Method and system for recovering bastnaesite acid leaching waste gas
Through the purification of cerium sulfate and the mixed treatment of alkaline solution, the problem of incomplete chlorine gas treatment in the oxidative roasting-acid leaching method is solved, and the efficient preparation of sodium hypochlorite and the utilization of resources are achieved, cost and energy consumption are reduced, and environmental pollution is solved. question.
Patent Information
- Application Number
- CN202411085310.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
During the oxidative roasting and acid leaching process of rare earth elements, the chlorine-containing waste gas produced is not thoroughly treated, and it is costly and energy consumption is high, so valuable by-products cannot be obtained.
The mixed gas is purified by cerium sulfate, hydrogen chloride is removed and the purity of chlorine is increased, and then mixed with an alkaline solution to prepare sodium hypochlorite, and the chlorine temperature is reduced by spray water and radiator to reduce cost and energy consumption.
Efficient purification and full utilization of chlorine gas is achieved, environmental pollution is reduced, cost is low, energy consumption is low, and impurities are further removed by mixing mixed rare earth chloride liquid and cerium sulfate to achieve resource utilization.
Smart Images

Figure CN118954433A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of waste gas recovery, and in particular to a method and a system for recovering waste gas from acid leaching of bastnaesite. Background Art
[0002] Rare earth, as an indispensable metal raw material, plays a vital role in high-tech and green-tech products such as permanent magnets, wind turbines, electric vehicles, nickel-metal hydride batteries, lasers and fluorescent lamps due to its unique optical, electrical and magnetic properties.
[0003] As a country with abundant rare earth resources, my country not only has a huge output, but also covers all varieties of light, medium and heavy rare earth elements. Usually, multiple rare earth elements coexist in minerals. In order to reasonably and effectively develop and utilize my country's rare earth resources, its smelting and separation technology is particularly critical. Different rare earth elements require different separation technologies due to their different chemical properties. Taking cerium as an example, the smelting and separation technologies mainly include oxidative roasting-acid leaching and alkaline smelting and separation methods.
[0004] Alkali smelting is to use sodium hydroxide solution to roast the concentrate at low temperature, wash and filter the generated hydroxide, dissolve it in concentrated hydrochloric acid and neutralize it in ammonia water to obtain a rare earth chloride solution, and then concentrate and crystallize it to finally obtain a mixed rare earth chloride. Although this method has a high rare earth recovery rate, the process is complicated, the equipment is easily corroded, and the safety is poor, so it is not used in industrial production. On the contrary, the oxidation roasting-acid leaching method has become a more common rare earth refining method in current industrial production. This method first roasts the concentrate, and then recovers rare earth elements such as cerium through an acid leaching process. This method is not only easy to operate, but also relatively low in cost, so it has been widely used in the rare earth smelting industry.
[0005] During the smelting process of oxidation roasting-acid leaching, a large amount of chlorine-containing waste gas is inevitably generated. The emission of this type of waste gas poses a serious threat to the environment, and there is an urgent need to find an effective treatment solution. At present, there are four mainstream methods for treating this type of waste gas: (1) Reduction method: Although the reaction between hydrochloric acid and cerium dioxide can be inhibited by adding a reducing agent during the acid leaching process, thereby controlling the generation of chlorine at the source, this method is expensive because it requires a large amount of reducing agent and is therefore not suitable for large-scale production. (2) Adsorption method: Activated carbon, molecular sieves and other materials are used to adsorb harmful substances in the waste gas. However, this method is not completely effective in absorbing the waste gas and cannot completely remove harmful substances. (3) Condensation method: Harmful substances in the waste gas are condensed into liquid by lowering the temperature, and then separated and removed. However, the condensation temperature of chlorine is extremely low, resulting in excessive energy consumption in the production of this method. (4) Alkali dechlorination: Alkaline substances such as sodium hydroxide are used to absorb the acidic components in the waste gas. Although it can treat tail gas, this method cannot obtain valuable by-products, and the consumption of alkali is large, and the amount of wastewater treatment generated is also large. Summary of the invention
[0006] The present invention aims to solve the problems of incomplete treatment of chlorine-containing waste gas, failure to obtain valuable by-products, high cost and high energy consumption in the existing process of separating rare earth elements by oxidation roasting-acid leaching of bastnaesite, and proposes a method and system for recovering waste gas from acid leaching of bastnaesite.
