Preparation process of low-oxygen water-atomized superfine copper powder

Through the preparation process of low oxygen water atomization ultrafine copper powder, the copper powder is coated in a wet environment with composite antioxidants, combined with vacuum low-temperature drying, the problems of low efficiency and bonding of ultrafine copper powder in the existing process are solved, and the problem of low-efficiency and bonding of ultrafine copper powder in the existing process is achieved. Efficient preparation and stability protection.

CN118951029APending Publication Date: 2024-11-15GUIZHOU BOTAO NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410859100.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing copper powder production process is inefficient and cumbersome when preparing ultrafine copper powder. The copper powder prepared by the reduction method is easy to bond and difficult to break down to below 5 microns.

Method used

The preparation process of ultrafine copper powder with low oxygen water atomization includes smelting atomization, centrifugal dehydration, antioxidant treatment, vacuum drying and airflow sorting. The copper powder is coated in a humid environment by composite antioxidants to avoid oxidation. , and the particle size of the ultrafine copper powder is retained under vacuum low-temperature drying conditions.

Benefits of technology

The yield and content of ultrafine copper powder with a particle size of less than 5 microns is increased, the production process is simplified, the bonding problem is avoided, the production efficiency is improved, and antioxidant protection is provided during storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the field of powder metallurgy, in particular to a preparation process of low-oxygen water atomized superfine copper powder, which comprises the following steps: S1, smelting and atomizing; s2, centrifugal dewatering is conducted, specifically, the atomized copper powder in the step S1 is put into a centrifugal machine to be subjected to high-speed centrifugal separation to obtain atomized water and the copper powder; s3, anti-oxidation treatment: preparing a composite antioxidant, injecting the composite antioxidant into a centrifugal machine by using a water pump after the centrifugal dewatering procedure in the step S2 is completed, opening a three-way valve below the centrifugal machine to a circulating system, performing low-speed centrifugal washing for 15-40 minutes, performing anti-oxidation treatment on the surface of the copper powder, performing centrifugal separation after centrifugal washing, and drying the copper powder to obtain the copper powder. Feeding clear water to wash the copper powder, and performing high-speed centrifugal dewatering on the copper powder after washing is completed; s4, vacuum drying; and S5, airflow sorting. Compared with the prior art, the oxygen content of the copper powder is reduced by arranging anti-oxidation treatment instead of traditional reduction treatment, and the technical problems that according to an existing copper powder production process, the production efficiency of the superfine copper powder is low, and the production process is tedious are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of powder metallurgy, in particular to a preparation process of low-oxygen water atomized ultrafine copper powder. Background Art

[0002] Ultrafine copper powder is an indispensable basic raw material for nano copper materials with good conductivity and high strength. Due to its excellent electrical properties, it is widely used in conductive adhesives, conductive coatings and electrode materials. In recent years, research has found that it can be used to make catalysts, lubricant additives, and even to treat osteoporosis and fractures.

[0003] The existing copper powder preparation process is generally as follows: the raw materials are first made into copper powder through an atomization powder making system, and then the water-containing copper powder is centrifugally dehydrated and dried. The dried copper powder is then reduced in a reduction furnace to reduce the oxygen content in the copper powder, and the reduced copper powder is crushed to obtain a finished copper powder with a qualified particle size.

[0004] The above existing process has the following defects in practice:

[0005] 1. Ultrafine powder refers to powder with a particle size of less than 5 microns. Nanoparticles have a small size effect, a large specific surface area and a macroscopic quantum tunneling effect, so nanopowders show many excellent properties that micron-level powders do not have. Ultrafine copper powder has a large specific surface area and a large number of surface active centers, and is an excellent catalyst in metallurgy and petrochemicals. In the hydrogenation and dehydrogenation reactions of polymers, ultrafine copper powder catalysts have extremely high activity and selectivity. In the process of acetylene polymerization to make conductive fibers, ultrafine copper powder is a very effective catalyst. In the process of automobile exhaust purification, ultrafine copper powder can be used as a catalyst to partially replace precious metals platinum and ruthenium, converting toxic carbon monoxide into carbon dioxide and nitric oxide into nitrogen dioxide. With the development of the electronics industry, ultrafine thick film slurries prepared from ultrafine copper powders will play an important role in large-scale integrated circuits. At the same time, the price is lower than that of precious metal silver powder and palladium powder, and has broad application prospects.

