in uneven stress and microstructural defects inside the mold. These problems will affect the precision and consistency of the final product.
[0004] Low production efficiency: Traditional tire mold production relies on multi-step machining and heat treatment, each step requires a lot of manual operation and time, which greatly reduces production efficiency.
[0005] Material Waste: Traditional forging and machining techniques often result in costly material waste due to the difficulty in achieving precise material control.
[0006] Uneven heat treatment: In conventional heat treatment processes, it is difficult to achieve uniform heating and cooling of the tire mold material due to heat conduction and environmental influences, which will affect the mechanical properties and life of the material.
[0007] To this end, those skilled in the art provide a simple die forging method for large gear processing to solve the problems raised in the above background technology. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a simple die forging method for large gear processing, which solves the problems of low production efficiency, material waste, uneven heat treatment and poor precision in the prior art.
[0009] To achieve the above objectives, the present invention is implemented through the following technical solutions: A simple die forging method for large gear processing, comprising the following steps: S1. Material preparation: Select high-performance alloy material as the simple tire mold blank; S2. Fetal membrane design: using metal 3D printing technology to make a fetal mold in the form of multiple modules to obtain a fetal membrane blank; S3, preheating: placing the tire mold blank in a box furnace for preliminary preheating treatment; S4. Billet heating: Equipped with high-efficiency induction heating equipment, and installed and debugged in the equipment intelligent temperature control system, real-time monitoring and adjustment of heating temperature, preset the best forging temperature range, after the equipment is ready, place the tire mold billet in the heating equipment and heat it to the target temperature according to the set program; S5, Forging: Configure a multi-axis forging device that can apply pressure from multiple directions, place the heated tire mold blank into the forging device, and execute the preset CNC program; S6. Rapid cooling: After forging is completed, the membrane blank is quickly transferred to the cooling equipment for cooling. The cooling equipment is equipped with multi-angle temperature monitoring sensors to monitor the temperature changes of the blank at multiple angles to reduce thermal stress concentration; S7, heat treatment: placing the cooled gear blank into a heat treatment device and performing heat treatment according to predetermined process parameters; S8, polishing: putting the tire mold blank that has undergone laser surface treatment into an ultrasonic polishing device for polishing; S9. Inspection: Assemble the polished modular membrane blanks and test the accuracy and durability of the membrane inner cavity through simulated forging.
[0010] Preferably, the high performance alloy material used in step S1 is H13 tool steel.
[0011] Preferably, in step S3, the preheating of the H13 tool steel in the box furnace includes preliminary preheating and main preheating, wherein the preliminary preheating temperature is set at 400°C-600°C, and the main preheating temperature is set at 600°C-800°C.
[0012] Preferably, in step S4, the predetermined heating temperature of the induction heating equipment is between 1020°C and 1180°C.
[0013] Preferably, the H13 tool steel forged by the multi-axis forging equipment in the step S5 needs to be maintained at 1040° C.-1150° C., and the pressure applied by the multi-axis forging equipment is 800t-1000t.
[0014] Preferably, in step S6, -196°C liquid nitrogen is used in the cooling equipment to cool the fetal membrane blank.
[0015] Preferably, the heat treatment equipment in step S7 is a vacuum furnace.
[0016] Preferably, the vacuum furnace heats the fetal membrane blank to a temperature of 1020°C to 1050°C.
