High-crack-resistance solid welding wire and preparation method thereof

By adding titanium nitride, titanium oxide and its adsorbents to the welding wire and performing electron beam irradiation, the crack problem during welding process is solved, high crack resistance and high strength welding wire effect is achieved, and the welding quality and structure are improved security.

CN118951485AActive Publication Date: 2024-11-15SHENYANG ZHONGYING HI TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411341227.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-15
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Existing welding wires are difficult to meet the requirements of high crack resistance during welding, especially in the welding of key structures such as bridges and pressure vessels, cracks are easily generated, affecting the safety and stability of the structure.

Method used

High crack resistance solid welding wire is formed by adding titanium nitride and titanium oxide and its adsorb into the wire substrate and electron beam irradiation is performed after melting and drawing. Titanium oxide adsorbs copper, lead and nickel under ultraviolet light, improving surface adsorption capacity and photocatalytic activity. Titanium nitride and titanium oxide are melt blended with welding wire substrate, destroying the cladding structure, forming a tight bond, and electron beam irradiation forms nano Precipitate the phase to improve the crack resistance of the welding wire.

Benefits of technology

The high crack resistance and high strength effect of the welding wire is achieved, which reduces the occurrence of cracks and defects during welding, improves the strength and toughness of the welding joints, and enhances the mechanical properties of the welding wire.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059755900000061
    Figure BDA0005059755900000061
  • Figure BDA0005059755900000071
    Figure BDA0005059755900000071
Patent Text Reader

Abstract

The invention discloses a high-crack-resistance solid welding wire and a preparation method thereof, and relates to the technical field of welding wires. Titanium nitride, titanium oxide and adsorbents thereof are added into a welding wire base material, and the high-crack-resistance solid welding wire is prepared through electron beam irradiation after wire drawing. Firstly, titanium oxide adsorbs copper, lead and nickel under ultraviolet irradiation, so that the titanium oxide has the capability of capturing free hydrogen atoms during welding, and hydrogen cracks are reduced; secondly, the welding wire base material and the alloy are subjected to melt blending and wire drawing and then subjected to electron beam irradiation, and the high-crack-resistance solid welding wire is obtained; the coating structure of titanium oxide can be damaged by high temperature, and metal elements on the surface are tightly combined with titanium atoms, so that the generation of defects such as cracks can be reduced; a nano precipitated phase can be formed in the welding wire through electron beam irradiation, meanwhile, the added alloy can promote formation of acicular ferrite, crack propagation is effectively prevented, and high crack resistance of the welding wire is achieved. The prepared high-crack-resistance solid welding wire has the effects of high crack resistance and high strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding wires, in particular to a high-crack-resistant solid welding wire and a preparation method thereof. Background Art

[0002] As domestic and foreign engineering machinery, coal mining machinery, marine equipment, hydropower equipment, etc. develop towards high quality, high strength, high toughness, large-scale and light weight, welding metal materials have expanded from traditional carbon steel and low alloy steel to high strength fine grain alloy. Welding wire is a metal wire welding material used as filler metal or as a conductor at the same time. In gas welding and tungsten inert gas shielded arc welding, welding wire is used as filler metal; in submerged arc welding, electroslag welding and other metallurgical gas shielded arc welding, welding wire is both filler metal and conductive electrode. At present, the variety of welding wire is single, which is far from meeting the growing demand for steel plate shielded welding.

[0003] During the welding process, cracks are prone to occur in the weld area due to various factors such as material thermal stress, chemical composition differences, improper welding process, etc. For the welding of certain special materials, traditional welding wires may be difficult to meet their crack resistance requirements. In the welding of key structures (such as bridges, pressure vessels, etc.), the crack resistance of the weld is directly related to the safety and stability of the structure.

[0004] Therefore, the present invention provides a high crack resistance solid welding wire and a preparation method thereof, which has the effects of high crack resistance and high strength. Summary of the invention

[0005] The object of the present invention is to provide a high crack resistance solid welding wire and a preparation method thereof, so as to solve the problems existing in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: a high crack-resistant solid welding wire, which is prepared by adding titanium nitride and titanium oxide and their adsorbates to a welding wire substrate, melting and drawing, and then irradiating with an electron beam.

[0007] Furthermore, the titanium oxide and the adsorbate thereof are prepared by adding a solution containing copper, lead and nickel metal ions into a titanium dioxide solution under ultraviolet light and then drying the solution.