[0006] However, after the copper powder obtained by the above process is reduced, the fine powder is easy to stick together, and after the subsequent crushing of the bonded copper powder blocks, the copper powder blocks cannot be crushed into ultrafine copper powder. Therefore, the above process can barely meet the requirements when preparing powder materials with larger particle sizes, but it is not applicable to the process of producing ultrafine copper powder, and the efficiency of producing ultrafine copper powder is low;

[0007] 2. The above process needs to go through drying, reduction, crushing and other processes after atomization powder making, which is a relatively cumbersome process. Summary of the invention

[0008] The present invention aims to provide a preparation process of low-oxygen water atomized ultrafine copper powder, which is mainly used to solve the technical problems of low efficiency and complicated production process of ultrafine copper powder in the existing copper powder production process.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0010] A preparation process of low-oxygen water atomized ultrafine copper powder, characterized in that it comprises the following steps:

[0011] S1: Melting atomization: The electrolytic copper plate is heated to a molten state and then the copper powder is obtained through an atomization powder making system;

[0012] S2: Centrifugal dehydration: The copper powder atomized in step S1 is placed in a centrifuge for high-speed centrifugation to separate the atomized water and the copper powder;

[0013] S3: Antioxidant treatment: prepare a composite antioxidant, after the centrifugal dehydration process in step S2 is completed, use a water pump to inject the composite antioxidant into the centrifuge, open the three-way valve below the centrifuge to the circulation system, perform low-speed centrifugal washing for 15-40 minutes, perform antioxidant treatment on the surface of the copper powder, perform centrifugal separation after centrifugal washing, and then connect clean water to wash the copper powder. After washing, the copper powder is centrifuged and dehydrated at high speed to obtain copper powder;

[0014] S4: vacuum drying: low-temperature drying the copper powder after dehydration in step S3 at 40-70° C. in a vacuum drying oven;

[0015] S5: airflow sorting: the copper powder dried in step S4 is subjected to airflow sorting to select copper powder with a particle size less than 5 microns, i.e., ultrafine copper powder.

[0016] Preferably, in step S1, the electrolytic copper plate is heated to 1200-1500° C. to be in a molten state, and after melting, the molten copper metal liquid needs to be kept warm for a period of not less than 2 minutes.

[0017] Preferably, in step S1, the atomization water pressure of the atomization powder making system is 100-130 MPa.

[0018] Preferably, in step S3, the mass ratio of the composite antioxidant to the dehydrated copper powder in step S2 is 1:80-120.

[0019] Preferably, in step S3, the mass ratio of the composite antioxidant to the dehydrated copper powder in step S2 is 1:99.

[0020] Preferably, in step S3, the components of the composite antioxidant include one or more of potassium soap solution, protein hydrolyzate, polyvinyl pyrrolidone solution, BTA, and alcohol solution.

[0021] Preferably, in step S3, the composite antioxidant comprises the following components by mass fraction: 5-7% potassium soap solution, 7-15% protein hydrolyzate, 5-7% polyvinyl pyrrolidone solution, 18-28% BTA, and 50-60% alcohol solution. The above components are stirred and mixed and placed in a constant temperature water bath at 50° C. for insulation and standby use.

[0022] Preferably, the protein hydrolyzate is prepared by reflux hydrolysis of 6 mol / L HCI and gelatin, wherein the ratio of HCI to gelatin is controlled at 3.5:1, the hydrolysis time is 2 h, and the protein hydrolyzate is obtained by cooling and filtering after hydrolysis.

