Preparation method of high-performance bamboo fiber bundle reinforced composite material based on normal-pressure plasma pretreatment

Through the methods of atmospheric plasma pretreatment and hot pressing, the defects of high-temperature and high-pressure treatment of bamboo fiber bundle reinforced composite materials are solved, which improves the adhesiveness and mechanical properties of bamboo fiber bundles, reduces production costs, and improves the Bamboo utilization and environmental protection.

CN118952404APending Publication Date: 2024-11-15FUJIAN AGRI & FORESTRY UNIV

Patent Information

Application Number
CN202411246337.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing bamboo fiber bundle reinforced composite technology, high temperature, high pressure or chemical treatment leads to excessive damage to bamboo, production of harmful chemicals, increased moisture content and high processing costs, and conventional treatment reduces bamboo utilization.

Method used

By using the method based on the normal pressure plasma pretreatment, bamboo materials with bamboo green and bamboo yellow are cut into bamboo fiber bundles, and surface treatment is performed in the normal pressure plasma device, then the adhesive is soaked and dried, and finally Hot press molding to prepare high-performance bamboo fiber bundle reinforced composite materials.

Benefits of technology

It improves the adhesiveness and interface bonding of bamboo fiber bundles, reduces production costs, avoids the negative impact of high temperature and high pressure or chemical treatment, and significantly improves the mechanical properties and durability of bamboo fiber bundle reinforced composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005030871920000011
    Figure HDA0005030871920000011
  • Figure HDA0005030871920000021
    Figure HDA0005030871920000021
  • Figure HDA0005030871920000022
    Figure HDA0005030871920000022
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-performance bamboo fiber bundle reinforced composite material based on normal-pressure plasma pretreatment. The preparation method comprises the following steps: S01, cutting bamboo wood with bamboo green and tabasheer into bamboo fiber bundles; s02, the bamboo fiber bundles are placed in a normal-pressure plasma device to be subjected to surface treatment; s03, the bamboo fiber bundles treated through the normal-pressure plasma device are soaked in an adhesive, and the bamboo fiber bundles are soaked at the preset environment temperature for the preset duration; s04, carrying out drying treatment on the bamboo fiber bundles subjected to gum dipping; and S05, after the dried bamboo fiber bundles are arranged in order, the bamboo fiber bundles are placed in a mold to be subjected to hot press molding treatment, and the high-performance bamboo fiber bundle reinforced composite material is prepared. According to the scheme, the bamboo fiber bundles with bamboo green and tabasheer are treated by using the normal-pressure plasma, so that the surface activity of the bamboo fiber bundles is enhanced, and the infiltration effect of the adhesive can be improved; and the bamboo fiber bundles subjected to plasma treatment only need to be subjected to simple gum dipping treatment and then are subjected to hot pressing, so that the high-performance bamboo fiber bundle reinforced composite material can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bamboo material processing, and in particular to a method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment. Background Art

[0002] Bamboo fiber bundle reinforced composite material is a high-performance building material made by decomposing and reorganizing raw bamboo, which has the advantages of high strength and good wear resistance. However, in the existing bamboo fiber bundle reinforced composite material technology, the pre-treatment process of bamboo fiber bundles usually adopts high temperature, high pressure or chemical treatment, which is easy to cause excessive damage to bamboo or produce harmful chemicals, affecting the performance and environmental protection of the final product; in addition, high temperature, high pressure or chemical treatment also causes the increase of moisture content of bamboo fiber bundles, increasing the number of drying times and drying costs of bamboo fiber bundles; at the same time, conventional bamboo fiber bundle processing in the existing technology mostly adopts the method of stripping bamboo green and yellow, which not only increases processing costs, but also reduces the utilization rate of bamboo; therefore, how to further improve its production continuity and reduce processing costs while ensuring the processing quality of bamboo is a very positive and realistic research topic. Summary of the invention

[0003] In view of this, the object of the present invention is to propose a method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment, which has reliable implementation, good production continuity, flexible application and good comprehensive performance of the obtained finished product.