[0008] Furthermore, the solution containing copper, lead and nickel metal ions is a copper sulfate solution, a lead acetate solution and a nickel sulfate solution.

[0009] Furthermore, a method for preparing a crack-resistant solid welding wire comprises the following preparation steps:

[0010] (1) Mix titanium dioxide and water in a mass ratio of 1.5 to 2:10, stir at 400 to 600 r / min for 1 to 3 hours, add titanium nitride 1 to 1.5 times the mass of titanium dioxide, stir at 600 to 700 r / min for 3 to 5 hours, and disperse with a 22KW high-speed disperser for 3 to 5 hours to obtain a titanium nitride-titanium dioxide suspension;

[0011] (2) mixing a copper sulfate solution, a lead acetate solution, a nickel sulfate solution and a titanium nitride-titanium dioxide suspension in a mass ratio of 0.3-0.5:0.3-0.5:0.3-0.5:1, stirring at 600-700 r / min for 1-2 hours, irradiating under ultraviolet light for 6-10 hours, filtering out the solid, and drying it in a vacuum drying oven at 100-120° C. and 50-60 kPa for 2-3 hours to obtain titanium nitride and titanium oxide and their adsorbates;

[0012] (3) Titanium nitride, titanium oxide and their adsorbates are mixed with a welding wire substrate at a mass ratio of 0.5 to 0.8:10 and then melted together. After smelting in a vacuum induction furnace, forging, hot rolling, drawing, annealing, and layer winding, and then electron beam irradiation, a high crack-resistant solid welding wire can be obtained.

[0013] Furthermore, in the step (1), the particle size of titanium dioxide is 50 to 80 nm, and the particle size of titanium nitride is 50 to 80 nm.

[0014] Furthermore, in step (2), the copper sulfate solution is a copper sulfate aqueous solution with a concentration of 40 to 60 g / L, the lead acetate solution is a lead acetate aqueous solution with a concentration of 40 to 60 g / L, and the nickel sulfate solution is a nickel sulfate aqueous solution with a concentration of 40 to 60 g / L.

[0015] Furthermore, the welding wire substrate in step (3) is molten steel smelted from desulfurized molten iron, and the molten steel is cast into a continuous casting billet.

[0016] Furthermore, the chemical composition of the desulfurized iron water includes, by weight percentage: C: 0.05% ~ 0.3%, Mn: 2.0% ~ 2.5%, Si: 0.20% ~ 0.70%, P: 0.003% ~ 0.006%, S: 0.002% ~ 0.005%, Cr: 2.1% ~ 2.5%, Mo ≤ 0.15%, N: 0.08% ~ 0.30%, V: 0.050% ~ 0.100%, W: 0.020% ~ 0.060%, B: 0.010% ~ 0.020%, and the rest is Fe and other inevitable impurities.

[0017] Furthermore, in the step (3), the smelting temperature is 825-850°C, the time is 10-20 min, the forging temperature is 650-750°C, the hot rolling temperature is 400-450°C, the extrusion speed is 0.5-2 m / min, the drawing passes are 10-25 passes, and after each drawing pass, the temperature is 300-350°C and annealed for 10-20 min, so that the diameter of the solid welding wire is 1.0-1.5 mm.

[0018] Furthermore, in the step (3), the electron beam irradiation is performed at an irradiation voltage of 3 MeV, a dose rate of 20 kGy / pass, and an absorbed radiation dose of 100 to 125 kgy.

[0019] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0020] The invention adds titanium nitride and titanium oxide and adsorbates thereof into a welding wire substrate, draws the wire and then irradiates the wire with electron beam to obtain a high crack resistance solid welding wire, so as to achieve the effects of high crack resistance and high strength.

[0021] First, under ultraviolet light, titanium oxide adsorbs copper, lead and nickel. Ultraviolet light can effectively improve the surface adsorption capacity of titanium oxide and stimulate the photocatalytic activity of titanium oxide, so that it has the ability to capture free hydrogen atoms during welding, reduce the generation of hydrogen cracks, and improve the quality of welding. At the same time, the presence of adsorbed copper, lead and nickel can further improve the mechanical properties and welding effect of the welding wire.

