Method for repairing defects of carbon steel and austenitic stainless steel composite plate

Through detailed inspection and repair procedures, the defects of carbon steel austenitic stainless steel composite boards are repaired, which solves the risks and costs problems caused by defects in composite board production, and achieves the satisfaction of high mechanical properties and corrosion resistance. Save steel mill costs.

CN118951589APending Publication Date: 2024-11-15NANJING IRON & STEEL CO LTD

Patent Information

Application Number
CN202411038713.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Defects inevitably arise in the production process of existing carbon steel austenitic stainless steel composite panels, resulting in increased user engineering risks and steel plant costs, and the existing repair methods cannot meet the requirements of high mechanical properties and corrosion resistance.

Method used

Using methods including pre-repair inspection, repair process and post-repair inspection, defects are evaluated in detail through coating thickness detection, ultrasonic detection, coloring detection and other means, and targeted repairs are carried out in combination with welding materials and processes suitable for stainless steel, including welding and Grinding ensures high mechanical properties and corrosion resistance of the composite panel after repair.

Benefits of technology

Effectively repair composite panel defects, meet the requirements of high mechanical performance and corrosion resistance for user engineering applications, significantly save steel plant costs, and improve welding quality through tungsten argon arc welding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004971809100000011
    Figure HDA0004971809100000011
  • Figure HDA0004971809100000012
    Figure HDA0004971809100000012
  • Figure HDA0004971809100000013
    Figure HDA0004971809100000013
Patent Text Reader

Abstract

The invention discloses a method for repairing defects of a carbon steel and austenitic stainless steel composite plate. The method comprises the steps of inspection before repairing, the repairing process and inspection after repairing. The inspection before repair comprises coating thickness detection, ultrasonic detection and coloring detection, after detection is completed, nondestructive detection results are summarized, a defect schematic diagram is drawn, defect positions and defect size parameters are marked, and traceability is provided for later polishing, repair welding and reinspection; the repairing process comprises a repairing method for coating surface defects, ultrasonic flaw detection layering defects, edge periphery coloring detection defects, ultrasonic flaw detection base material defects, stainless steel coating thickness standard exceeding defects, edge material shortage defects and plate deformation after repair welding, and corresponding welding materials are adopted for a base layer and a coating; the inspection after repairing comprises ultrasonic wave, coloring nondestructive testing and coating thickness measurement after repairing. The repaired composite board meets the requirements of high mechanical performance, corrosion resistance and the like of user engineering application, and the cost of a steel mill can be greatly saved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of composite plate defect repair, and in particular to a method for repairing defects of a carbon steel austenite stainless steel composite plate. Background Art

[0002] With the development of modern industry, many industries have higher and higher requirements for steel plate materials. For example, various organic solvent storage tanks, PTA silos, and liquefied gas storage tanks require not only good mechanical properties of steel plates, but also corrosion resistance. In this context, carbon steel austenitic stainless steel composite plates came into being. This material not only maintains the mechanical properties of the base carbon steel (excellent tensile strength, impact resistance, etc.), but also has the corrosion resistance of the cladding stainless steel, and is favored by various users.

[0003] There are two production methods for carbon steel austenitic stainless steel composite plates on the market: explosive composite and rolling composite. Explosive composite uses explosives or other strong impact means to combine the base layer and the cladding layer together; rolling composite welds the base layer and the cladding slab together in advance, and then directly produces the finished composite plate by rolling. However, no matter which method is used to make composite plates, various defects will inevitably occur. Defects pose a huge risk to user engineering use and are also a huge loss to steel mills.

[0004] Therefore, it is necessary to develop a targeted method for repairing defects in carbon steel austenitic stainless steel composite plates so that the repaired composite plates can meet the requirements of high mechanical properties and corrosion resistance for user engineering applications. Summary of the invention

[0005] Purpose of the invention: In view of the shortcomings and defects of the prior art, the present invention provides a method for repairing defects of a carbon steel austenitic stainless steel composite plate, which includes three parts: inspection before repair, repair process, and inspection after repair. The three parts are used in combination to ensure that the defects of the composite plate are repaired as much as possible, so that the repaired composite plate meets the requirements of high mechanical properties and corrosion resistance of user engineering applications, which can greatly save the cost of the steel plant.