[0007] The technical method of the present invention is as follows:
[0008] The present invention provides a method for recovering waste gas from acid leaching of bastcerium lanthanum ore, the method comprising:
[0009] S1, roasting bastnaesite to obtain oxidative roasted rare earth ore;
[0010] S2, leaching the oxidatively roasted rare earth ore with hydrochloric acid to obtain a mixed rare earth chloride solution and a mixed gas containing hydrogen chloride and chlorine;
[0011] S3, purifying the mixed gas with cerium sulfate to obtain purified chlorine and cerium sulfate;
[0012] S4. Mixing the purified chlorine gas with an alkaline solution to obtain sodium hypochlorite.
[0013] Optionally, step S3 further includes: after purifying the mixed gas with ceric sulfate, detecting the concentration of ceric sulfate, and if the concentration is lower than 10 g / L, replacing ceric sulfate with a concentration of 50 to 80 g / L.
[0014] Optionally, step S3 further includes: after purifying the mixed gas with cerium sulfate, spraying water to remove residual hydrogen chloride after purification.
[0015] Furthermore, after the water spraying step, the acidity of the water is detected, and if the acidity is higher than 0.5 mol / L, the spraying water is replaced.
[0016] Optionally, the method further comprises: mixing the mixed rare earth chloride solution with cerium sulfate.
[0017] Optionally, the purification temperature is 45-55° C., and the purification time is 1.5-2 hours.
[0018] Optionally, the mixing temperature is 30-40° C., and the mixing time is 1.5-2 h.
[0019] Optionally, the alkaline solution is sodium hydroxide, and the concentration of sodium hydroxide is 29-32%.
[0020] The present invention provides a system for recovering waste gas from acid leaching of bastnaesite. The method for recovering waste gas from acid leaching of bastnaesite adopts a recovery system, comprising: a roasting acid leaching unit, a purification tower, and an absorption tower connected in sequence.
[0021] The roasting and acid leaching unit is provided with an exhaust port, and the exhaust port of the roasting and acid leaching unit is used to discharge the mixed gas;
[0022] An air inlet and an exhaust port are arranged outside the purification tower, and a containing cavity is arranged inside the purification tower. The containing cavity, the exhaust port of the roasting acid leaching unit and the air inlet of the purification tower are connected, and high cerium sulfate is placed in the containing cavity, and high cerium sulfate purifies the mixed gas;
[0023] An air inlet is arranged outside the absorption tower, an absorption tank is arranged inside the purification tower, an alkaline solution is placed in the absorption tank, an exhaust port of the purification tower is connected with the air inlet of the absorption tower, and the purified gas is mixed with the alkaline solution to obtain sodium hypochlorite.
[0024] Furthermore, a deep purification tower is installed between the purification tower and the absorption tower, and a sprayer is provided at the top of the deep purification tower; a radiator is provided at the bottom of the deep purification tower.
[0025] The present invention has the following beneficial effects:
[0026] (1) The present invention uses cerium sulfate to purify a mixed gas containing hydrogen chloride and chlorine to remove hydrogen chloride in the mixed gas and improve the purity and yield of chlorine. The purified chlorine is then mixed with an alkaline solution to prepare sodium hypochlorite, thereby making full use of the chlorine and avoiding harm to the environment.
[0027] (2) The mass fraction of sodium hypochlorite obtained by the present invention is in the range of 12% to 13%, which meets industrial requirements.
[0028] (3) Compared with the prior art, the harmful substances in the exhaust gas are condensed into liquid by cooling. The present invention installs a sprayer and a radiator to cool the chlorine gas to 30-40°C, and reacts the 30-40°C chlorine gas with an alkaline solution to remove the chlorine gas. This method has low cost and low energy consumption.
[0029] (4) The present invention mixes the mixed rare earth chloride solution produced after roasting and hydrochloric acid leaching and the cerium sulfate produced during the purification process to further remove impurities, thereby realizing resource utilization.