[0022] Secondly, titanium nitride, titanium oxide and their adsorbates are added to the welding wire substrate, and after wire drawing, they are subjected to electron beam irradiation to obtain a solid welding wire with high crack resistance. When titanium nitride, titanium oxide and their adsorbates are melt-blended with the welding wire substrate, the high temperature will destroy the coating structure of titanium oxide, and the metal elements on the surface will melt first, diffuse into the titanium oxide, and form a tight bond with the titanium atoms. The tight bond of alloy atoms helps to reduce defects such as spatter and pores during welding, and will also form a stronger bond with the base metal during welding, which helps to improve the strength and toughness of the welded joint and reduce the occurrence of defects such as cracks. Electron beam irradiation can form a nano-precipitated phase in the welding wire. The nano-precipitated phase can not only improve the strength and hardness of the welding wire, but also capture free hydrogen atoms, thereby improving the crack resistance of the welding wire. The titanium oxide, titanium nitride and nickel in the welding wire can promote the formation of acicular ferrite during the wire drawing process, which can improve the strength and toughness of the welding wire, effectively prevent crack propagation, and achieve high crack resistance of the welding wire. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0024] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the high crack resistance solid welding wire prepared in the following examples are as follows:

[0025] High strength: The high crack resistance solid welding wires prepared in the embodiment and the comparative example of the same mass were tested for tensile properties and bending properties in accordance with GB / T2652-2022 "Destructive test of welds on metallic materials - Longitudinal tensile test of weld metal of fusion weld joint".

[0026] High crack resistance: The high crack resistance solid welding wires prepared in the embodiment and the comparative example of the same mass were welded under the same conditions and then placed in an alternating high temperature and high humidity environment for 20 days to observe whether cracks would occur after welding.

[0027] Example 1

[0028] A method for preparing a high crack-resistant solid welding wire comprises the following preparation steps:

[0029] (1) Titanium dioxide with a particle size of 50 nm and water were mixed at a mass ratio of 1.5:10, stirred at 400 r / min for 1 h, titanium nitride with a particle size of 50 nm and a mass of 1 times that of titanium dioxide was added, stirred at 600 r / min for 3 h, and dispersed with a 22KW high-speed disperser for 3 h to obtain a titanium nitride-titanium dioxide suspension;

[0030] (2) 40 g / L copper sulfate aqueous solution, 40 g / L lead acetate aqueous solution, 40 g / L nickel sulfate aqueous solution and titanium nitride-titanium dioxide suspension were mixed in a mass ratio of 0.3:0.3:0.3:1, stirred at 600 r / min for 1 hour, irradiated under ultraviolet light for 6 hours, filtered to obtain solids, and dried in a vacuum drying oven at 100°C and 50 kPa for 2 hours to obtain titanium nitride and titanium oxide and their adsorbates;

[0031] (3) The chemical composition of the desulfurized iron water includes, by weight percentage, C: 0.05%, Mn: 2.0%, Si: 0.20%, P: 0.003%, S: 0.002%, Cr: 2.1%, Mo: 0.08%, N: 0.08%, V: 0.050%, W: 0.020%, B: 0.010%, and the remainder is Fe and other inevitable impurities. The desulfurized iron water is smelted into molten steel, and the molten steel is cast into continuous casting billets to obtain welding wire substrates;

[0032] (4) Titanium nitride and titanium oxide and their adsorbates are mixed with a welding wire substrate in a mass ratio of 0.5:10 and then melted together. The mixture is subjected to a vacuum induction furnace smelting, forging, hot rolling, drawing, annealing, and layer winding process. The smelting temperature is 825°C, the time is 10 min, the forging temperature is 650°C, the hot rolling temperature is 400°C, the extrusion speed is 0.5 m / min, the drawing passes are 10 times, and each drawing pass is annealed at 300°C for 10 min to obtain a solid welding wire with a diameter of 1.0 mm. The solid welding wire is then irradiated with an electron beam at an irradiation voltage of 3 MeV and a dose rate of 20 kGy / pass, and an absorbed radiation dose of 100 kgy to obtain a high crack-resistant solid welding wire.