[0006] Technical solution: A method for repairing defects of a carbon steel austenitic stainless steel composite plate of the present invention is characterized in that it comprises three parts: pre-repair inspection, repair process, and post-repair inspection; the pre-repair inspection includes coating thickness detection, ultrasonic detection, and coloring detection. After the detection is completed, the non-destructive testing results are summarized, and a defect schematic diagram is drawn to indicate the defect position, defect size and other parameters to provide traceability for subsequent grinding, repair welding and re-inspection; the repair process includes repair methods for coating surface defects, ultrasonic flaw detection delamination defects, coloring detection defects around the edges, ultrasonic flaw detection base material defects, stainless steel coating thickness exceeding the standard defect, edge material shortage defect, and plate deformation after repair welding, and corresponding welding materials are used for the base layer and the coating; the post-repair inspection includes ultrasonic, coloring non-destructive testing, and coating thickness measurement after repair.

[0007] Among them, the coating thickness test before repair is as follows: 100% corrosion is carried out on the four sides of the workpiece using 3% nitric acid alcohol, and the side surface is polished with a polishing sheet of 80 mesh or above before testing to remove rust, oxide scale, welding spatter, iron filings, and burrs; the coating thickness is measured with a steel ruler, and the parts exceeding 4mm are photographed and marked.

[0008] Among them, the ultrasonic detection of the inspection before repair: after the coating thickness detection, a dual crystal straight probe with a frequency of 2MHz-5MHz and a focal length close to the coating thickness is used to perform ultrasonic detection and flaw detection on the edge of the base material within 300mm, and the detection is performed from the stainless steel side of the coating; the probe is placed at the fully bonded position of the composite plate, and the height of the first bottom echo is adjusted to 80% of the full scale of the display screen as the reference sensitivity; in order to scan for defects in the substrate, a dual crystal straight probe or a single crystal straight probe with a focal length of half the thickness of the plate is used for ultrasonic detection; the scanning sensitivity is increased by 6dB on the basis of the reference sensitivity; when the height of the first bottom echo is lower than 5% of the full scale of the display screen, and there is obviously an unbonded defect echo, that is, when the echo height is >5%, the part is determined to be an unbonded defect area; after the detection, the defect position and defect size are photographed and marked.

[0009] Among them, the color detection of the inspection before repair: after the coating thickness detection and ultrasonic detection, 100% color detection is performed around the edge of the workpiece; before the detection, the side is polished twice with a polishing sheet of 80 mesh or above to remove rust, oxide scale, welding spatter, iron filings, and burrs; after completing the pretreatment, the penetrant is sprayed on the surface to be inspected with a spray can, and it is continued for 10min-20min at room temperature. After the penetrant on the surface of the workpiece is removed with a cleaning agent, it is naturally dried at room temperature for 5min-10min. After the surface of the workpiece is dry, the developer is directly sprayed on the surface to be inspected, and then wait for natural drying to observe whether there are surface defects; after the detection is completed, the defect position and size are photographed and marked.

[0010] Among them, the coating surface defect repairing method in the repair process is: use a grinding wheel and an internal grinder suitable for stainless steel to grind until the defects are eliminated. If the height of the coating surface is reduced after grinding, use ER308L welding wire to perform surface surfacing welding, and then grind and smooth it after surfacing welding.

[0011] The ultrasonic flaw detection delamination defect repair method in the repair process comprises the following steps:

[0012] 1) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm;

[0013] 2) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0014] 3) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0015] The method for repairing defects by coloring the edges of the repair process comprises the following steps:

[0016] 1) If point defects appear in the base material, use ER50-6 to repair the polished area;

[0017] 2) If point defects appear in the cladding area, use ER308L to repair the polished area;

[0018] 3) If the point defect appears within the depth range of 2mm from the substrate to the bonding surface, it is necessary to use a grinder to grind from the coating surface to the defect depth, ensure that the surface to be repaired is level after grinding, and then use ER50-6, ER309MoL, and ER308L in sequence for repair welding.