[0023] Preferably, in step S4, the vacuum degree in the vacuum drying oven is -0.1 to -0.03 MPa, and the drying time is 1 to 2 hours.

[0024] Preferably, in step S5, the metal powder after airflow sorting is fed into a mixer and mixed in a mass ratio of copper powder: BTA: alcohol solution = 100:0.5:1 for 10 minutes, and the copper powder is packaged after mixing.

[0025] Preferably, in step S5, airflow sorting is completed in an airflow classification fan, the frequency of the airflow classification fan is set to 45 Hz, the first-level classification frequency is 7 Hz, and the second-level frequency is 9 Hz, so as to classify the copper powder.

[0026] Working principle and beneficial effects of the present invention:

[0027] The core of this solution is to perform antioxidant treatment on the copper powder. The copper powder is repeatedly washed with a composite antioxidant, and the surface of the copper powder is subjected to antioxidant treatment to form a coating film to prevent the copper powder from coming into contact with oxygen during the manufacturing process and thus being oxidized, thereby increasing the oxygen content and affecting the quality of the copper powder. Specifically, this solution has the following beneficial effects:

[0028] 1. In this scheme, the copper powder obtained by atomization powder making is subjected to an antioxidant treatment, and a product with a qualified oxygen content can be obtained after the treatment, and the product can be directly dried and packaged. However, in the prior art, when copper powder is prepared by the reduction method, the copper powder after the reduction reaction will be sticky, and the bonded copper powder needs to be crushed again. However, most of the crushing devices on the market are difficult to crush the material to less than 5 microns. Therefore, the reduction method powder making is not suitable for preparing ultrafine copper powder. In this scheme, the atomization powder making process can usually prepare ultrafine copper powder below 5 microns, and this scheme does not use a reduction furnace to treat the copper powder. Due to the deoxidation treatment, there is no copper powder adhesion, so it has an advantage that cannot be ignored in the preparation of ultrafine copper powder, that is, with the same amount of raw materials, the amount of ultrafine copper powder produced by this scheme is larger than that of the existing process; and in this scheme, the antioxidant treatment is completed in a centrifuge, and there is no need to dehydrate and separate the copper powder and then perform antioxidant treatment in another device, which simplifies the production equipment. At the same time, the copper powder is just discharged from the atomization powder making system and is already in a wet state. This scheme performs antioxidant treatment on the copper powder in a wet environment, dehydrates it after treatment and directly dries it, which simplifies the production process and improves production efficiency. In summary, this scheme solves the technical problems of low efficiency in producing ultrafine copper powder and complicated production process in the existing copper powder production process.

[0029] 2. Copper is unstable in the air, so it is inevitable that copper powder will be oxidized in the air, especially in a humid environment. The surface of copper powder easily absorbs water vapor in the air to form a water film. Moreover, since the water film formed in the concave part of the particle surface is thick, less oxygen penetrates and the oxygen concentration is low, it becomes a micro anode, and a micro cathode is formed in the convex part where oxygen can easily reach. As a result, a battery effect of concentration difference is formed on the surface of copper powder, and the copper powder is gradually oxidized. The special feature of this scheme is that the undried copper powder just discharged from the powder making machine is subjected to corrosion inhibition treatment in a humid environment by a composite antioxidant. The main working principle of the composite antioxidant is to form a coating film on the surface of the copper powder particles, so that the surface of the copper powder is isolated from the oxygen in the air to achieve the purpose of anti-oxidation. Among them, the polyvinyl pyrrole in the composite antioxidant Alkyl ketone and potassium soap solution have excellent film-forming and adhesive properties, and are easy to form a coating film on the surface of copper powder particles; BTA is chemically adsorbed on the copper surface, and then forms a polymer film with copper oxide, and the addition of alcohol solution is mainly used to dissolve BTA; and the protein hydrolyzate has reducing, antioxidant and film-forming properties, and is coated on the surface of copper powder to inhibit corrosion of the copper powder and prevent the copper powder from being oxidized. Through precise ratio design, the above components work synergistically to produce a dense coating film to provide antioxidant protection for the copper powder, and a variety of coating films wrap the copper powder. In the subsequent drying process, the components work synergistically, making the coating film not easy to be damaged, which can effectively prevent the copper powder particles from being quickly oxidized during the drying process. The water content of the copper powder can be reduced to below 0.1% by vacuum drying. In the dry state, the copper powder has stable properties and is not easy to oxidize.