[0033] Example 2

[0034] A method for preparing a high crack-resistant solid welding wire comprises the following preparation steps:

[0035] (1) Titanium dioxide with a particle size of 70 nm and water were mixed at a mass ratio of 1.7:10, stirred at 500 r / min for 2 h, titanium nitride with a particle size of 70 nm and a mass of 1.3 times that of titanium dioxide was added, stirred at 650 r / min for 4 h, and dispersed with a 22KW high-speed disperser for 4 h to obtain a titanium nitride-titanium dioxide suspension;

[0036] (2) 50 g / L of copper sulfate aqueous solution, 50 g / L of lead acetate aqueous solution, 50 g / L of nickel sulfate aqueous solution and titanium nitride-titanium dioxide suspension were mixed in a mass ratio of 0.4:0.4:0.4:1, stirred at 650 r / min for 1.5 h, irradiated under ultraviolet light for 8 h, filtered to obtain solid, and dried in a vacuum drying oven at 110° C. and 55 kPa for 2.5 h to obtain titanium nitride and titanium oxide and their adsorbates;

[0037] (3) The chemical composition of the desulfurized iron water includes, by weight percentage, C: 0.25%, Mn: 2.3%, Si: 0.50%, P: 0.004%, S: 0.004%, Cr: 2.3%, Mo: 0.1%, N: 0.15%, V: 0.08%, W: 0.04%, B: 0.015%, and the rest is Fe and other inevitable impurities. The desulfurized iron water is smelted into molten steel, and the molten steel is cast into continuous casting billets to obtain welding wire substrates;

[0038] (4) Titanium nitride and titanium oxide and their adsorbates are mixed with a welding wire substrate in a mass ratio of 0.6:10 and then melted together. The mixture is subjected to a vacuum induction furnace smelting, forging, hot rolling, drawing, annealing, and layer winding process. The smelting temperature is 840°C, the time is 15 min, the forging temperature is 700°C, the hot rolling temperature is 430°C, the extrusion speed is 1.5 m / min, the drawing passes are 18 times, and each drawing pass is annealed at 325°C for 15 min. The diameter of the obtained solid welding wire is 1.3 mm. The solid welding wire is then irradiated with an electron beam at an irradiation voltage of 3 MeV and a dose rate of 20 kGy / pass, and an absorbed radiation dose of 110 kgy to obtain a high crack resistance solid welding wire.

[0039] Example 3

[0040] A method for preparing a high crack-resistant solid welding wire comprises the following preparation steps:

[0041] (1) Titanium dioxide with a particle size of 50 to 80 nm and water were mixed at a mass ratio of 2:10, stirred at 600 r / min for 3 h, titanium nitride with a particle size of 80 nm and a mass of 1.5 times that of titanium dioxide was added, stirred at 700 r / min for 5 h, and dispersed with a 22KW high-speed disperser for 5 h to obtain a titanium nitride-titanium dioxide suspension;

[0042] (2) A 60 g / L copper sulfate aqueous solution, a 60 g / L lead acetate aqueous solution, a 60 g / L nickel sulfate aqueous solution and a titanium nitride-titanium dioxide suspension were mixed in a mass ratio of 0.5:0.5:0.5:1, stirred at 700 r / min for 2 h, irradiated under ultraviolet light for 10 h, filtered to obtain a solid, and dried in a vacuum drying oven at 120° C. and 60 kPa for 3 h to obtain titanium nitride and titanium oxide and their adsorbates;

[0043] (3) The chemical composition of the desulfurized molten iron includes, by weight percentage, C: 0.3%, Mn: 2.5%, Si: 0.70%, P: 0.006%, S: 0.005%, Cr: 2.5%, Mo: 0.15%, N: 0.30%, V: 0.100%, W: 0.060%, B: 0.020%, and the remainder is Fe and other inevitable impurities. The desulfurized molten iron is smelted into molten steel, which is then cast into continuous casting billets to obtain welding wire substrates;

[0044] (4) Titanium nitride and titanium oxide and their adsorbates are mixed with a welding wire substrate in a mass ratio of 0.8:10 and then melted together. The mixture is subjected to a vacuum induction furnace smelting, forging, hot rolling, drawing, annealing, and layer winding process. The smelting temperature is 850°C, the time is 20 min, the forging temperature is 750°C, the hot rolling temperature is 450°C, the extrusion speed is 2 m / min, the drawing passes are 25 times, and each drawing pass is annealed at 350°C for 20 min. The diameter of the obtained solid welding wire is 1.5 mm. The solid welding wire with high crack resistance is then irradiated with an electron beam at an irradiation voltage of 3 MeV and a dose rate of 20 kGy / pass, and an absorbed radiation dose of 125 kgy.