[0019] The method for repairing defects of a substrate by ultrasonic flaw detection in the repair process comprises the following steps:

[0020] 1) First, use ER50-6 welding wire to repair the base material so that the carbon steel layer is higher than the joint; then grind the carbon steel layer so that its height is the same as the joint or 0.5mm-1mm higher than the joint;

[0021] 2) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm;

[0022] 3) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0023] 4) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0024] Among them, the edge material shortage repair method in the repair process is:

[0025] 1) Use an angle grinder to grind the periphery of the missing part until the edge is smooth and clean;

[0026] 2) Use ER50-6 welding wire to perform repair welding on the Q345R base layer in a horizontal welding manner, fill the missing part in width or length, and the height of the repaired base material is higher than the joint; then grind the carbon steel layer to make its height the same as the joint or 0.5mm-1mm higher than the joint; before welding, stick a ceramic village pad under the repaired part to prevent the molten pool from collapsing during the repair welding of the bottom layer;

[0027] 3) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, with a repair welding thickness of 2mm;

[0028] 4) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0029] 5) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0030] The post-repair inspection includes ultrasonic non-destructive testing, coloring non-destructive testing, and post-repair coating thickness measurement, which specifically includes the following steps:

[0031] 1) Restore the original morphology of the steel plate surface and side, and there is no welding spatter, welding slag, water or oil on the surface;

[0032] 2) The surface, side and surrounding 200mm of the repaired steel plate are color tested and there are no surface defects;

[0033] 3) Ultrasonic detection of internal defects at the repaired steel plate and within 200mm around it meets the requirements of GB / T8165-2008R1 level, with a bonding rate of 100%, a single unbonded area of ​​0, and a single unbonded length of 0;

[0034] 4) The thickness of the side covering repair of the steel plate is >3mm and <4mm, and there is no mixed layer phenomenon;

[0035] 5) After the repair welding inspection is completed, the original on-site record data will be compiled into a complete non-destructive testing report.

[0036] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the present invention covers a full range of defect types, has a clear repair method, and is highly operable. It includes three parts: pre-repair inspection, repair process, and post-repair inspection. The three parts are used in conjunction to ensure that the defects of the composite plate are repaired as much as possible, so that the repaired composite plate meets the high mechanical properties and corrosion resistance requirements of the user's engineering applications, which can greatly save the cost of the steel plant. The repair of the present invention adopts tungsten inert gas welding (TIG) to improve the welding quality, and adopts small heat input, multi-layer and multi-pass welding. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 It is a schematic diagram of point defects at the base layer of the composite plate of the present invention;

[0038] Figure 2 This is a schematic diagram of the qualified morphology of the composite plate after the point defect is repaired and reworked according to the present invention;

[0039] Figure 3 A schematic diagram of the composite plate delamination defect by ultrasonic flaw detection according to the present invention;

[0040] Figure 4 It is a schematic diagram of the qualified morphology of the composite plate after ultrasonic flaw detection and repair of the delamination defect of the composite plate of the present invention. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and specific implementation methods.

[0042] The method for repairing defects of a carbon steel austenite stainless steel composite plate of the present invention can ensure that the composite plate after repair can still meet the requirements of high mechanical properties and corrosion resistance of user engineering applications.

[0043] 1. Inspection before repair:

[0044] ① Coating thickness detection:

[0045] Use 3% nitric acid alcohol to 100% corrode the periphery of the workpiece. Before testing, the side must be polished with a polishing sheet of 80 mesh or above (applicable to stainless steel materials). There must be no rust, oxide scale, welding spatter, iron filings, burrs and various protective layers. Use a steel ruler to measure the coating thickness, and take photos and mark the parts exceeding 4mm.

[0046] ②Ultrasonic testing:

[0047] After the coating thickness is detected, a dual crystal straight probe with a frequency of 2-5MHz and a focal length close to the coating thickness is used to perform ultrasonic testing within 300mm of the edge of the base material, and the test is performed from the stainless steel side of the coating. The probe is placed at the fully bonded part of the composite plate, and the height of the first bottom echo is adjusted to 80% of the full scale of the display screen as the reference sensitivity. In order to scan the defects in the substrate, a dual crystal straight probe or a single crystal straight probe with a focal length of half the thickness of the plate is also required for ultrasonic testing. The scanning sensitivity is increased by 6dB on the basis of the reference sensitivity. The detection sensitivity can be appropriately increased within 200mm of the edge of the plate. When the height of the first bottom echo is lower than 5% of the full scale of the display screen, and there is obviously an unbonded defect echo (echo height>5%), the part is determined to be an unbonded defect area. After the test, the defect position and defect size are photographed and marked.