[0030] 3. Because copper powder is very easy to oxidize in a high temperature and humid environment, the dehydrated powder is vacuum dried at low temperature in this scheme. On the one hand, the drying rate is faster in a vacuum environment, and on the other hand, the contact between copper powder and oxygen is reduced, and the low temperature environment also slows down the oxidation of copper powder;

[0031] 4. This solution does not use the reduction process, which fundamentally avoids the oxidation of copper powder and can effectively ensure the surface smoothness and high sphericity of copper powder;

[0032] 5. In the traditional process, the atomizing water pressure is usually 20MPa. The ultrafine copper powder produced under such water pressure is relatively small. If the atomizing water pressure is increased, the output of ultrafine copper powder can be increased. In the traditional scheme, the copper powder is reduced, and a large amount of ultrafine copper powder is easy to stick together and agglomerate. After crushing, the copper powder particles cannot be crushed to less than 5 microns, so the output of ultrafine copper powder is still very small. The atomizing water pressure of this scheme is much higher than the traditional water pressure, and the anti-oxidation treatment of the copper powder replaces the reduction treatment in the traditional process, which avoids the stickiness of the copper powder during the reduction treatment process, and can retain the ultrafine copper powder produced in the atomizing powder making stage, which greatly increases the content of ultrafine copper powder in the finished product.

[0033] 6. In this scheme, BAT and alcohol solution are added again to the copper powder after sorting and before packaging, so that a layer of polymer film is evenly adsorbed on the surface of the copper powder, which provides antioxidant protection for the packaged copper powder and further improves the storage period of the copper powder. DETAILED DESCRIPTION

[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Embodiment 1:

[0036] A preparation process of low-oxygen water atomized ultrafine copper powder comprises the following steps:

[0037] S1: Melting and atomization: First, the electrolytic copper plate is cut into plates with a width of 5 cm. When the medium frequency furnace is heated, the electrolytic copper plate is placed in the furnace and heated to 1380°C. After the electrolytic copper plate is melted, it is kept warm for about 15 minutes. After the insulation, nitrogen is introduced into the atomization barrel to start atomization. The atomization water pressure of the atomization powder making system is 130MPa. After testing, the copper powder produced under this water pressure has the highest content of ultrafine copper powder, and the surface finish and sphericity are the best.

[0038] S2: Centrifugal dehydration: The copper powder atomized in step S1 is placed in a centrifuge for high-speed centrifugation to separate the atomized water and the copper powder; the centrifuge model used is PD800-N;

[0039] S3: Antioxidant treatment:

[0040] S301: preparing a composite antioxidant: mixing 6% potassium soap solution, 10% protein hydrolyzate, 6% polyvinyl pyrrolidone solution, 22% BTA, and 56% alcohol solution by mass, and placing in a constant temperature water bath at 50°C for heat preservation; wherein the protein hydrolyzate is prepared by reflux hydrolysis of 6 mol / L HCI and gelatin, the ratio of HCI to gelatin is controlled at 3.5:1, the hydrolysis time is 2 hours, and after hydrolysis, the protein hydrolyzate is obtained by cooling and filtering;