[0030] (5) The system of the present invention comprises a roasting acid leaching unit, a purification tower and an absorption tower, wherein the roasting acid leaching unit performs roasting acid leaching, the gas after roasting acid leaching is passed into the purification tower for purification, and finally the purified gas is passed into the absorption tower for mixing. The system has a simple structure and is easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The present invention is a flow chart of the method for recovering waste gas from acid leaching of bastnaesium lanthanum ore. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below through specific implementation cases and accompanying drawings. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of protection of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0033] The present invention provides a method for recovering waste gas from acid leaching of bastnaesite. Figure 1 , the recovery method comprises:
[0034] S1. Roasting bastnaesite to obtain oxidatively roasted rare earth ore.
[0035] Here, the calcination temperature is 510 to 520° C., and the calcination time is 1.5 to 2.5 hours. For example, the temperature is 515° C. or 517° C., and the calcination time is 2 hours.
[0036] In one embodiment, bastnaesite includes ReFCO3 and an impurity barium oxide with a content of about 2-3%. Re includes one or more of Ce, La, Pr, and Nd.
[0037] Specifically, ReFCO3 roasting will decompose into oxidized roasted rare earth ore (including Re2O3, CeO2), ReF3, and CO2. Here, Re includes one or more of Ce, La, Pr, and Nd.
[0038] S2, leaching the oxidatively roasted rare earth ore with hydrochloric acid to obtain a mixed rare earth chloride solution and a mixed gas containing hydrogen chloride and chlorine.
[0039] Here, the oxidized roasted rare earth ore is passed through a 200-mesh sample sieve, and the rare earth mass percentage and cerium dioxide content in the oxidized roasted rare earth ore are detected. Here, the consumption of hydrochloric acid in the acid leaching process is determined based on the rare earth mass percentage and the rare earth leaching rate in the acid leaching process. The amount of chlorine generated is estimated based on the cerium dioxide content and the rare earth leaching rate.
[0040] Specifically, the acid leaching step includes: using pure water as base water, using oxidative roasting rare earth ore for slurry preparation, adding industrial hydrochloric acid to the slurry for stirring reaction according to the rare earth content, and controlling the residual acidity of the reaction to be 1.1 mol / L to 1.4 mol / L.
[0041] Here, the acid immersion temperature is 80° C. or higher, and the acid immersion time is 0.5 to 1.5 h.
[0042] S3. Purify the mixed gas with cerium sulfate to obtain purified chlorine and cerium sulfate.
[0043] Specifically, cerium sulfate is in a mixed rare earth sulfate solution. Among them, the mixed rare earth sulfate solution containing 76.46 g / L cerium sulfate has an acidity of 2.5 mol / L.
[0044] Here, when the acidity of the mixed rare earth sulfate solution is too low, the cerium sulfate is easily hydrolyzed to produce cerium hydroxide precipitation, which reduces the actual use effect of the cerium sulfate.
[0045] In one embodiment, the preparation method of cerium sulfate includes: sulfuric acid reacts with cerium dioxide in oxidative roasting of rare earth ore to generate cerium sulfate.
[0046] The reaction formula is:
[0047] 2H2SO4+CeO2=Ce(SO4)2+2H2O
[0048] In one embodiment, step S3 includes: reacting ceric sulfate with hydrogen chloride in the mixed gas to obtain ceric sulfate and chlorine.
[0049] The reaction formula is:
[0050] 3Ce(SO4)2+3HCl=1Ce2(SO4)3+1H2SO4+1Cl2↑
[0051] It should be noted that cerium sulfate does not react with chlorine.
[0052] In one embodiment, the cerium sulfate in step S3 is mixed with a mixed rare earth chloride solution. Here, the mixed rare earth chloride solution contains barium chloride impurities, and the addition of cerium sulfate will cause a double decomposition reaction to generate barium sulfate precipitate and mixed rare earth chloride solution.
[0053] The purification temperature is 45-55°C and the purification time is 1.5-2h. It should be noted that after the oxidation roasting rare earth ore is leached with hydrochloric acid, there is still water vapor in the mixed gas. When reacting at 45-55°C, the water vapor and chlorine gas are cooled while ensuring that the cerium sulfate fully and efficiently absorbs the hydrogen chloride gas, thereby ensuring that the initial temperature of the subsequent alkali absorption tower is too high, which will cause the sodium hypochlorite to decompose again, and the water vapor is removed during the cooling process.