[0017] The present invention provides a simple die forging method for large gear processing, which has the following beneficial effects: The present invention significantly improves the production efficiency and quality of tire molds by integrating advanced metal 3D printing technology, intelligent temperature control systems, multi-axis forging equipment, liquid nitrogen rapid cooling technology and precise heat treatment processes. It can optimize the durability and structural integrity of tire molds, reduce material consumption, shorten production cycles, and improve the accuracy and surface finish of final products. By achieving more precise processing control and enhanced performance parameters, the present invention effectively reduces manufacturing costs while ensuring that tire molds can meet the needs of higher loads and more demanding working conditions, providing a cost-effective solution for high-performance gear manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the process of the present invention. DETAILED DESCRIPTION
[0019] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. For examples, please see the attached Figure 1 The embodiment of the present invention provides a simple die forging method for large gear processing, comprising the following steps:
[0020] S1. Material preparation: Select a high-performance alloy material as the simple tire mold blank; the high-performance alloy material used in the S1 step is H13 tool steel. Select a high-performance alloy material as the simple tire mold blank. In this step, the selected material is H13 tool steel, which is an alloy widely used in high-temperature applications and is selected for its excellent thermal stability and wear resistance. H13 tool steel has good hardness and toughness and can withstand continuous thermal cycles without failure. The use of H13 tool steel improves the heat resistance and durability of the tire mold, ensures performance stability during high-temperature forging, reduces frequent replacement due to material degradation, and reduces production costs.
[0021] S2. Fetal membrane design: Use metal 3D printing technology to make the tire mold in multiple modules to obtain the tire membrane blank; Use metal 3D printing technology to make the tire mold in multiple modules. This method allows complex tire mold designs to be printed accurately, while reducing material waste and processing time in traditional mechanical processing.
[0022] The modular design simplifies the assembly and maintenance process, allowing single damaged parts to be replaced individually, improving the operating efficiency of the overall equipment and reducing maintenance costs.
[0023] S3, preheating: the tire mold blank is placed in a box furnace for preliminary preheating treatment; in the S3 step, the box furnace preheating of H13 tool steel includes preliminary preheating and main preheating, wherein the preliminary preheating temperature is set at 400℃-600℃, and the main preheating temperature is set at 600℃-800℃. The staged preheating strategy helps to uniform the material properties, improves the safety of subsequent processing and the machinability of the material, and avoids energy waste caused by overheating.
[0024] S4, billet heating: configure high-efficiency induction heating equipment, install and debug the intelligent temperature control system in the equipment, monitor and adjust the heating temperature in real time, preset the optimal forging temperature range, and after the equipment is ready, place the tire mold blank in the heating equipment and heat it to the target temperature according to the set program; in the S4 step, the predetermined heating temperature of the induction heating equipment is 1020℃-1180℃. Induction heating provides a fast and uniform heating method, reduces energy consumption and reduces heating time. The intelligent temperature control system ensures the accuracy of the heating process and improves product quality and consistency.
[0025] S5, Forging: Configure a multi-axis forging device that can apply pressure from multiple directions, place the heated tire mold blank into the forging device, and execute the preset CNC program; the H13 tool steel forged by the multi-axis forging device in the S5 step needs to be maintained at 1040℃-1150℃, and the pressure applied by the multi-axis forging device is 800t-1000t. The multi-axis forging device can provide a more uniform stress distribution, reduce defects and deformation during the forging process, and improve the mechanical properties and structural integrity of the product. By controlling the forging temperature and pressure, the high-precision molding of the tire mold is guaranteed.
[0026] S6, rapid cooling: After forging is completed, the tire membrane blank is quickly transferred to the cooling equipment for cooling. The cooling equipment is equipped with multi-angle temperature monitoring sensors to monitor the temperature changes of the blank at multiple angles to reduce thermal stress concentration. In the S6 step, -196°C liquid nitrogen is used in the cooling equipment to cool the tire membrane blank. Liquid nitrogen rapid cooling technology enables the tire mold to cool down quickly, avoiding structural changes and stress concentration caused by long-term high temperature. Multi-angle temperature monitoring ensures the uniformity of cooling, further reduces thermal stress, and improves the mechanical properties and durability of the material.
[0027] S7, heat treatment: put the cooled gear blank into the heat treatment equipment and perform heat treatment according to the predetermined process parameters; the heat treatment equipment in step S7 is a vacuum furnace, and the vacuum furnace heats the tire film blank at a temperature of 1020℃ to 1050℃. Vacuum furnace heat treatment can prevent oxidation and contamination, improve the purity and performance stability of the material. Accurate temperature control ensures the heat treatment effect, makes the tire mold have higher hardness and toughness, and prolongs its service life.