[0041] S302: corrosion inhibition treatment: after the centrifugal dehydration process in step S3 is completed, the prepared composite antioxidant is injected into the centrifuge by a water pump, the three-way valve below the centrifuge is opened to the circulation system, low-speed centrifugal washing is performed for 15 minutes, and the surface of the copper powder is subjected to antioxidant treatment. After centrifugal washing, centrifugal separation is performed, and clean water is connected to wash the copper powder for 20 minutes. After washing, the copper powder is subjected to high-speed centrifugal dehydration; wherein the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:99;

[0042] S4: vacuum drying: the copper powder dehydrated in step S3 is dried at low temperature in a vacuum drying oven, wherein the vacuum degree in the vacuum drying oven is -0.05 MPa, the drying temperature is 50° C., and the drying time is 1.5 h;

[0043] S5: airflow sorting: the copper powder dried in step S4 is sorted by an airflow classification fan, the frequency of the airflow classification fan is set to 45 Hz, the first-level classification frequency is 7 Hz, and the second-level frequency is 9 Hz, the copper powder is classified and screened, and the copper powder with a particle size less than 5 microns is selected, that is, the ultrafine copper powder;

[0044] S6: Packaging: The copper powders sorted in step S5 are mixed in a mass ratio of copper powder: BTA: alcohol solution = 100: 0.5: 1 for 10 minutes. After mixing, the copper powders are packaged.

[0045] Embodiment 2:

[0046] A preparation process of low-oxygen water atomized ultrafine copper powder comprises the following steps:

[0047] S1: Melting and atomization: First, the electrolytic copper plate is cut into plates with a width of 5 cm. When the medium frequency furnace is heated, the electrolytic copper plate is placed in the furnace and heated to 1380°C. After the electrolytic copper plate is melted, it is kept warm for about 20 minutes. After the insulation, nitrogen is introduced into the atomization barrel to start atomization. The atomization water pressure of the atomization powder making system is 110MPa. After testing, the copper powder produced under this water pressure has the highest content of ultrafine copper powder, and the surface finish and sphericity are the best.

[0048] S2: Centrifugal dehydration: The copper powder atomized in step S1 is placed in a centrifuge for high-speed centrifugation to separate the atomized water and the copper powder; the centrifuge model used is PD800-N;

[0049] S3: Antioxidant treatment:

[0050] S301: preparing a composite antioxidant: mixing 7% potassium soap solution, 9% protein hydrolyzate, 6% polyvinyl pyrrolidone solution, 22% BTA, and 56% alcohol solution by mass, and placing in a constant temperature water bath at 50°C for heat preservation; wherein the protein hydrolyzate is prepared by reflux hydrolysis of 6 mol / L HCI and gelatin, the ratio of HCI to gelatin is controlled at 3.5:1, the hydrolysis time is 2 hours, and after hydrolysis, the protein hydrolyzate is obtained by cooling and filtering;

[0051] S302: corrosion inhibition treatment: after the centrifugal dehydration process in step S3 is completed, the prepared composite antioxidant is injected into the centrifuge by a water pump, the three-way valve below the centrifuge is opened to the circulation system, low-speed centrifugal washing is performed for 20 minutes, and the surface of the copper powder is subjected to antioxidant treatment. After the centrifugal washing, centrifugal separation is performed, and clean water is connected to wash the copper powder for 20 minutes. After washing, the copper powder is subjected to high-speed centrifugal dehydration; wherein the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:80;

[0052] S4: vacuum drying: the copper powder dehydrated in step S3 is dried at low temperature in a vacuum drying oven, wherein the vacuum degree in the vacuum drying oven is -0.08 MPa, the drying temperature is 60° C., and the drying time is 1.4 h;

[0053] S5: airflow sorting: the copper powder dried in step S4 is sorted by an airflow classification fan, the frequency of the airflow classification fan is set to 45 Hz, the first-level classification frequency is 7 Hz, and the second-level frequency is 10 Hz. The copper powder is graded and screened to obtain copper powders of different particle sizes, including ultrafine copper powder.