[0054] Step S3 also includes: ① After purifying the mixed gas with cerium sulfate, the concentration of cerium sulfate is detected. If the concentration is lower than 10g / L, cerium sulfate with a concentration of 50-80g / L is replaced. For example, cerium sulfate with a concentration of 60, 70, or 75g / L can be replaced. Here, the purpose of replacement is because when the concentration of cerium sulfate solution is lower than 10g / L, the absorption conversion rate of hydrogen chloride gas is too low.
[0055] Here, since residual hydrogen chloride may exist during the purification process, step S3 also includes: ② after purifying the mixed gas with cerium sulfate, spray water is used to remove the residual hydrogen chloride after purification. Here, the spray water containing hydrogen chloride can be used as acid leaching bottom water.
[0056] It should be noted that there is a strict order relationship between ① and ②, ① comes first and ② comes later. ① first converts hydrogen chloride to increase the chlorine content, and then ② is used to further remove the residual hydrogen chloride after purification. Both ① and ② are methods for further removing hydrogen chloride from the mixed gas to ensure the purity of chlorine, thereby ensuring the qualified rate of the generated sodium hypochlorite.
[0057] Here, if the concentration of ① cerium sulfate is lower than 10g / L, the absorption conversion rate of hydrogen chloride gas is too low, resulting in a large amount of hydrogen chloride being sprayed with water, so that there is a small amount of hydrogen chloride in the mixed gas, thereby increasing the workload of chlorine purification.
[0058] Here, after the step ② of spraying water, the acidity of the water is tested. If the acidity is higher than 0.5 mol / L, the spraying water is replaced. Because when the acidity is higher than 0.5 mol / L, hydrogen chloride will slowly volatilize, and with the continuous increase in acidity, the amount of volatilization will increase, which will cause the subsequent hydrogen chloride gas to react with the alkaline solution, reduce the concentration of sodium hypochlorite, and make the generated sodium hypochlorite unqualified. At the same time, spraying water can reduce the temperature to 30-40°C, which is convenient for subsequent reactions.
[0059] S4. Mixing the purified chlorine gas with an alkaline solution to obtain sodium hypochlorite.
[0060] The mass ratio of the purified chlorine gas to the 30% alkaline solution is 70-73:263-268. For example, the mass ratio is 71:266; the mass ratio is 72:267.
[0061] Specifically, the alkaline solution is sodium hydroxide. The concentration of sodium hydroxide is 29 to 32%. For example, the concentration of sodium hydroxide is 30%.
[0062] Here, the mixing temperature is 30-40°C, and the mixing time is 1.5-2 hours. Here, it should be noted that the mixing time is mainly based on the qualified mass percentage content of sodium hypochlorite in the subsequent No. 1 alkaline solution absorption tank.
[0063] Preferably, the step of mixing the purified chlorine gas with the alkaline solution comprises: sequentially placing the purified chlorine gas into two alkaline solutions of the same mass percentage until the reaction is completed.
[0064] Specifically, the mass fraction of sodium hypochlorite is mainly determined by the mass percentage of the alkaline solution. The mass fraction of sodium hypochlorite obtained by fully absorbing chlorine with 29% to 32% alkaline solution is maintained at 12% to 13%. The higher the purity of chlorine, the higher the sodium hypochlorite content. In order to prevent excessive chlorine from escaping, a two-stage sodium hydroxide absorption is set.
[0065] The present invention utilizes rare earth liquid containing cerium sulfate and alkaline solution to efficiently absorb and convert hydrogen chloride gas, thereby increasing the yield of chlorine gas, and simultaneously dissolves a small amount of oxidized roasted rare earth ore in the waste gas to produce cerium sulfate molecules, thereby increasing the conversion efficiency of hydrogen chloride gas, and obtaining a sodium hypochlorite solution with a mass fraction of 12% to 13%. Here, the sodium hypochlorite with a mass fraction of 12% to 13% meets the industrial grade requirements.
