Two-step chemically modified reinforced recycled aggregate and preparation method thereof
Through a two-step chemical modification method, active ions are excited and reacted with siliceous raw materials to form gel-filled regenerated aggregates, solving the problems of complex reinforcement process of regenerated aggregates, high energy consumption and harmful ion pollution in the prior art. It has achieved improvement in the performance of recycled aggregates and strengthened interface transition zones, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202411206934.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing recycled aggregate strengthening methods have complex operations, high energy consumption, high cost and harmful ion pollution, making it difficult to achieve safe, environmentally friendly and low-cost resource utilization.
Using a two-step chemical modification method, the first step is to soak the regenerated aggregate using an exciter solution with a pH value less than 7. The second step is to add siliceous raw materials for mechanical stirring, excite active ions and react with siliceous raw materials to form Gel matter fills the pores of cement-based materials to improve the strength of regenerated aggregates and the performance of interface transition zones.
It has achieved significant improvement in the performance of recycled aggregates, which are simple to operate, low cost, safe, and free of harmful ions. It is suitable for large-scale production, and reduces porosity and enhances the application potential of recycled aggregates.
Smart Images

Figure CN118954994A_ABST
Abstract
Description
Technical Field
[0001] The invention discloses a two-step chemically modified reinforced recycled aggregate and a preparation method thereof, belonging to the field of building materials. Background Art
[0002] With the acceleration of my country's urbanization process, the amount of construction waste generated during the construction process is also increasing. Recycled aggregate is a product obtained by sorting, removing or crushing waste concrete. Recycled aggregate can be used to prepare resource-based products such as recycled concrete and mortar. The reuse of recycled aggregate is a key step in realizing the resource utilization of construction waste, and the resource utilization of recycled aggregate can also effectively solve a series of problems such as the shortage of construction resources.
[0003] The defects of recycled aggregates such as complex sources, many edges and corners, rough surface and internal microcracks limit the recycling of recycled aggregates from construction waste. Some studies have strengthened recycled aggregates by removing attached mortar. CN202211359790.3 discloses a method for strengthening recycled aggregates. In this invention, the recycled aggregates are first screened and cleaned, and then the recycled aggregates are soaked in acid for 7 days, taken out and rinsed with clean water, and then the treated recycled aggregates are placed in an autoclave and autoclaved for 8 hours, and finally ball-milled in a ball mill for 4 minutes, and the treated recycled aggregates are obtained after screening. Although this method can improve the performance of recycled aggregates, the process is complicated, the energy consumption is high, and the cost is high. Acid treatment will increase harmful ions, such as Cl - and SO4 2- , reducing the durability of concrete. At the same time, in order to reduce the acidity, the flushing process requires a large amount of water. The waste treatment of these washing water and residual treatment solutions will cause new environmental problems. There are also studies that achieve the purpose of strengthening recycled aggregates by strengthening the interface transition zone. For example, the "Journal of Building Science and Engineering" titled "Research Progress on Performance Strengthening of Recycled Aggregates from Construction Waste" reported that adding appropriate mineral admixtures (such as fly ash, silica fume, slag, etc.) to concrete can improve the performance of concrete. The principle of mineral admixtures to improve aggregate performance is the pore refinement of the attached mortar and the secondary hydration between the mineral admixture and the cement hydration product (mainly Ca(OH)2). If a method for strengthening recycled aggregates that is simple to operate, low in cost, safe, free of harmful ions, low in energy consumption and more environmentally friendly can be invented, it will effectively promote the resource utilization of recycled aggregates. For the current single chemical strengthening, such as acid strengthening, it is easy to cause pollution, and the leachate will introduce harmful ions, causing secondary pollution. The siliceous raw material reacts with the hydration product calcium oxide in the regenerated mortar to produce secondary hydration, but the long-term carbonization of calcium hydroxide is affected and the effect is not good. Therefore, this patent involves two-step chemical excitation. Summary of the invention
[0004] In view of the shortcomings of the existing methods, the present invention provides a two-step chemically modified recycled aggregate strengthening method, which is simple and controllable.
[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0006] The present invention provides a two-step chemically modified recycled aggregate strengthening method, wherein the first step is chemical activator soaking, and the second step is siliceous raw material filling. Furthermore, the recycled aggregate is strengthened by the following two steps:
[0007] (1) dissolving the activator in deionized water, and adjusting the activator solution to an acidic solution with a pH value less than 7;
[0008] (2) Under room temperature conditions, the recycled aggregate is soaked in an activator solution for several hours to obtain the first step of strengthening the recycled aggregate;
[0009] (3) Add the siliceous raw material to the activator solution, mix evenly under mechanical stirring conditions, and soak for several hours to obtain the second step reinforced recycled aggregate.