[0054] S6: Packaging: The copper powders sorted in step S5 are mixed in a mass ratio of copper powder: BTA: alcohol solution = 100: 0.5: 1 for 10 minutes. After mixing, the copper powders are packaged.

[0055] Embodiment 3:

[0056] A preparation process of low-oxygen water atomized ultrafine copper powder comprises the following steps:

[0057] S1: Melting and atomization: First, the electrolytic copper plate is cut into plates with a width of 5 cm. When the medium frequency furnace is heated, the electrolytic copper plate is placed in the furnace and heated to 1380°C. After the electrolytic copper plate is melted, it is kept warm for about 25 minutes. After the insulation, nitrogen is introduced into the atomization barrel to start atomization. The atomization water pressure of the atomization powder making system is 100 MPa. After testing, the copper powder produced under this water pressure has the highest content of ultrafine copper powder, and the best surface finish and sphericity.

[0058] S2: Centrifugal dehydration: The copper powder atomized in step S1 is placed in a centrifuge for high-speed centrifugation to separate the atomized water and the copper powder; the centrifuge model used is PD800-N;

[0059] S3: Antioxidant treatment:

[0060] S301: preparing a composite antioxidant: mixing 7% potassium soap solution, 12% protein hydrolyzate, 6% polyvinyl pyrrolidone solution, 21% BTA, and 54% alcohol solution by mass, and placing in a constant temperature water bath at 50°C for heat preservation; wherein the protein hydrolyzate is prepared by reflux hydrolysis of 6 mol / L HCI and gelatin, the ratio of HCI to gelatin is controlled at 3.5:1, the hydrolysis time is 2 hours, and after hydrolysis, the protein hydrolyzate is obtained by cooling and filtering;

[0061] S302: corrosion inhibition treatment: after the centrifugal dehydration process in step S3 is completed, the prepared composite antioxidant is injected into the centrifuge by a water pump, the three-way valve below the centrifuge is opened to the circulation system, low-speed centrifugal washing is performed for 15 minutes, and the surface of the copper powder is subjected to antioxidant treatment. After centrifugal washing, centrifugal separation is performed, and clean water is connected to wash the copper powder for 20 minutes. After washing, the copper powder is subjected to high-speed centrifugal dehydration; wherein the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:120;

[0062] S4: vacuum drying: the copper powder dehydrated in step S3 is dried at low temperature in a vacuum drying oven, wherein the vacuum degree in the vacuum drying oven is -0.08 MPa, the drying temperature is 70° C., and the drying time is 1.3 h;

[0063] S5: airflow sorting: the copper powder dried in step S4 is sorted by an airflow classification fan, the frequency of the airflow classification fan is set to 45 Hz, the first-level classification frequency is 7 Hz, and the second-level frequency is 10 Hz. The copper powder is graded and screened to obtain copper powders of different particle sizes, including ultrafine copper powder.

[0064] S6: Packaging: The copper powders sorted in step S5 are mixed in a mass ratio of copper powder: BTA: alcohol solution = 100: 0.5: 1 for 10 minutes. After mixing, the copper powders are packaged.

[0065] Comparative Example 1:

[0066] The difference from Example 1 is that the antioxidant treatment of the copper powder in step S3 is removed, and the original step S4 directly performs vacuum low-temperature drying on the copper powder after centrifugal separation in the original step S2.

[0067] Comparative Example 2:

[0068] A preparation process of low-oxygen water atomized ultrafine copper powder comprises the following steps:

[0069] S1: Melting and atomization: First, the electrolytic copper plate is cut into plates with a width of 5 cm. When the medium frequency furnace is heated, the electrolytic copper plate is placed in the furnace and heated to 1380°C. After the electrolytic copper plate is melted, it is kept warm for about 15 minutes. After the insulation, nitrogen is introduced into the atomization barrel to start atomization. The atomization water pressure of the atomization powder making system is 130MPa. After testing, the copper powder produced under this water pressure has the highest content of ultrafine copper powder, and the surface finish and sphericity are the best.