[0048] ③Coloring detection:

[0049] After the coating thickness test and ultrasonic test, 100% color test is performed around the edge of the workpiece. Before the test, the side must be polished twice with a polishing sheet of 80 mesh or above (applicable to stainless steel materials), and there must be no rust, oxide scale, iron filings, burrs and various protective layers. After completing the pretreatment, spray the penetrant on the surface to be tested with a spray can for 10-20 minutes at room temperature. After removing the penetrant on the surface of the workpiece with a cleaning agent, dry it naturally at room temperature, usually waiting for 5-10 minutes. After the surface of the workpiece is dry, spray the developer directly on the surface to be tested, and then wait for it to dry naturally to observe whether there are surface defects. After the test is completed, take photos and mark the location and size of the defects.

[0050] After the inspection is completed, the non-destructive testing results are summarized, and a defect diagram is drawn to indicate the defect location, defect size and other parameters to provide traceability for subsequent grinding, repair welding and re-inspection.

[0051] 2. Repair process and related technology:

[0052] According to the summary of inspection results before repair, defects that are likely to occur in composite panels are mainly divided into seven categories, including coating surface defects, ultrasonic flaw detection delamination defects, edge coloring detection defects, ultrasonic flaw detection substrate defects, stainless steel coating thickness exceeding the standard, edge material shortage, and plate deformation after repair welding.

[0053] For edge defects, if the repair welding length exceeds 500mm, a restraint angle steel shall be applied to the back of the repair welding to prevent serious deformation during welding. After grinding and removing the restraint angle steel at the end of the repair welding, the restrained surface shall be ground and repaired. For the restrained repair welding part, the surrounding 200mm range shall be supplemented with ultrasonic and / or color testing after welding.

[0054] The type of composite plate repaired in the present invention is taken as an example of Q345R+S30403 container composite plate. Different types of composite plates should be repaired with welding materials corresponding to their respective base layers and coatings. In order to ensure that the composite plate after repair can still meet the high mechanical properties and corrosion resistance requirements of user engineering applications, tungsten inert gas arc welding (TIG) is used to repair the base material, transition layer, and coating to improve the welding quality, and low heat input, multi-layer and multi-pass welding should be used. The types of welding wires and shielding gases used are shown in the following table:

[0055] Repair area Welding material grade Welding material diameter Protective gas Grassroots ER50-6 1.6mm Argon (99.99%) Transition layer ER309MoL 1.6mm Argon (99.99%) Cladding ER308L 1.6mm Argon (99.99%)

[0056] Welding process can refer to the following table:

[0057] Repair area Current Voltage Welding speed Line Energy Layer and pass temperature Transition layer 100~120A 20~25V 8~10cm / min 10~12kJ / cm ≤80℃ Cladding 100~120A 20~25V 8~10cm / min 10~12kJ / cm ≤80℃ Substrate 100~120A 20~25V 8~10cm / min 10~12kJ / cm ≤80℃

[0058] ① Method for repairing coating surface defects:

[0059] Use grinding wheel and internal grinder suitable for stainless steel to grind until the defects are completely eliminated. If the height of the cladding surface is reduced after grinding, use ER308L welding wire for surface surfacing. Grind and smooth it after surfacing.

[0060] ②Ultrasonic flaw detection layer defect repair method:

[0061] For the delamination defects of the composite plate, use an angle grinder to grind away the entire coating thickness, and ensure that the surface to be repaired is level after grinding to avoid irregular morphology after grinding, which will cause difficulties for repair welding. The thickness of the grinding substrate cannot exceed 0.5mm. After grinding, use 3% nitric acid alcohol to corrode the grinding surface to ensure that the stainless steel coating is completely removed. Color flaw detection is required before repair welding after grinding, and welding can only be performed after passing the test. The repair welding steps are as follows:

[0062] 1) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm.

[0063] 2) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0064] 3) Grind the repaired welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0065] ③ Method for repairing defects detected by coloring around the edges:

[0066] Point defects are eliminated by grinding with an internal grinder;

[0067] The coloring and delamination defects are eliminated with an angle grinder. The thickness of the grinding substrate cannot exceed 0.5mm, and the surface to be repaired after grinding must be level to avoid irregular morphology after grinding, which will cause trouble for repair welding. After grinding, the surface is corroded with 3% nitric acid alcohol to ensure that the stainless steel coating is completely removed.

[0068] After grinding, color flaw detection is required, and only after passing the inspection can welding be carried out.