[0028] S8. Polishing: Put the tire mold blank that has been treated with laser surface into the ultrasonic polishing equipment for polishing; ultrasonic polishing technology can effectively remove surface micro defects, improve surface quality and finish, and reduce friction and wear. This treatment makes the tire mold show better durability and stability during use.
[0029] S9. Inspection: Assemble the polished modular membrane blanks and test the accuracy and durability of the membrane inner cavity through simulated forging.
[0030] By introducing advanced technologies such as metal 3D printing, intelligent temperature control systems, multi-axis forging equipment, rapid cooling with liquid nitrogen, and heat treatment in vacuum furnaces, the manufacturing efficiency and quality of tire molds have been significantly improved. Specifically, the temperature and pressure control during the production process has been optimized, reducing material consumption and production time, improving the durability and structural integrity of tire molds, and ensuring high-precision and high-performance product output.
[0031] Example 1: Basic 3D Printing Die Forging step: S1. Material selection: Use H13 tool steel powder.
[0032] S2. Tire mold design and 3D printing: Design a simple gear tire mold and print it using laser melting 3D printing technology.
[0033] S3. Preheating: Preliminary preheating is performed at 600°C for 2 hours in a box furnace.
[0034] S4, heating: heating the tire mold to 1040°C in an induction heating device.
[0035] S5. Forging: Forging is performed on a uniaxial press with a force of 800 tons.
[0036] S6. Rapid cooling: Use room temperature water for rapid cooling.
[0037] S7. Heat treatment: Tempering treatment is performed in a conventional furnace with the temperature set at 560°C for 2 hours.
[0038] S8, Polishing: Use mechanical polishing to process the surface.
[0039] S9. Inspection: Verify the quality of the tire mold through size inspection and hardness test.
[0040] Summary of embodiments: This example demonstrates a basic die forging method using standard 3D printing and traditional heat treatment techniques, suitable for general-purpose applications that do not require extreme performance.
[0041] Example 2: Advanced 3D Printing and Multi-Axis Forging step: S1. Material selection: Cobalt-based alloy powder is used.
[0042] S2. Tire mold design and 3D printing: Electron beam melting technology is used to print complex tire mold structures.
[0043] S3. Preheating: Preheat at 800°C for 4 hours in a box furnace.
[0044] S4, heating: heating the tire mold to 1150°C in an induction heating device.
[0045] S5. Forging: Forging is performed at 1000 tons force in a multi-axis forging equipment.
[0046] S6. Rapid cooling: Use liquid nitrogen for rapid cooling.
[0047] S7. Heat treatment: Perform precisely controlled tempering treatment in a vacuum furnace with the temperature set at 620°C for 4 hours.
[0048] S8. Polishing: Use ultrasonic polishing technology.
[0049] S9. Inspection: Verify the performance of the tire mold through simulated forging tests and durability tests.
[0050] Summary of embodiments: This example demonstrates a high-level manufacturing process that combines advanced 3D printing technology, multi-axis forging and precise heat treatment for tire mold production that requires high performance and complex shapes.
[0051] Example 3, customized high temperature and durable tire mold step: S1. Material selection: high temperature nickel-based super alloy.
[0052] S2. Tire mold design and 3D printing: Use direct metal deposition technology to make a tire mold with enhanced cooling channels.
[0053] S3. Preheating: Preheat in a box furnace at 850°C for 6 hours.
[0054] S4, heating: heat the tire mold to 1180°C.
[0055] S5, Forging: Use multi-axis forging equipment with high-precision control to apply 1,200 tons of pressure.
[0056] S6. Rapid cooling: Use liquid nitrogen for rapid cooling to ensure that the mold temperature is quickly reduced and thermal stress is minimized.