[0010] Furthermore, in the process of preparing the activator, the proportion of the activator is 0.1-2% of the mass of the recycled aggregate.
[0011] Furthermore, during the process of adding the siliceous raw material, the proportion of the siliceous raw material is 0-20% of the mass of the recycled aggregate.
[0012] Furthermore, in the first step of the reaction, the recycled aggregate is first soaked in an activator solution at room temperature for 30 minutes to 48 hours, and in the second step of the reaction, a siliceous raw material is added, mixed evenly under mechanical stirring conditions, and then soaked for 30 minutes to 24 hours.
[0013] Furthermore, the siliceous raw materials are silica ash, fly ash, silicon dioxide, mineral powder and the like.
[0014] The present invention is under room temperature conditions.
[0015] Through two-step chemical modification, the first step excites active ions, which then react with the siliceous raw materials in the second step to achieve efficient strengthening of dissolution and filling, significantly improve the performance of the recycled aggregate, and at the same time improve the performance of the interface transition zone, thereby increasing the application potential of the recycled aggregate. The two-step chemical modification and strengthening of the recycled aggregate provided by the present invention, wherein the activator solution is prepared in the laboratory, and the siliceous raw materials are purchased commercially. The purpose of the first step of the two-step chemical modification and strengthening of the recycled aggregate provided by the present invention is to reduce the weak interface transition zone, and the excitation process excites more active ions such as Ca through the reaction of the activator with hydration products such as calcium hydroxide CH, calcium carbonate CaCO3 and calcium silicate hydrate CSH. 2+ 、Al 3+ , Fe3+ . The second step of chemical modification is based on the reaction of the siliceous raw materials with the active ions stimulated by the first step of modification. Through the volcanic ash reaction, a gel substance is formed, which is filled in the pores of the cement-based material at the same time, thereby enhancing the performance of the recycled aggregate. The siliceous raw materials can react chemically with the old cement mortar. By accelerating the hydration reaction and filling the micropores in the aggregate and mortar structure of the recycled aggregate, the porosity of the recycled aggregate can be reduced and the strength of the recycled aggregate can be enhanced. The inorganic silicate solution reacts chemically with the calcium hydroxide on the surface of the recycled aggregate. The generated silicate silicate gel allows the microcracks on the surface of the recycled aggregate to be bonded, making the recycled aggregate more soluble. The leachate can be used for the molding of recycled mortar and recycled concrete at the same time, without causing secondary pollution, and at the same time improving the hydration performance.
[0016] The beneficial effects of the present invention are:
[0017] (1) Two-step chemical modification: first, active ions are excited, and then in the second step, they react with the siliceous raw materials to achieve efficient strengthening of dissolution and filling, improve the performance of recycled aggregates, and at the same time improve the strength of the interface transition zone, thereby increasing the application potential of recycled aggregates.
[0018] (2) The two-step chemical modification method for strengthening recycled aggregates is simple to operate and has the advantages of low cost, safety, no harmful ions, low energy consumption and greater environmental protection, and is suitable for large-scale production.
[0019] (3) The filtrate after treating the recycled aggregate can be used for the molding of recycled mortar and recycled concrete without loss, which is beneficial to the cement hydration process.
[0020] (4) Based on the two-step chemical modification method to strengthen recycled aggregate, the weak interface transition zone of the recycled aggregate is reduced, the filling of CSH gel and the improvement of the interface transition zone between the new and old mortar are synergistically strengthened. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The saturated surface dry water absorption of recycled aggregate was enhanced by two-step chemical modification.
[0022] Figure 2 Crushing value for two-step chemical modification enhanced regeneration.
[0023] Figure 3 The compressive strength of recycled aggregate is enhanced by two-step chemical modification.
[0024] Figure 4 It is the compressive strength of mortar from recycled aggregate filtrate after two-step chemical modification.
[0025] Figure 5 Comparison of the interface transition zone between unmodified recycled aggregate and modified recycled aggregate. DETAILED DESCRIPTION
[0026] The present invention is further described below by way of examples. The following description is only for the purpose of explaining the present invention and is not intended to limit its contents.