[0004] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:

[0005] A method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment, comprising:

[0006] S01, cutting bamboo materials with bamboo green and bamboo yellow into bamboo fiber bundles;

[0007] S02, placing the bamboo fiber bundle in a normal pressure plasma device for surface treatment, wherein the nozzle distance is 1.5-3 cm, the plasma power is 600-900 W, and the treatment rate is 30-60 mm / s;

[0008] S03, soaking the bamboo fiber bundle treated by the normal pressure plasma device in an adhesive, and soaking it at a preset ambient temperature for a preset time;

[0009] S04, drying the bamboo fiber bundle after the dip, so that the moisture content is lower than 12% and the adhesive in the bamboo fiber bundle is not cured or not completely cured;

[0010] S05. Arrange the dried bamboo fiber bundles neatly and place them in a mold for hot pressing to obtain a high-performance bamboo fiber bundle reinforced composite material.

[0011] As a possible implementation manner, further, in the present solution S01, the bamboo material is carbonized or uncarbonized bamboo material.

[0012] As a possible implementation manner, further, in the present solution S02, the surface of the bamboo fiber bundle is cleaned before being placed in the atmospheric pressure plasma device for surface treatment.

[0013] As a possible implementation mode, further, in the present scheme S02, the parameters of the atmospheric pressure plasma device for surface treatment of the bamboo fiber bundle are: nozzle distance is 1.5-3cm, plasma power is 600-900W, and treatment rate is 30-60mm / s.

[0014] As a possible implementation mode, further, in the present solution S03, the adhesive is phenolic resin or polyurethane; and the bamboo fiber bundle is immersed in the adhesive at room temperature for 10-15 minutes.

[0015] As a possible implementation mode, further, in the present scheme S04, the bamboo fiber bundles after being impregnated with glue are drained and then placed in an oven for drying at a drying temperature of 50°C so that the moisture content is lower than 12% and the adhesive in the bamboo fiber bundles is not cured or not completely cured.

[0016] As a possible implementation mode, further, in the present scheme S05, the neatly arranged bamboo fiber bundles are placed in a mold for hot pressing molding, the hot pressing temperature is 120-160°C, the pressure is 5-10Mpa, and the hot pressing time is 30-60min, so as to obtain a high-performance bamboo fiber bundle reinforced composite material.

[0017] As a possible implementation, further, in the present solution S05, the bamboo fiber bundle after drying is heated to 1.0-1.2 g / cm 3 The predetermined bamboo fiber bundle composite material density, length and width specifications of 2440mm×1220mm, and thickness of 10mm~50mm are planned to control the mass of the added bamboo bundles. After being arranged neatly in a mold, they are placed in a hot press for hot pressing. The hot pressing conditions are controlled to be 150℃, the pressure is 8MPa, and the hot pressing time is 1.5~3 minutes / mm thickness; after the hot pressing is completed, it is cooled to no more than 30℃ above room temperature and then the pressure is released to obtain a bamboo fiber bundle composite material sheet.

[0018] Based on the above, the present invention also provides a high-performance bamboo fiber bundle reinforced composite material, which is prepared by the preparation method described above.

[0019] By adopting the above technical scheme, the present invention has the following beneficial effects compared with the prior art: the present invention uses atmospheric pressure plasma to treat bamboo fiber bundles with bamboo green and bamboo yellow, so that their surface activity is enhanced, which can improve the wetting effect of the adhesive; and the bamboo fiber bundles treated with plasma only need to be simply dipped in glue, and then hot-pressed to prepare high-performance bamboo fiber bundle reinforced composite materials. In summary, the present scheme has the following advantages:

[0020] (1) The process is environmentally friendly and simple: This solution uses atmospheric pressure plasma to treat the surface of bamboo fiber bundles while retaining the green and yellow colors of bamboo, so that they have better adhesiveness and interfacial bonding force, thereby improving the overall performance of bamboo fiber bundle reinforced composite materials; and the use of atmospheric pressure plasma treatment technology to treat bamboo fiber bundles avoids the negative impact of high temperature, high pressure or chemical treatment on the environment and materials;