[0069] The solution for repairing point defects is as follows:

[0070] 1) If point defects appear in the base material, use ER50-6 to repair the polished area;

[0071] 2) If point defects appear in the cladding area, use ER308L to repair the polished area;

[0072] 3) If the point defect appears within the depth range of 2mm from the substrate to the bonding surface, it is necessary to use a grinder to grind from the coating surface to the defect depth, ensure that the surface to be repaired is level after grinding, and then use ER50-6, ER309MoL, and ER308L for repair welding in sequence;

[0073] The steps for repairing the colored delamination defect are as follows:

[0074] 1) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm.

[0075] 2) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0076] 3) Grind the repaired welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0077] ④Ultrasonic flaw detection substrate defect repair method:

[0078] According to the defect location, select the closest surface to grind to the defect location and eliminate the defect. For the slender strip defects at the end, try to make the part to be repaired into a V-shaped or U-shaped groove during the grinding process, and avoid directly grinding into a slender rectangular groove to prevent the occurrence of incomplete penetration defects after repair welding; after grinding, color flaw detection is required, and repair welding can only be performed after passing the test. If the defect is close to the coating surface, the repair welding steps are as follows:

[0079] 1) First, use ER50-6 welding wire to repair the base material so that the carbon steel layer is slightly higher than the joint; then grind the carbon steel layer so that its height is the same as the joint or 0.5-1mm higher than the joint;

[0080] 2) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm.

[0081] 3) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0082] 4) Grind the repaired welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0083] If the defect is close to the surface of the Q345R substrate, the repair welding steps are as follows:

[0084] 1) Use ER50-6 welding wire to repair the base material until the thickness of the repaired base material weld is slightly higher than the base material surface.

[0085] 2) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0086] ⑤ Repair method for stainless steel coating thickness exceeding the standard defect:

[0087] Use an angle grinder to grind layer by layer until all the stainless steel materials in the base material are removed, ensure that the surface to be repaired is level after grinding, and avoid irregular morphology after grinding, which will cause trouble for repair welding. After grinding, use 3% nitric acid alcohol to check again to ensure that all the stainless steel layers are removed. Repair welding can only be carried out after the polished surface passes the color flaw detection. The repair welding steps are as follows:

[0088] 1) First, use ER50-6 welding wire to repair the base material so that the carbon steel layer is slightly higher than the joint; then grind the carbon steel layer so that its height is the same as the joint or 0.5-1mm higher than the joint;

[0089] 2) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm.

[0090] 3) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0091] 4) Grind the repaired welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0092] ⑥Methods for repairing missing materials on the edge:

[0093] 1) Use an angle grinder to grind the periphery of the missing part until the edge is smooth and clean.

[0094] 2) Use ER50-6 welding wire to perform repair welding on the Q345R base layer in a horizontal welding manner, fill the missing part in width or length, and the height of the repaired base material is slightly higher than the joint; then grind the carbon steel layer to make its height the same as the joint or 0.5-1mm higher than the joint; before welding, a ceramic village pad should be attached under the repaired part to prevent the molten pool from collapsing during the repair welding of the bottom layer;

[0095] 3) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, with a repair welding thickness of 2mm;

[0096] 4) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding;

[0097] 5) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

[0098] ⑦Methods for repairing plate deformation after repair welding:

[0099] For shrinkage angle deformation greater than 3mm after repair welding, if the length does not exceed 500mm and the plate thickness is less than or equal to 20mm, oxyacetylene heating combined with a hammer is used for on-site correction. If the shrinkage angle deformation exceeds 500mm or the plate thickness is greater than 20mm, local or global heating correction is adopted in the furnace, and 520-degree tempering stress relief treatment is performed before straightening. After the correction is completed, ultrasonic testing is required for the corrected part and the range of 200mm around the corrected part to prevent new defects caused by the correction. If global heating straightening is adopted, ultrasonic testing is required at the edge 500mm after straightening.

[0100] 3. Inspection after repair:

[0101] In order to ensure that the repaired composite board can meet the factory requirements, relevant inspections are required to ensure the quality of the repair.