[0057] S7. Heat treatment: Precisely controlled dissolution and aging treatment is carried out in a vacuum furnace with the temperature set at 1080°C for 6 hours.
[0058] S8, Polishing: Use laser polishing technology to achieve high-precision surface treatment.
[0059] S9. Inspection: Conduct comprehensive quality inspection, including durability testing at high temperatures and geometric accuracy testing.
[0060] Summary of embodiments: This embodiment is suitable for the production of tire molds with extreme working conditions, such as in the aviation and automobile fields. By using high-performance materials and advanced manufacturing technology, the high temperature resistance and wear resistance of the tire mold are greatly improved.
[0061] Experimental design and testing In order to verify the performance of the above three embodiments, the following comparative experiments are designed: Hardness test: Measure the hardness of each tire mold material after forging and heat treatment, and compare the effects of different materials and treatment processes on hardness.
[0062] Wear resistance test: The wear resistance of each tire mold is evaluated through standard wear tests such as loose sand wear test.
[0063] Thermal cycle durability test: The tire mold is subjected to multiple high-temperature cycles to detect changes in its performance under repeated thermal stress.
[0064] Test data table design: Experimental Project Example 1 Example 2 Example 3 Hardness (HRC) 52 56 60 Wear rate (mg / hour) 0.5 0.3 0.1 Hardness change after thermal cycling -4 HRC -2 HRC -1 HRC Summary: From the above experimental data, we can observe that: Example 3 provided the highest hardness and the lowest wear rate, indicating that the materials and technology used are most suitable for high load and high temperature environments.
[0065] Compared with Example 1, Example 2 has a significant improvement in hardness and wear resistance, which shows the importance of multi-axis forging and precise heat treatment in improving tire mold performance.
[0066] Thermal cycling tests show that advanced thermal treatment (such as the vacuum furnace treatment in Example 3) significantly improves the thermal stability of the material.
[0067] in conclusion: The three examples show the scope of application and advantages of the method of the present invention, which can provide significant performance advantages from basic industrial applications to high-end special needs. In addition, the experimental data clearly demonstrates the important role of advanced materials and manufacturing technology in improving tire mold performance.
[0068] Comparative experiment Comparative experiment 1: production efficiency Purpose: To compare production time and material consumption between two methods.
[0069] Parameters: The total time and amount of material required to complete a standard tire mold.
[0070] Comparative experiment 2: durability test Purpose: To evaluate the performance of tire molds manufactured by two methods under high load cycle testing.
[0071] Parameters: Wear rate and structural integrity of tire molds after 1000 high load cycles.
[0072] Comparative experiment 3: quality control Purpose: To test the dimensional accuracy and surface roughness of tire molds made by two methods.
[0073] Parameters: The dimensional accuracy is measured using a three-dimensional coordinate measuring machine, and the surface roughness is measured using a surface roughness meter.
[0074] Experimental data table design: Experimental Project Traditional methods Method of the present invention Comparison results Production time (hours) 12 8 The method of the present invention reduces production time by 33% and improves efficiency Material consumption (kg) 5 3.5 Reduce material consumption by 30% and reduce costs Wear rate (mg / 1000 cycles) 0.8 0.3 Improve tire mold durability by about 166% Structural Integrity Crack appears 800 times No cracks Significantly improve structural durability Dimensional accuracy (mm) ±0.02 ±0.01 Improve dimensional accuracy by 100% Surface roughness (Ra, μm) 0.8 0.4 Smoother surface, 50% improvement Comprehensive analysis and conclusion Through the above comparative experimental data, it can be clearly seen that the method of the present invention has significant advantages in many key aspects compared with the traditional simple tire die forging method: Improve production efficiency: By using 3D printing and efficient heat treatment equipment, the method of the present invention greatly shortens the production time and reduces the consumption of materials, which is especially important for large-scale production.
[0075] Enhanced durability: The method of the present invention significantly improves the durability of the tire mold, reduces the wear rate, and enhances the structural integrity by optimizing the forging process and cooling technology, so that the tire mold can withstand higher workloads and longer service life.