[0021] (2) Cost-effectiveness: This solution does not require the removal of green and yellow bamboo from bamboo. While simplifying the process, it avoids the additional drying times in conventional bamboo fiber bundle pretreatment, reduces drying energy consumption, effectively reduces production costs, and improves bamboo utilization;

[0022] (3) Good performance of finished products: This solution enhances the activity of the bamboo fiber bundle surface through atmospheric plasma treatment, improves the wetting effect of the adhesive, and significantly improves the mechanical properties and durability of the bamboo fiber bundle reinforced composite material. Compared with vacuum plasma, the static bending strength of the best bamboo fiber bundle composite material pressed from the carbonized bamboo bundle treated with vacuum plasma is 172MPa, while the static bending strength of the bamboo fiber bundle composite material pressed from the carbonized bamboo bundle treated with atmospheric plasma can reach more than 175MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 The SEM comparison pictures of bamboo surface (bamboo green and bamboo yellow) before and after treatment;

[0025] Figure 2 Schematic diagram of XPS on bamboo surface before and after treatment;

[0026] Figure 3 Schematic diagram of static bending strength and elastic modulus of bamboo fiber bundle composites made from carbonized bamboo bundles at different processing powers;

[0027] Figure 4 Schematic diagram of the static bending strength and elastic modulus of bamboo fiber bundle composites made from uncarbonized bamboo bundles at different processing powers;

[0028] Figure 5 Schematic diagram of static bending strength and elastic modulus of bamboo fiber bundle composites prepared by carbonizing bamboo bundles at different processing rates;

[0029] Figure 6 Schematic diagram of the static bending strength and elastic modulus of bamboo fiber bundle composites prepared at different processing rates of uncarbonized bamboo bundles;

[0030] Figure 7 Schematic diagram of static bending strength and elastic modulus of bamboo fiber bundle composites made from carbonized bamboo bundles at different nozzle distances;

[0031] Figure 8 Schematic diagram of the static bending strength and elastic modulus of bamboo fiber bundle composites made from uncarbonized bamboo bundles at different nozzle distances;

[0032] Fig. 9 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composite material prepared by carbonized bamboo bundle under different processing powers;

[0033] Fig.10 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composite material made of uncarbonized bamboo bundle under different processing powers;

[0034] Fig.11 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composites prepared by carbonizing bamboo bundles at different treatment rates;

[0035] Fig.12 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composites prepared at different treatment rates of uncarbonized bamboo bundles;

[0036] Fig.13 The schematic diagram of the water absorption thickness expansion rate of the bamboo fiber bundle composite material prepared by carbonizing the bamboo bundle at different nozzle distances;

[0037] Fig.14 Schematic diagram of the water absorption thickness expansion rate of bamboo fiber bundle composite materials made from uncarbonized bamboo bundles at different nozzle distances. DETAILED DESCRIPTION

[0038] The present invention will be further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Similarly, the following examples are only partial embodiments of the present invention rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0039] Example

[0040] The present embodiment provides a method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment, which comprises:

[0041] 1) Preparation of bamboo bundles

[0042] Cutting and rolling some bamboo materials with green and yellow bamboo to form bamboo fiber bundles (referred to as bamboo bundles) to obtain uncarbonized bamboo fiber bundles;

[0043] Carbonizing some bamboo materials with green bamboo and yellow bamboo and then rolling and loosening them into bamboo fiber bundles to obtain carbonized bamboo fiber bundles;

[0044] The carbonized bamboo fiber bundles and the uncarbonized bamboo fiber bundles are divided into two different groups. The two groups of green and yellow bamboo bundles are put into an oven and dried to a moisture content of about 8% to obtain a better processing effect and to be prepared for subsequent processing.

[0045] 2) Surface plasma treatment of bamboo bundles

[0046] Two groups of bamboo fiber bundles were placed in a normal pressure plasma device for surface treatment, with a nozzle distance of 1.5-3 cm, a plasma power of 600-900 W, and a treatment rate of 30-60 mm / s.