[0045] Comparative Example 1

[0046] The difference between Comparative Example 1 and Example 1 is that step (1) is omitted, and step (3) is changed to: 40 g / L copper sulfate aqueous solution, 40 g / L lead acetate aqueous solution, and 40 g / L nickel sulfate aqueous solution are mixed in a mass ratio of 1:1:1, stirred at 600 r / min for 1 h, irradiated under ultraviolet light for 6 h, filtered to obtain a solid, and dried in a vacuum drying oven at 100° C. and 50 kPa for 2 h to obtain an alloy additive; the remaining steps are the same as those in Example 1.

[0047] Comparative Example 2

[0048] The difference between Comparative Example 2 and Example 1 is that step (2) is different. Step (2) is changed to: 40 g / L copper sulfate aqueous solution, 40 g / L lead acetate aqueous solution, 40 g / L nickel sulfate aqueous solution and titanium nitride-titanium dioxide suspension are mixed in a mass ratio of 0.3:0.3:0.3:1, stirred at 600 r / min for 1 h, filtered to obtain the solid, and placed in a vacuum drying oven at 100°C and 50 kPa for 2 h to obtain titanium nitride and titanium oxide and their adsorbates; the remaining steps are the same as those in Example 1.

[0049] Comparative Example 3

[0050] The difference between Comparative Example 3 and Example 1 is that step (2) is different. Step (2) is changed to: the titanium nitride-titanium dioxide suspension is placed in a vacuum drying oven at 100°C and 50 kPa for 2 hours to obtain titanium nitride and titanium oxide and their adsorbates; the remaining steps are the same as Example 1.

[0051] Comparative Example 4

[0052] The difference between Comparative Example 4 and Example 1 lies in step (4). Step (4) is changed to: titanium nitride, titanium oxide and their adsorbates are mixed with a welding wire substrate in a mass ratio of 0.5:10 and then smelted together, and subjected to vacuum induction furnace smelting, forging, hot rolling, drawing, annealing and layer winding processes. The smelting temperature is 825°C, the time is 10 min, the forging temperature is 650°C, the hot rolling temperature is 400°C, the extrusion speed is 0.5 m / min, the drawing passes are 10 times, and each drawing pass is 300°C and annealed for 10 min to obtain a high crack resistance solid welding wire with a diameter of 1.0 mm. The remaining steps are the same as Example 1.

[0053] Effect example

[0054] Table 1 below shows the performance analysis results of high crack resistance solid welding wires using Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.

[0055] Table 1

[0056]

[0057]

[0058] From the comparison of the experimental data of the embodiment and the comparative example, it can be found that the present invention allows titanium oxide to adsorb copper, lead and nickel under ultraviolet light, and ultraviolet light can effectively improve the surface adsorption capacity of titanium oxide and stimulate the photocatalytic activity of titanium oxide, so that it has the ability to capture free hydrogen atoms during welding, reduce the generation of hydrogen cracks, and improve the quality of welding; at the same time, the presence of the adsorbed copper, lead and nickel can further improve the mechanical properties and welding effect of the welding wire. Moreover, when titanium nitride, titanium oxide and their adsorbates are melted and blended with the welding wire substrate, the high temperature will destroy the coating structure of titanium oxide, and the metal elements on the surface will melt first, diffuse into the titanium oxide, and form a close bond with the titanium atoms. The close bonding of alloy atoms helps to reduce defects such as spatter and pores during welding, and will also form a stronger bond with the substrate metal during welding, which helps to improve the strength and toughness of the welded joint and reduce the occurrence of defects such as cracks; electron beam irradiation can form nano-precipitated phases in the welding wire, which can not only improve the strength and hardness of the welding wire, but also capture free hydrogen atoms, thereby improving the crack resistance of the welding wire. The titanium oxide, titanium nitride and nickel in the welding wire can promote the formation of acicular ferrite during the wire drawing process, which can improve the strength and toughness of the welding wire, effectively prevent crack propagation, and achieve high crack resistance of the welding wire.

[0059] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A high crack resistance solid welding wire, characterized in that: The high crack resistance solid welding wire is prepared by adding titanium nitride and titanium oxide and adsorbates thereof into a welding wire substrate, melting and drawing the wire, and then irradiating the wire with electron beams.