[0076] Improved quality control: The method of the present invention achieves higher dimensional accuracy and lower surface roughness through precise processing control and surface treatment, which helps to improve the overall quality of the final product.
[0077] In summary, the method of the present invention has significant advantages in both technical performance and economic benefits, and is particularly suitable for high-performance, high-quality and high-efficiency tire mold production, and is particularly suitable for those application fields that have strict requirements on precision and durability. In general, the present invention not only improves production efficiency and product quality, but also reduces manufacturing costs by optimizing the process flow, thereby providing users with significant economic and technical advantages.
[0078] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A simple die forging method for large gear processing, characterized in that: The following steps are involved: S1. Material preparation: Select high-performance alloy material as the simple tire mold blank; S2. Fetal membrane design: using metal 3D printing technology to make a fetal mold in the form of multiple modules to obtain a fetal membrane blank; S3, preheating: placing the tire mold blank in a box furnace for preliminary preheating treatment; S4. Billet heating: Equipped with high-efficiency induction heating equipment, and installed and debugged in the equipment intelligent temperature control system, real-time monitoring and adjustment of heating temperature, preset the best forging temperature range, after the equipment is ready, place the tire mold billet in the heating equipment and heat it to the target temperature according to the set program; S5, Forging: Configure a multi-axis forging device that can apply pressure from multiple directions, place the heated tire mold blank into the forging device, and execute the preset CNC program; S6. Rapid cooling: After forging is completed, the membrane blank is quickly transferred to the cooling equipment for cooling. The cooling equipment is equipped with multi-angle temperature monitoring sensors to monitor the temperature changes of the blank at multiple angles to reduce thermal stress concentration; S7, heat treatment: placing the cooled gear blank into a heat treatment device and performing heat treatment according to predetermined process parameters; S8, polishing: putting the tire mold blank that has undergone laser surface treatment into an ultrasonic polishing device for polishing; S9. Inspection: Assemble the polished modular membrane blanks and test the accuracy and durability of the membrane inner cavity through simulated forging.
2. A simple die forging method for large gear processing according to claim 1, characterized in that: The high performance alloy material used in step S1 is H13 tool steel.
3. A simple die forging method for large gear processing according to claim 1, characterized in that: In the step S3, the preheating of H13 tool steel in the box furnace includes preliminary preheating and main preheating, wherein the preliminary preheating temperature is set at 400°C-600°C, and the main preheating temperature is set at 600°C-800°C.
4. A simple die forging method for large gear processing according to claim 1, characterized in that: In the step S4, the predetermined heating temperature of the induction heating device is 1020°C-1180°C.
5. A simple die forging method for large gear processing according to claim 1, characterized in that: The H13 tool steel forged by the multi-axis forging equipment in the step S5 needs to be maintained at 1040° C.-1150° C., and the pressure applied by the multi-axis forging equipment is 800t-1000t.
6. A simple die forging method for large gear processing according to claim 1, characterized in that: In the step S6, -196°C liquid nitrogen is used in the cooling equipment to cool the fetal membrane blank.
7. A simple die forging method for large gear processing according to claim 1, characterized in that: The heat treatment equipment in step S7 is a vacuum furnace.
8. A simple die forging method for large gear processing according to claim 7, characterized in that: The vacuum furnace heats the fetal membrane blank to a temperature of 1020°C to 1050°C.
Citation Information
Patent Citations
Gear forging forming die without flash as well as preparation method and forging method
CN111054882A
Manufacturing method of double-alloy double-structure titanium alloy blisk
CN112296602A
Cladding type composite additive production line manufacturing method
CN112974835A
Forging method of wind power high-speed gear
CN114653887A
Quality control method for forge piece subjected to ultrafine grain treatment after multidirectional forging
CN114951527A
Cited By
Tapered pressing process for two ends of round steel
CN120001823A