[0027] Example 1
[0028] (1) First step chemical modification and strengthening of recycled aggregate: 1 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 17 h to obtain the first step chemical modification and strengthening of recycled aggregate.
[0029] (2) 24 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the solution was soaked for 1 hour. After the soaking time was reached, the recycled aggregate was strengthened by the second step of chemical modification. The test showed that the recycled aggregate was strengthened.
[0030] Figure 1 , Figure 2 , Figure 3 , Figure 4 The two-step chemical modification strengthens the saturated surface dry water absorption rate, crushing value, mortar compressive strength of the recycled aggregate and the mortar compressive strength of the filtrate of the recycled aggregate, respectively, in Example 1, Example 2 and Comparative Example 1. The specific test methods for the saturated surface dry water absorption rate, crushing value, mortar compressive strength of the recycled aggregate and the mortar compressive strength of the filtrate of the recycled aggregate are as follows:
[0031] ① Saturated surface dry water absorption
[0032] The saturated surface dry water absorption rate of the recycled aggregates treated in Example 1, Example 2 and Comparative Example 1 was tested. The change in saturated surface dry water absorption rate was used to characterize the effect of the two-step chemical modification on the performance of the recycled aggregate. The water absorption rate test experiment was conducted with reference to the saturated surface dry water absorption rate step 7.19 of GB / T 14684-2011 "Standard for Construction Sand".
[0033] ② Crushing index
[0034] The crushing value test was performed on the recycled aggregates after being treated in Example 1, Example 2 and Comparative Example 1, and the test was performed with reference to the crushing index step 7.11 in GB / T14685-2011 "Crushed Stone and Pebbles for Construction".
[0035] ③ Preparation, molding and strength testing of mortar with two-step chemical modification and strengthening of recycled aggregate
[0036] The recycled aggregates treated in Example 1, Example 2 and Comparative Example 1 were subjected to mortar preparation, molding and strength testing, and the water-cement ratio was determined to be 0.45, with reference to 7 mortar preparation, 8.2 molding and 10.2 compressive strength determination in GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)".
[0037] ④ Preparation, molding and strength testing of mortar with two-step chemical modification to strengthen recycled aggregate filtrate
[0038] The mortar preparation and strength test were performed on the recycled aggregate filtrate after treatment in Example 1, Example 2 and Comparative Example 1, and the water-cement ratio was determined to be 0.5. The recycled aggregate after two-step chemical modification and strengthening was passed through a 50-mesh sieve to obtain a filtrate. According to 7 Preparation of mortar, 8.2 Molding and 10.2 Compressive strength determination in GB / T17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)", the preparation, molding and compressive strength test of the recycled aggregate filtrate mortar were performed.
[0039] Example 2
[0040] (1) First step chemical modification and strengthening of recycled aggregate: 1 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 17 h to obtain the first step chemical modification and strengthening of recycled aggregate.
[0041] (2) 14.4 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the solution was soaked for another hour to obtain the second step chemically modified and strengthened recycled aggregate. The test showed that the recycled aggregate was strengthened.
[0042] Figure 1 , Figure 2 , Figure 3 , Figure 4 They are respectively Example 1, Example 2 and Comparative Example 1, and the saturated surface dry water absorption, crushing value, mortar compressive strength of the recycled aggregate and the mortar compressive strength of the recycled aggregate filtrate are strengthened by two-step chemical modification. The specific test method is as described in Example 1.
[0043] Example 3
[0044] (1) First step chemical modification and strengthening of recycled aggregate: 0.5 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 48 h to obtain the first step chemical modification and strengthening of recycled aggregate.
[0045] (2) 24 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the solution was soaked for 1 hour. After the soaking time was reached, the recycled aggregate was strengthened by the second step of chemical modification. The test showed that the recycled aggregate was strengthened.
[0046] Example 4
[0047] (1) First step chemical modification and strengthening of recycled aggregate: 9.5 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 1 hour to obtain the first step chemical modification and strengthening of recycled aggregate.
[0048] (2) 24 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the solution was soaked for 1 hour. After the soaking time was reached, the recycled aggregate was strengthened by the second step of chemical modification. The test showed that the recycled aggregate was strengthened.
[0049] Example 5
[0050] (1) First step chemical modification and strengthening of recycled aggregate: 3 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 10 h to obtain the first step chemical modification and strengthening of recycled aggregate.