[0047] 3) Bamboo bundles are dipped in glue

[0048] The two groups of bamboo fiber bundles treated with normal pressure plasma were immersed in a phenolic resin adhesive with a solid content of about 20% for 12.5 minutes to allow the adhesive to penetrate into the cell walls of the bamboo fiber bundles.

[0049] After the dipping is completed, the two groups of bamboo bundles are taken out and the glue liquid is drained, and then placed in an oven at 50° C. for drying, and the moisture content of the bamboo bundles after the dipping is controlled to be below 12%.

[0050] 4) Compression of bamboo fiber bundle composite materials

[0051] The two groups of dried bamboo bundles with glue were assembled along the grain in a bamboo fiber bundle composite material mold. 3The predetermined bamboo fiber bundle composite material density, length and width specifications of 2440mm×1220mm, and thickness of 25mm are planned to control the mass of the added bamboo bundle, and then placed in a hot press for hot pressing, and the hot pressing conditions are controlled to be 150℃, the pressure is 8MPa, and the hot pressing time is 2.5 minutes / mm thickness; after the hot pressing is completed, it is cooled to not more than 30℃ above room temperature and then the pressure is released to obtain a bamboo fiber bundle composite material sheet; two groups of pressed bamboo fiber bundle composite materials products are obtained, namely, a bamboo fiber bundle composite material product made of uncarbonized bamboo fiber bundles and a bamboo fiber bundle composite material product made of carbonized bamboo fiber bundles.

[0052] In order to facilitate the comparison of microstructures, this study conducted SEM characterization on the green and yellow sides of the uncarbonized bamboo fiber bundles and carbonized bamboo fiber bundles. The results are shown in the figure. Figure 1 As shown, Figure 1 In the figure, a-1) and a-2) are SEM characterization pictures of the green bamboo of the uncarbonized bamboo bundle at different magnifications, b-1) and b-2) are SEM characterization pictures of the green bamboo of the carbonized bamboo bundle at different magnifications, c-1) and c-2) are SEM characterization pictures of the yellow bamboo of the uncarbonized bamboo bundle at different magnifications, d-1) and d-2) are SEM characterization pictures of the yellow bamboo of the carbonized bamboo bundle at different magnifications.

[0053] Furthermore, this scheme also compares the uncarbonized bamboo fiber bundle (before treatment) and the carbonized bamboo fiber bundle (after treatment) through XPS characterization, and the results are as follows: Figure 2 shown.

[0054] In order to facilitate the comparison of the strength performance changes of bamboo fiber bundle composite materials (finished products) brought about by the changes in the parameters of the surface plasma treatment of bamboo bundles (including carbonized bamboo bundles and uncarbonized bamboo bundles), this scheme only adjusts the parameters of the above step "2) surface plasma treatment of bamboo bundles" to compare the elastic modulus and static bending strength of bamboo fiber bundle composite materials obtained by plasma at different nozzle distances (treatment distances), powers and treatment rates under normal pressure. Among them, when only the plasma power is used as a variable factor, the nozzle distance (treatment distance) and the treatment rate are both taken as the median of the range value, and when the nozzle distance or the treatment rate is used as a variable factor, the other two parameters are not taken as the median of the range value; the comparison results are as follows:

[0055] Figure 3 Schematic diagram of static bending strength and elastic modulus of bamboo fiber bundle composites made from carbonized bamboo bundles at different processing powers;

[0056] Figure 4 Schematic diagram of the static bending strength and elastic modulus of bamboo fiber bundle composites made from uncarbonized bamboo bundles at different processing powers;

[0057] Figure 5 Schematic diagram of static bending strength and elastic modulus of bamboo fiber bundle composites prepared by carbonizing bamboo bundles at different processing rates;

[0058] Figure 6 Schematic diagram of the static bending strength and elastic modulus of bamboo fiber bundle composites prepared at different processing rates of uncarbonized bamboo bundles;