[0066] The present invention provides a system for recovering waste gas from acid leaching of bastcerium lanthanum ore. The method for recovering waste gas from acid leaching of bastcerium lanthanum ore adopts a recovery system, comprising: a roasting and acid leaching unit, a purification tower, and an absorption tower connected in sequence. The roasting and acid leaching unit is provided with an exhaust port, and the exhaust port of the roasting and acid leaching unit is used to discharge mixed gas; the purification tower is provided with an air inlet and an exhaust port on the outside, and the purification tower is provided with a containing cavity inside, and the containing cavity, the exhaust port of the roasting and acid leaching unit, and the air inlet of the purification tower are connected, and high cerium sulfate is placed in the containing cavity, and the high cerium sulfate purifies the mixed gas; the absorption tower is provided with an air inlet on the outside, and the purification tower is provided with an absorption tank inside, and an alkaline solution is placed in the absorption tank, and the exhaust port of the purification tower is connected with the air inlet of the absorption tower, and the purified gas is mixed with the alkaline solution to obtain sodium hypochlorite.
[0067] Specifically, a fan is provided between the roasting and acid leaching unit and the purification tower, and the fan transmits the chlorine in the roasting and acid leaching unit to the purification tower. The mixed rare earth sulfate solution with an acidity of 2.5±0.5 mol / L in the purification tower contains 50-80 g / L of cerium sulfate as a purifier to treat the mixed gas. The bottom of the purification tower is provided with a radiator to ensure that the purification temperature is 45-55°C.
[0068] There is a deep purification tower between the purification tower and the absorption tower. The top of the deep purification tower is equipped with a sprayer, and the bottom of the deep purification tower is equipped with a radiator. When the purified chlorine gas is introduced from the bottom of the purification tower, pure water is sprayed out from the top as the purification liquid. A radiator is installed at the bottom to remove trace hydrogen chloride in the gas and obtain high-purity chlorine gas with a temperature below 40°C.
[0069] Specifically, the absorption tower has the function of absorbing chlorine. There are absorption tank No. 1 and absorption tank No. 2 inside the absorption tower. The chlorine is passed into absorption tank No. 1 containing 29-32% alkaline solution, and its reaction temperature is controlled at 30-40°C through a radiator. After the reaction is completed, a sample is taken to detect the concentration of sodium hypochlorite, and the remaining gas enters absorption tank No. 2; the same mass fraction of alkaline solution is added to absorption tank No. 2 to absorb the residual chlorine after the above reaction again. When the sodium hypochlorite concentration in absorption tank No. 1 is qualified and discharged, the alkaline solution in absorption tank No. 2 is transferred to absorption tank No. 1, and a new alkaline solution is injected into absorption tank No. 2, and the exhaust gas meets the emission standards.
[0070] Here, the absorption method adopts the foaming method. Foaming is to disperse the chlorine gas from the bottom of the absorption tank through the explosion plate, which can increase the absorption area, control the gas flow rate, and fully absorb the chlorine gas.
[0071] Here, the chlorine is basically completely absorbed by the No. 1 absorption tank and the No. 2 absorption tank, and almost no chlorine is discharged into the atmosphere. The No. 1 absorption tank is used to obtain a sodium hypochlorite solution with a mass fraction of 12% to 13%, and the No. 2 absorption tank absorbs the unused chlorine in the No. 1 absorption tank.
[0072] In order to better understand the above exemplary embodiments of the present invention, they are further described below with reference to specific examples.