[0051] (2) 48 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the soaking was continued for 2 h. After the soaking time was reached, the recycled aggregate was chemically modified and strengthened in the second step. After testing, the recycled aggregate was strengthened.
[0052] Example 6
[0053] (1) First step chemical modification and strengthening of recycled aggregate: 1 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 36 h to obtain the first step chemical modification and strengthening of recycled aggregate.
[0054] (2) 96 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the soaking was continued for 1 hour. After the soaking time was reached, the recycled aggregate was chemically modified and strengthened in the second step. After testing, the recycled aggregate was strengthened.
[0055] Example 7
[0056] (1) First step chemical modification and strengthening of recycled aggregate: 2 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 24 h to obtain the first step chemical modification and strengthening of recycled aggregate.
[0057] (2) 96 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the solution was soaked for 30 min. After the soaking time was reached, the recycled aggregate was strengthened by the second step of chemical modification. The test showed that the recycled aggregate was strengthened.
[0058] Example 8
[0059] (1) First step chemical modification and strengthening of recycled aggregate: 9.6 g of activator was dissolved in 420 g of deionized water, stirred evenly at room temperature, 480 g of recycled aggregate was poured into the prepared activator solution, and soaked for 30 min to obtain the first step chemical modification and strengthening of recycled aggregate.
[0060] (2) 96 g of siliceous raw material was added to the activator solution in which the recycled aggregate was soaked, and the solution was soaked for 30 min. After the soaking time was reached, the recycled aggregate was strengthened by the second step of chemical modification. The test showed that the recycled aggregate was strengthened.
[0061] Comparative Example 1
[0062] (1) Prepare 420 g of deionized water, pour 480 g of recycled aggregate into the prepared deionized water, and soak for 17 hours to obtain the recycled aggregate processed in the first step.
[0063] (2) Add 24 g of siliceous raw material into the activator solution for soaking the recycled aggregate and continue soaking for 1 hour. After the soaking time is reached, the recycled aggregate for the second step treatment is obtained.
[0064] Figure 1 , Figure 2 , Figure 3 , Figure 4 They are respectively Example 1, Example 2 and Comparative Example 1, and the saturated surface dry water absorption, crushing value, mortar compressive strength of the recycled aggregate and the mortar compressive strength of the recycled aggregate filtrate are strengthened by two-step chemical modification. The specific test method is as described in Example 1.
[0065] Comparative Example 2
[0066] (1) Dissolve 1 g of activator in 420 g of deionized water and stir evenly at room temperature. Pour 480 g of recycled aggregate into the prepared activator solution and soak for 17 hours to obtain the first step of treated recycled aggregate.
[0067] (2) No siliceous raw material is added to the activator solution for soaking the recycled aggregate, and the soaking is continued for 1 hour. After the soaking time is reached, the recycled aggregate for the second step treatment is obtained.
Claims
1. A two-step chemically modified recycled aggregate strengthening method, characterized in that: The first step is chemical activator soaking, and the second step is silicon raw material filling.
2. The two-step chemically modified recycled aggregate strengthening method according to claim 1, characterized in that: The strengthening of recycled aggregates is done by the following method; method: (1) Prepare an activator solution with a pH value less than 7; (2) Soaking the recycled aggregate in an activator solution for several hours to obtain the first step of strengthening the recycled aggregate; (3) After the first step of strengthening treatment, the siliceous raw material is added to the activator solution, mixed evenly under mechanical stirring conditions, and soaked for several hours to obtain the recycled aggregate for the second step of strengthening.
3. The two-step chemically modified recycled aggregate strengthening method according to claim 2, characterized in that: The proportion of the activator is 0.1-2% of the mass of the recycled aggregate.
4. The two-step chemically modified recycled aggregate strengthening method according to claim 2, characterized in that: The proportion of the siliceous raw material is 0-20% of the mass of the recycled aggregate.
5. The two-step chemically modified recycled aggregate strengthening method according to claim 2, characterized in that: In the reaction, the regenerated aggregate is first soaked in an activator solution at room temperature for 30 minutes to 48 hours, and then the siliceous raw material is added, mixed evenly under mechanical stirring conditions, and then soaked for 30 minutes to 24 hours.
6. The two-step chemically modified recycled aggregate strengthening method according to claim 2, characterized in that: The siliceous raw materials include silica ash, fly ash, silicon dioxide, mineral powder and the like.
Citation Information
Patent Citations
Method for strengthening recycled aggregate
CN115893891A