[0070] S2: Centrifugal dehydration: The copper powder atomized in step S1 is placed in a centrifuge for high-speed centrifugation to separate the atomized water and the copper powder; the centrifuge model used is PD800-N;

[0071] S3: Reduction treatment: The powder produced in step S2 is subjected to reduction treatment in a reduction furnace in a mixed atmosphere of hydrogen and nitrogen, the reduction time is 1.4 h, and the reduction temperature is 550° C.;

[0072] S4: vacuum drying: the copper powder treated in step S3 is dried at low temperature in a vacuum drying oven, wherein the vacuum degree in the vacuum drying oven is -0.05 MPa, the drying temperature is 50° C., and the drying time is 1.5 h;

[0073] S5: airflow sorting: the copper powder dried in step S4 is sorted by an airflow classification fan, the frequency of the airflow classification fan is set to 45 Hz, the first-level classification frequency is 7 Hz, and the second-level frequency is 10 Hz. The copper powder is graded and screened to obtain copper powders of different particle sizes, including ultrafine copper powder.

[0074] Comparative Example 3:

[0075] Different from Example 1, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:50.

[0076] Comparative Example 4:

[0077] Different from Example 1, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:60.

[0078] Comparative Example 5:

[0079] Different from Example 1, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:70.

[0080] Comparative Example 6:

[0081] Different from Example 1, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:130.

[0082] Comparative Example 7:

[0083] Different from Example 1, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:140.

[0084] Comparative Example 8:

[0085] Different from Example 1, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is 1:150.

[0086] The finished copper powders in Examples 1-3 and Comparative Examples 1-2 were tested for performance, and the test results are as follows:

[0087]

[0088]

[0089] From the above data, we can know that:

[0090] 1. Under the same atomizing water pressure, in the process of reducing the copper powder (Comparative Example 2), the content of ultrafine copper powder is much lower than that of the ultrafine copper powder produced by this scheme, which proves that the process used in Comparative Example 2 greatly reduces the content of ultrafine copper powder due to the adhesion of ultrafine copper powder, while this scheme uses antioxidant treatment instead of the reduction treatment in Comparative Example 2, which effectively avoids the adhesion of ultrafine copper powder and is suitable for high-yield ultrafine copper powder;

[0091] 2. When the copper powder is not subjected to antioxidant treatment (Comparative Example 1), the oxygen content of the copper powder is much greater than that of Comparative Example 2 and Examples 1-3, indicating that antioxidant treatment of the copper powder can effectively reduce the oxygen content in the finished copper powder: Compared with Comparative Example 2, in Examples 1-3, the oxygen content in the finished copper powder is about 650 to 840 ppm, indicating that this scheme is effective in reducing the oxygen content of the finished copper powder.

[0092] The finished copper powders in Examples 1-3 and Comparative Examples 1-8 were tested for performance, and the test results are as follows:

[0093] Case Mass ratio of composite antioxidant to copper powder Copper powder oxygen content (ppm) Comparative Example 3 1:50 900 Comparative Example 4 1:60 830 Comparative Example 5 1:70 850 Example 2 1:80 840 Example 1 1:99 650 Example 3 1:120 730 Comparative Example 6 1:130 750 Comparative Example 7 1:140 720 Comparative Example 8 1:150 760 Comparative Example 1 / 4200 Comparative Example 2 / 550

[0094] From the above data, we can know that:

[0095] 1. With the reduction of composite antioxidant, the oxygen content of copper powder gradually increased, proving that when the coating film did not completely cover the copper powder, the copper powder was exposed to the air and oxidized;

[0096] 2. When the amount of the composite antioxidant added is large (the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is greater than 1:80, such as comparative examples 3-5), it can be observed that the oxygen content of the copper powder does not decrease, but increases. The reason is mainly because it is difficult to fully rinse the copper powder after the composite antioxidant is adjusted in too much amount, and the composite antioxidant contains oxygen ions. If there is too much residual oxidant on the surface of the copper powder, the oxygen content of the copper powder will also increase. At the same time, when the amount of the composite antioxidant added is large, the antioxidant protection of the copper powder is not enhanced;