[0073] Example 1
[0074] Step 1: Weigh 12 kg of Sichuan fluorocarbon cerium rare earth flotation ore after oxidation roasting, grind it for sample preparation, and pass all of it through a 200-mesh sample sieve to obtain an oxidation roasted rare earth ore; wherein the oxidation roasted rare earth ore is tested to have a rare earth content of 50.12% and a cerium dioxide content of 24.05%;
[0075] Step 2: Add 4L of pure water as bottom water to a 50L closed reaction tank, weigh 11Kg of the oxidized roasted rare earth ore obtained in step 1 for slurry preparation, and continuously add 15L of industrial hydrochloric acid to the slurry for stirring reaction, the reaction temperature is 85°C, the reaction time is 1h, and the residual acidity of the reaction is detected to be 1.3mol / L;
[0076] Step 3: Pass the mixed gas produced by the reaction in step 2 into a purification spray tower, and treat the mixed gas with 10L of a mixed rare earth sulfate solution with an acidity of 2.5mol / L and a cerium sulfate content of 76.46g / L as a conversion and purification agent, and control the reaction temperature to 50°C. After the reaction is completed, the cerium sulfate content in the rare earth solution is detected to be 14.21g / L;
[0077] Step 4: The chlorine gas obtained in step 3 is passed into a deep purification tower, and 4L of pure water is used as a purification liquid to deeply treat the mixed gas. After the reaction is completed, the acidity of the purified liquid is detected to be 0.05mol / L;
[0078] Step 5: Add 2L of 30% alkaline solution to the No. 1 absorption tank, introduce the gas obtained in step 4 into the explosion plate, disperse and pass it from the bottom of the absorption tank, absorb chlorine in a foaming manner, control the reaction temperature to 40°C, and detect the sodium hydroxide concentration of 0.25mol / L and the sodium hypochlorite concentration of 12.42% at the end of the reaction;
[0079] Step 6: Add 2L of 30% alkaline solution to absorption tank No. 2 to absorb the residual chlorine after the reaction in step 5 in the same way. After the reaction, the sodium hydroxide concentration is detected to be 8.82 mol / L.
[0080] Example 2
[0081] Step 1: Weigh 12 kg of Sichuan fluorocarbon cerium rare earth flotation ore after oxidation roasting, grind and sample, and pass all of them through a 200-mesh sample sieve to obtain oxidation roasted rare earth ore; wherein, the rare earth content is 60.24%, and the cerium dioxide content is 28.91%;
[0082] Step 2: Add 4L of pure water as bottom water to a 50L closed reaction tank, weigh 11Kg of the oxidized roasted rare earth ore obtained in step 1 for slurry preparation, and continuously add 15.5L of industrial hydrochloric acid to the slurry for stirring reaction. The reaction temperature is 84°C, the reaction time is 1h, and the residual acidity of the reaction is detected to be 1.26mol / L;
[0083] Step 3: Pass the mixed gas produced by the reaction in step 2 into a purification spray tower, and treat the mixed gas with 10L of a mixed rare earth sulfate solution with an acidity of 2.6mol / L and a cerium sulfate content of 75.58g / L as a conversion and purification agent, and control the reaction temperature to 50±5°C. After the reaction is completed, the cerium sulfate content in the rare earth solution is detected to be 13.02g / L;
[0084] Step 4: The chlorine gas obtained in step 3 is passed into a deep purification tower, and 4L of pure water is used as a purification liquid to deeply treat the mixed gas. After the reaction is completed, the acidity of the purified liquid is detected to be 0.07mol / L;
[0085] Step 5: Add 2L of 30% alkaline solution to the No. 1 absorption tank, introduce the gas obtained in step 4 into the explosion plate, disperse and pass it from the bottom of the absorption tank, absorb chlorine in a foaming manner, control the reaction temperature to 35±5°C, and detect the sodium hydroxide concentration of 0.21mol / L and the sodium hypochlorite concentration of 12.49% at the end of the reaction;
[0086] Step 6: Add 2L of 30% alkaline solution to absorption tank No. 2 to absorb the residual chlorine gas after the reaction in step 5 in the same way. After the reaction, the sodium hydroxide concentration is detected to be 8.54 mol / L.
[0087] Example 3
[0088] Step 1: Weigh 12 kg of Sichuan fluorocarbon cerium rare earth flotation ore after oxidation roasting, grind and sample, and pass all of them through a 200-mesh sample sieve to obtain oxidation roasting rare earth ore; wherein, the rare earth content is 70.14% and the cerium dioxide content is 33.66%;
[0089] Step 2: Add 4L of pure water as bottom water to a 50L closed reaction tank, weigh 11Kg of the oxidized roasted rare earth ore obtained in step 1 for slurry preparation, and continuously add 15.7L of industrial hydrochloric acid to the slurry for stirring reaction. The reaction temperature is 88°C, the reaction time is 1h, and the residual acidity of the reaction is detected to be 1.14mol / L;
[0090] Step 3: Pass the mixed gas produced by the reaction in step 2 into a purification spray tower, and treat the mixed gas with 10L of a mixed rare earth sulfate solution with an acidity of 2.8mol / L and a cerium sulfate content of 73.28g / L as a conversion and purification agent, and control the reaction temperature to 50±5°C. After the reaction is completed, the cerium sulfate content in the rare earth solution is detected to be 11.62g / L;
[0091] Step 4: The clean gas obtained in step 3 is passed into a deep purification tower, and 4L of pure water is used as a purification liquid to deeply treat the mixed gas. After the reaction is completed, the acidity of the purified liquid is detected to be 0.09mol / L;
[0092] Step 5: Add 2L of 30% alkaline solution to the No. 1 absorption tank, introduce the gas obtained in step 4 into the explosion plate, disperse and pass it from the bottom of the absorption tank, absorb chlorine in a foaming manner, control the reaction temperature to 35±5°C, and detect the sodium hydroxide concentration of 0.15mol / L and the sodium hypochlorite concentration of 12.59% at the end of the reaction;
[0093] Step 6: Add 2L of 30% alkaline solution to absorption tank No. 2 to absorb the residual chlorine after the reaction in step 5 in the same way. After the reaction, the sodium hydroxide concentration is detected to be 8.14 mol / L.