[0059] Figure 7 Schematic diagram of static bending strength and elastic modulus of bamboo fiber bundle composites made from carbonized bamboo bundles at different nozzle distances;

[0060] Figure 8 Schematic diagram of the static bending strength and elastic modulus of bamboo fiber bundle composites made from uncarbonized bamboo bundles at different nozzle distances;

[0061] Fig. 9 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composite material prepared by carbonized bamboo bundle under different processing powers;

[0062] Fig.10 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composite material made of uncarbonized bamboo bundle under different processing powers;

[0063] Fig.11 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composites prepared by carbonizing bamboo bundles at different treatment rates;

[0064] Fig.12 Schematic diagram of water absorption thickness expansion rate of bamboo fiber bundle composites prepared at different treatment rates of uncarbonized bamboo bundles;

[0065] Fig.13 The schematic diagram of the water absorption thickness expansion rate of the bamboo fiber bundle composite material prepared by carbonizing the bamboo bundle at different nozzle distances;

[0066] Fig.14 Schematic diagram of the water absorption thickness expansion rate of bamboo fiber bundle composite materials made from uncarbonized bamboo bundles at different nozzle distances.

[0067] The above descriptions are only some embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Any equivalent device or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment, characterized in that: It includes: S01, cutting bamboo materials with bamboo green and bamboo yellow into bamboo fiber bundles; S02, placing the bamboo fiber bundle in a normal pressure plasma device for surface treatment, wherein the nozzle distance is 1.5-3 cm, the plasma power is 600-900 W, and the treatment rate is 30-60 mm / s; S03, soaking the bamboo fiber bundle treated by the atmospheric pressure plasma device in an adhesive, and allowing it to soak at a preset ambient temperature for a preset time; S04, drying the impregnated bamboo fiber bundles to reduce their moisture content to less than 12% and ensuring that the adhesive in the bamboo fiber bundles is not cured or is not completely cured; S05. Arrange the dried bamboo fiber bundles neatly and place them in a mold for hot pressing to produce a high-performance bamboo fiber bundle reinforced composite material.

2. The method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment according to claim 1, characterized in that: In S01, the bamboo material is carbonized or uncarbonized bamboo material.

3. The method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment according to claim 1, characterized in that: In S02, the surface of the bamboo fiber bundle is cleaned before being placed in a normal pressure plasma device for surface treatment; The parameters of the atmospheric pressure plasma device for treating the surface of the bamboo fiber bundle are: nozzle distance of 1.5-3 cm, plasma power of 600-900 W, and treatment rate of 30-60 mm / s.

4. The method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment according to claim 1, characterized in that: In S03, the adhesive is phenolic resin or polyurethane; and the bamboo fiber bundle is immersed in the adhesive at room temperature for 10-15 minutes.

5. The method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment according to claim 1, characterized in that: In S04, the bamboo fiber bundles after being dipped in glue are drained and then placed in an oven for drying at a drying temperature of 50° C. to reduce the moisture content to less than 12% and to ensure that the adhesive in the bamboo fiber bundles is not cured or not completely cured.

6. The method for preparing a high-performance bamboo fiber bundle reinforced composite material based on atmospheric pressure plasma pretreatment according to claim 1, characterized in that: In S05, the neatly arranged bamboo fiber bundles are placed in a mold for hot pressing processing at a temperature of 120-160° C., a pressure of 5-10 MPa, and a hot pressing time of 30-60 min to produce a high-performance bamboo fiber bundle reinforced composite material.

7. A high-performance bamboo fiber bundle reinforced composite material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Method for preparing environment-friendly bamboo recombinant material

    CN102528893A

  • Method for manufacturing reorganized bamboos by adopting plasma technology

    CN103465322A

  • Method utilizing atmospheric-pressure plasma to modify plastic thin film for environment-friendly plywood preparation

    CN106965273A

  • Manufacturing method of bamboo fiber / polylactic acid degradable composite board with large length-diameter ratio

    CN115570820A

  • KR20190074076A

Cited By

  • Bamboo wood processing treatment method and treatment system

    CN119610307A