[0097] When the amount of the composite antioxidant added is small (the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is less than 1:80, such as comparative examples 6-8), the composite antioxidant has a poor coating effect on the copper powder, resulting in excessive exposure of the copper powder surface to the air and oxidation before drying;

[0098] Therefore, the mass ratio of the composite antioxidant to the copper powder after dehydration in step S2 is recommended to be between 1:80-120, and the optimal ratio is 1:99, and the oxygen content of the copper powder is controlled between 650 and 840 ppm.

[0099] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A process for preparing low-oxygen water atomized ultrafine copper powder, characterized in that: The steps include: S1: Melting atomization: The electrolytic copper plate is heated to a molten state and then the copper powder is obtained through an atomization powder making system; S2: Centrifugal dehydration: The copper powder atomized in step S1 is placed in a centrifuge for high-speed centrifugation to separate the atomized water and the copper powder; S3: Antioxidant treatment: prepare a composite antioxidant, after the centrifugal dehydration process in step S2 is completed, use a water pump to inject the composite antioxidant into the centrifuge, open the three-way valve below the centrifuge to the circulation system, perform low-speed centrifugal washing for 15-40 minutes, perform antioxidant treatment on the surface of the copper powder, perform centrifugal separation after centrifugal washing, and then connect clean water to wash the copper powder. After washing, the copper powder is centrifuged and dehydrated at high speed to obtain copper powder; S4: vacuum drying: low-temperature drying the copper powder after dehydration in step S3 at 40-70° C. in a vacuum drying oven; S5: airflow sorting: the copper powder dried in step S4 is subjected to airflow sorting to select copper powder with a particle size less than 5 microns, i.e., ultrafine copper powder.

2. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In the step S1, the electrolytic copper plate is heated to 1200-1500° C. to be in a molten state. After melting, the molten copper metal liquid needs to be kept warm for a period of not less than 2 minutes.

3. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In the step S1, the atomization water pressure of the atomization powder making system is 100-130 MPa.

4. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In the step S3, the mass ratio of the composite antioxidant to the copper powder dehydrated in the step S2 is 1:80-120.

5. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In the step S3, the mass ratio of the composite antioxidant to the copper powder dehydrated in the step S2 is 1:

99.

6. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In step S3, the ingredients of the composite antioxidant include one or more of potassium soap solution, protein hydrolyzate, polyvinyl pyrrolidone solution, BTA, and alcohol solution.

7. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In step S3, the composite antioxidant comprises the following components by mass fraction: 5-7% potassium soap solution, 7-15% protein hydrolyzate, 5-7% polyvinyl pyrrolidone solution, 18-28% BTA, and 50-60% alcohol solution. The above components are stirred and mixed, and then placed in a constant temperature water bath at 50° C. to keep warm for use.

8. A process for preparing low-oxygen water atomized ultrafine copper powder according to claim 6 or 7, characterized in that: The protein hydrolyzate is prepared by reflux hydrolysis of 6 mol / L HCI and gelatin, wherein the ratio of HCI to gelatin is controlled at 3.5:1, the hydrolysis time is 2 hours, and the protein hydrolyzate is obtained by cooling and filtering after hydrolysis.

9. The process for preparing a low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In step S4, the vacuum degree in the vacuum drying oven is -0.1 to -0.03 MPa, and the drying time is 1 to 2 hours.

10. The process for preparing low-oxygen water atomized ultrafine copper powder according to claim 1, characterized in that: In the step S5, the metal powder after airflow sorting is fed into a mixer and mixed in a mass ratio of copper powder: BTA: alcohol solution = 100: 0.5: 1 for 10 minutes. After mixing, the copper powder is packaged.