[0102] Ultrasonic and color non-destructive testing after repair, as well as the thickness measurement of the coating after repair, must meet the following requirements:

[0103] 1) Restore the original appearance of the steel plate surface and side, and there must be no welding spatter, welding slag, water, oil, etc.;

[0104] 2) The surface, side and surrounding 200mm of the repaired steel plate are color tested and there are no surface defects;

[0105] 3) Ultrasonic detection of internal defects in the repaired steel plate and the surrounding 200mm range must meet the requirements of GB / T8165-2008 R1 level. The bonding rate is 100%, the single unbonded area is 0, and the single unbonded length is 0 (including 900mm 2 The following non-fitting area);

[0106] 4) The repair thickness of the side covering of the steel plate should be >3mm and <4mm, and there should be no mixed layer phenomenon.

[0107] 5) After the repair welding inspection is completed, the original on-site record data will be compiled into a complete non-destructive testing report.

[0108] 4. Effect analysis:

[0109] like Figure 1 , 2 As shown in the figure, after the coating thickness inspection, ultrasonic inspection and coloring inspection before repair, the edge of the container composite plate Q345R+S30403 has point defects. Appears in the substrate. According to the repair method ③ of the present invention, the defect repair method of coloring around the edge is firstly polished with an internal grinder to eliminate the point defects, and then ER50-6 is repaired at the polished position. After the repair is completed, the repair position is re-inspected according to the post-repair inspection method of the present invention to ensure that the rework is qualified.

[0110] like Figure 3 , 4 As shown in the figure, after the coating thickness inspection, ultrasonic inspection and color inspection of the container composite plate Q345R+S30403 before repair, the ultrasonic inspection found 700mm near the edge. 2 Delamination defect. According to the repair method ② of the present invention, the ultrasonic flaw detection delamination defect repair method, first use an angle grinder to grind and remove the entire coating thickness, and ensure that the surface to be repaired is level after grinding to avoid irregular morphology after grinding. After grinding, use 3% nitric acid alcohol to corrode the polished surface to ensure that the stainless steel coating is completely removed. Color flaw detection is required before repair welding after grinding, and welding can only be performed after passing the inspection. After that, ER309MoL welding wire is used to perform transition layer repair welding on the Q345R base surface, and the repaired area is evenly filled with a repair thickness of 2mm; then ER308L welding wire is used for coating cover welding until the height of the repaired coating weld is higher than the coating. After the repair welding is completed, grind the repair welding area to make its surface smooth and flat, and keep it consistent with the original appearance of the plate. Finally, the repair position is re-inspected according to the post-repair inspection method of the present invention to ensure that the rework is qualified.

Claims

1. A method for repairing defects of carbon steel austenitic stainless steel composite plate, Features: It includes three parts: pre-repair inspection, repair process, and post-repair inspection; The pre-repair inspection includes coating thickness detection, ultrasonic detection, and color detection. After the inspection is completed, the non-destructive testing results are summarized, and a defect diagram is drawn to indicate the defect location and defect size parameters, so as to provide traceability for subsequent grinding, repair welding and re-inspection; The repair process includes repair methods for coating surface defects, ultrasonic flaw detection delamination defects, color detection defects around the edges, ultrasonic flaw detection base material defects, stainless steel coating thickness exceeding the standard defect, edge material shortage defect, and plate deformation after repair welding, and corresponding welding materials are used for the base layer and coating; the post-repair inspection includes ultrasonic, color non-destructive testing, and measurement of coating thickness after repair.

2. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The coating thickness test before repair is as follows: 100% corrosion is performed on the periphery of the workpiece using 3% nitric acid alcohol, and the side surface is polished with a polishing sheet of 80 mesh or above before testing to remove rust, oxide scale, welding spatter, iron filings, and burrs; the coating thickness is measured with a steel ruler, and the parts exceeding 4mm are photographed and marked.

3. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The ultrasonic test for inspection before repair: after the coating thickness is detected, a dual crystal straight probe with a frequency of 2MHz-5MHz and a focal length close to the coating thickness is used to perform ultrasonic testing on the edge of the base material within 300mm, and the test is performed from the stainless steel side of the coating; the probe is placed at the fully bonded part of the composite plate, and the height of the first bottom echo is adjusted to 80% of the full scale of the display screen as the reference sensitivity; in order to scan for defects in the substrate, a dual crystal straight probe or a single crystal straight probe with a focal length of half the thickness of the plate is used for ultrasonic testing; the scanning sensitivity is increased by 6dB on the basis of the reference sensitivity; when the height of the first bottom echo is lower than 5% of the full scale of the display screen, and there is obviously an unbonded defect echo, that is, when the echo height is >5%, the part is determined to be an unbonded defect area; after the test, the defect position and defect size are photographed and marked.

4. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The color detection of the inspection before repair is as follows: after the coating thickness detection and ultrasonic detection are completed, 100% color detection is performed around the edge of the workpiece; before the detection, the side is polished twice with a polishing sheet of 80 mesh or above to remove rust, oxide scale, welding spatter, iron filings, and burrs; after completing the pretreatment, the penetrant is sprayed on the surface to be inspected with a spray can, and the spray is continued for 10min-20min at room temperature, and the penetrant on the surface of the workpiece is removed with a cleaning agent and then naturally dried at room temperature for 5min-10min. After the surface of the workpiece is dry, the developer is directly sprayed on the surface to be inspected, and then wait for natural drying to observe whether there are surface defects; after the detection is completed, the defect position and size are photographed and marked.

5. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The method for repairing the surface defects of the coating in the repair process is as follows: grinding with a grinding wheel suitable for stainless steel and an internal grinder until the defects are eliminated. If the height of the coating surface is reduced after grinding, ER308L welding wire is used for surface surfacing, and then the surface is ground and leveled after surfacing.

6. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The ultrasonic flaw detection delamination defect repair method in the repair process comprises the following steps: 1) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm; 2) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding; 3) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

7. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The method for repairing defects by coloring the edges of the repair process comprises the following steps: 1) If point defects appear in the base material, use ER50-6 to repair the polished area; 2) If point defects appear in the cladding area, use ER308L to repair the polished area; 3) If the point defect appears within the depth range of 2mm from the substrate to the bonding surface, it is necessary to use a grinder to grind from the coating surface to the defect depth, ensure that the surface to be repaired is level after grinding, and then use ER50-6, ER309MoL, and ER308L in sequence for repair welding.

8. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The ultrasonic flaw detection substrate defect repair method in the repair process comprises the following steps: 1) First, use ER50-6 welding wire to repair the base material so that the carbon steel layer is higher than the joint; then grind the carbon steel layer so that its height is the same as the joint or 0.5mm-1mm higher than the joint; 2) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, fill the grinding area evenly, and the repair welding thickness is 2mm; 3) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding; 4) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

9. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The edge missing material repair method in the repair process described is as follows: 1) Use an angle grinder to grind the periphery of the missing part until the edge is smooth and clean; 2) Use ER50-6 welding wire to perform repair welding on the Q345R base layer in a horizontal welding manner, fill the missing part in width or length, and the height of the repaired base material is higher than the joint; then grind the carbon steel layer to make its height the same as the joint or 0.5mm-1mm higher than the joint; before welding, stick a ceramic village pad under the repaired part to prevent the molten pool from collapsing during the repair welding of the bottom layer; 3) Use ER309MoL welding wire to perform transition layer repair welding on the Q345R base surface, with a repair welding thickness of 2mm; 4) Use ER308L welding wire to weld the cladding cover until the height of the repair cladding weld is higher than the cladding; 5) Grind the repair welding area to make its surface smooth and flat, consistent with the original appearance of the plate.

10. The method for repairing defects of a carbon steel austenitic stainless steel composite plate according to claim 1, Features: The post-repair inspection includes ultrasonic, color non-destructive testing, and post-repair coating thickness measurement, and specifically includes the following steps: 1) Restore the original morphology of the steel plate surface and side, and there is no welding spatter, welding slag, water or oil on the surface; 2) The surface, side and surrounding 200mm of the repaired steel plate are color tested and there are no surface defects; 3) Ultrasonic detection of internal defects at the repaired steel plate and within 200mm around it meets the requirements of GB / T8165-2008R1 level, with a bonding rate of 100%, a single unbonded area of ​​0, and a single unbonded length of 0; 4) The thickness of the side covering repair of the steel plate is >3mm and <4mm, and there is no mixed layer phenomenon; 5) After the repair welding inspection is completed, the original on-site record data will be compiled into a complete non-destructive testing report.

Citation Information

Patent Citations

  • Defect repair welding process of stainless steel composite board coating

    CN101774063A

  • Efficient path planning method for visual detection of surface defects

    CN101819161A

  • Argon arc welding repair method for defects of stainless steel composite plate

    CN114346586A

  • Plywood defect repairing method

    CN115781834A

  • Surface defect grinder of steel plate and method

    JP2016078150A

Cited By

  • POC gas holder side plate deformation repairing method

    CN119973443A