2. A high crack resistance solid welding wire according to claim 1, characterized in that: The titanium oxide and the adsorbent thereof are prepared by adding a solution containing copper, lead and nickel metal ions into a titanium dioxide solution under ultraviolet light irradiation and then drying the solution.

3. A high crack resistance solid welding wire according to claim 2, characterized in that: The solutions containing copper, lead and nickel metal ions are copper sulfate solution, lead acetate solution and nickel sulfate solution.

4. A method for preparing a high crack resistance solid welding wire, characterized in that: The method comprises the following preparation steps: (1) Mix titanium dioxide and water in a mass ratio of 1.5 to 2:10, stir at 400 to 600 r / min for 1 to 3 hours, add titanium nitride 1 to 1.5 times the mass of titanium dioxide, stir at 600 to 700 r / min for 3 to 5 hours, and disperse with a 22KW high-speed disperser for 3 to 5 hours to obtain a titanium nitride-titanium dioxide suspension; (2) mixing a copper sulfate solution, a lead acetate solution, a nickel sulfate solution and a titanium nitride-titanium dioxide suspension in a mass ratio of 0.3-0.5:0.3-0.5:0.3-0.5:1, stirring at 600-700 r / min for 1-2 hours, irradiating under ultraviolet light for 6-10 hours, filtering out the solid, and drying it in a vacuum drying oven at 100-120° C. and 50-60 kPa for 2-3 hours to obtain titanium nitride and titanium oxide and their adsorbates; (3) Titanium nitride, titanium oxide and their adsorbates are mixed with a welding wire substrate at a mass ratio of 0.5 to 0.8:10 and then melted together. After smelting in a vacuum induction furnace, forging, hot rolling, drawing, annealing, and layer winding, and then electron beam irradiation, a high crack-resistant solid welding wire can be obtained.

5. The method for preparing a high crack resistance solid welding wire according to claim 4, characterized in that: In the step (1), the particle size of titanium dioxide is 50 to 80 nm, and the particle size of titanium nitride is 50 to 80 nm.

6. The method for preparing a high crack resistance solid welding wire according to claim 4, characterized in that: In the step (2), the copper sulfate solution is a copper sulfate aqueous solution with a concentration of 40 to 60 g / L, the lead acetate solution is a lead acetate aqueous solution with a concentration of 40 to 60 g / L, and the nickel sulfate solution is a nickel sulfate aqueous solution with a concentration of 40 to 60 g / L.

7. The method for preparing a high crack resistance solid welding wire according to claim 4, characterized in that: The welding wire substrate in step (3) is molten steel smelted from desulfurized molten iron, and the molten steel is cast into a continuous casting billet.

8. The method for preparing a high crack resistance solid welding wire according to claim 7, characterized in that: The chemical components in the desulfurized iron water include, by weight percentage: C: 0.05%-0.3%, Mn: 2.0%-2.5%, Si: 0.20%-0.70%, P: 0.003%-0.006%, S: 0.002%-0.005%, Cr: 2.1%-2.5%, Mo≤0.15%, N: 0.08%-0.30%, V: 0.050%-0.100%, W: 0.020%-0.060%, B: 0.010%-0.020%, and the rest are Fe and other inevitable impurities.

9. The method for preparing a high crack resistance solid welding wire according to claim 4, characterized in that: In the step (3), the smelting temperature is 825-850° C., the time is 10-20 min, the forging temperature is 650-750° C., the hot rolling temperature is 400-450° C., the extrusion speed is 0.5-2 m / min, the drawing passes are 10-25 passes, and after each drawing pass, the temperature is 300-350° C. and annealing is performed for 10-20 min, so that the diameter of the obtained solid welding wire is 1.0-1.5 mm.

10. The method for preparing a high crack resistance solid welding wire according to claim 4, characterized in that: In the step (3), the electron beam irradiation is carried out at an irradiation voltage of 3 MeV, a dose rate of 20 kGy / pass, and an absorbed radiation dose of 100 to 125 kgy.

Citation Information

Patent Citations

  • Welded metal and titanium dioxide flux-cored wire

    CN101352790A

  • Welding wire for welding casing and preparation method and application thereof

    CN112059472A

  • Nickel-based alloy welding wire and preparation method thereof

    CN116475623A

  • Coated arc-welding bar

    WO2014021097A1