Claims
1. A method for recovering waste gas from acid leaching of bastnaesite, characterized in that: The recovery method comprises: S1, roasting bastnaesite to obtain oxidative roasted rare earth ore; S2, leaching the oxidatively roasted rare earth ore with hydrochloric acid to obtain a mixed rare earth chloride solution and a mixed gas containing hydrogen chloride and chlorine; S3, purifying the mixed gas with cerium sulfate to obtain purified chlorine and cerium sulfate; S4. Mixing the purified chlorine gas with an alkaline solution to obtain sodium hypochlorite.
2. The recycling method according to claim 1, characterized in that: The S3 step also includes: After purifying the mixed gas with ceric sulfate, the concentration of ceric sulfate is detected. If the concentration is lower than 10 g / L, ceric sulfate with a concentration of 50 to 80 g / L is replaced.
3. The recycling method according to claim 1, characterized in that: The S3 step also includes: After the mixed gas is purified by high cerium sulfate, the residual hydrogen chloride is removed by spraying water.
4. The recycling method according to claim 3, characterized in that: After the water spraying step, the acidity of the water is tested. If the acidity is higher than 0.5 mol / L, the spraying water is replaced.
5. The recycling method according to claim 1, characterized in that: The method further comprises: The mixed rare earth chloride solution is mixed with cerium sulfate.
6. The recycling method according to claim 1, characterized in that: The purification temperature is 45-55°C and the purification time is 1.5-2h.
7. The recycling method according to claim 1, characterized in that: The mixing temperature is 30-40°C, and the mixing time is 1.5-2h.
8. The recycling method according to claim 1, characterized in that: The alkaline solution is sodium hydroxide, and the concentration of sodium hydroxide is 29-32%.
9. A system for recovering waste gas from acid leaching of bastnaesite, characterized in that: The method for recovering waste gas from acid leaching of bastnaesite according to any one of claims 1 to 8 adopts a recovery system, comprising: a roasting and acid leaching unit, a purification tower, and an absorption tower connected in sequence, The roasting and acid leaching unit is provided with an exhaust port, and the exhaust port of the roasting and acid leaching unit is used to discharge the mixed gas; An air inlet and an exhaust port are arranged outside the purification tower, and a containing cavity is arranged inside the purification tower. The containing cavity, the exhaust port of the roasting acid leaching unit and the air inlet of the purification tower are connected, and high cerium sulfate is placed in the containing cavity, and high cerium sulfate purifies the mixed gas; An air inlet is arranged outside the absorption tower, an absorption tank is arranged inside the purification tower, an alkaline solution is placed in the absorption tank, an exhaust port of the purification tower is connected with the air inlet of the absorption tower, and the purified gas is mixed with the alkaline solution to obtain sodium hypochlorite.
10. The recovery system according to claim 9, characterized in that: A deep purification tower is installed between the purification tower and the absorption tower. A sprayer is provided at the top of the deep purification tower; and a radiator is provided at the bottom of the deep purification tower.
Citation Information
Patent Citations
Method for selectively extracting non-cerium rare earth from mixed rare earth ore concentrate
CN109161702A
Non-metal-containing oxyanion removal from waters using rare earths
WO2012141897A2