Tunnel secondary lining concrete material, preparation and application
By optimizing the basalt fiber dosage and concrete matrix material, the compressive, flexural and split strength of tunnel secondary lining concrete is improved, and the problem of low basalt fiber dosage in the prior art is solved, and the strength increase is reduced. Cost has achieved widespread application in tunnel engineering.
Patent Information
- Application Number
- CN202411442698.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing concrete materials with basalt fibers have limited improvements in compressive strength, flexural strength and split strength under the conditions of low basalt fiber doping, and are relatively high in cost, making it difficult to be widely used in actual tunnel engineering. application.
By optimizing the doping amount, length of basalt fibers and the composition of concrete matrix materials, including reasonably setting the doping amount of basalt fibers to 0.09~0.12%, using three-level continuous grade coarse aggregate and appropriate amount of water reducing agent to improve concrete The fluidity and compactness of the tunnel secondary lining concrete material with high compression, flexural and split strength.
The compressive strength, flexural strength and split strength of tunnel secondary lining concrete have been significantly improved, while reducing costs, making its promotion and application in the field of tunnel lining more feasible.
Smart Images

Figure CN118955060A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of concrete, and in particular to tunnel secondary lining concrete materials, preparation and application. Background Art
[0002] Concrete is still the world's largest and most widely used building material, but it has the disadvantages of low tensile strength, high brittleness and easy cracking. Generally speaking, adding fibers to concrete helps to overcome the inherent defects of concrete materials.
[0003] Some current basalt fiber cement-based composite materials are composite materials with cement as the matrix and basalt fiber added to reinforce them. Such basalt fiber cement-based composite materials are expensive, so they are mostly used in theoretical research or in high-performance and special environments, and are not widely used in actual tunnel engineering.
[0004] The existing technology (such as CN111439977A, CN112159168B) has a technical solution of applying basalt fiber to concrete to improve its performance and applying it to related engineering structures. However, the conventional concrete material with basalt fiber has limited improvement in the compressive strength, flexural strength and splitting strength of the concrete material under the condition of low basalt fiber content. Summary of the invention
[0005] The main purpose of the present invention is to provide a tunnel secondary lining concrete, preparation and application, so as to solve the technical problem that the existing concrete materials with basalt fibers have limited improvement in the compressive strength, flexural strength and splitting strength of the concrete materials under the condition of low basalt fiber content.
[0006] To achieve the above-mentioned object, the present invention provides a tunnel secondary lining concrete material, comprising basalt fiber and a concrete matrix material, wherein the concrete matrix material comprises, by mass, 324 to 364 parts of cement, 28 to 32 parts of fly ash, 755 to 775 parts of fine aggregate, 1000 to 1300 parts of coarse aggregate, 150 to 170 parts of water and 5.10 to 5.30 parts of a water reducing agent; wherein the volume of the basalt fiber is 0.09 to 0.12% of the total volume of the concrete matrix material; and the length of the basalt fiber is 12 mm.
[0007] The coarse aggregate includes three grades of continuously graded crushed stone; Among them, the particle size range of the first-grade crushed stone is 4.75-9.5mm, and the apparent density is 2804kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.5%, mud content 0.8%, needle-like content 5.5%; The particle size range of the second-grade crushed stone is 9.5-19mm, and the apparent density is 2796kg / m 3 , Bulk density 1670kg / m 3 , porosity 40.3%, mud content 0.3%, needle-like content 4.5%; The particle size range of the third-grade crushed stone is 19-31.5mm, and the apparent density is 2801kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.8%, mud content 0.3%, needle-like content 5.9%; The mass ratio of the first-stage crushed stone, the second-stage crushed stone and the third-stage crushed stone is 1:3:1.
[0008] According to an implementation manner of the present application, the concrete matrix material includes, by mass, 344 parts of cement, 30 parts of fly ash, 765 parts of fine aggregate, 1100 parts of coarse aggregate, 161 parts of water and 5.23 parts of water reducer; the volume of the basalt fiber is 0.1% of the total volume of the concrete matrix material; the length of the basalt fiber is 12 mm.
[0009] According to the embodiment of the present application, the diameter of the basalt fiber is 16.1 μm and the density is 2650 kg / m 3 , the breaking strength is 1723MPa, the breaking elongation is 2.7%, the elastic modulus is 8100GPa, and the water content is 0.02%.
[0010] According to the embodiment of the present application, the fine aggregate is sand, and the apparent density of the sand is 2784 kg / m 3 , Bulk density 1660kg / m 3 , porosity 40.4%, mud content 0.2%, mud content 1.1%, and fineness modulus 2.88Mx.
[0011] According to the implementation mode of the present application, the particle size of the sand satisfies: the cumulative screening rate under the sieve hole of 4.75 mm is 8.4%, the cumulative screening rate under the sieve hole of 2.36 mm is 28.4%, the cumulative screening rate under the sieve hole of 1.18 mm is 35.8%, the cumulative screening rate under the sieve hole of 0.6 mm is 60.5%, the cumulative screening rate under the sieve hole of 0.3 mm is 82.1%, and the cumulative screening rate under the sieve hole of 0.15 mm is 98.8%.
[0012] The present application also provides a method for preparing the above-mentioned tunnel secondary lining concrete material, comprising the following steps: After the corresponding mass parts of cement, fly ash, fine aggregate and coarse aggregate are uniformly mixed by the first dry mixing, the corresponding volume of basalt fiber is added and uniformly mixed by the second dry mixing; After the mixture is obtained by the second dry mixing, corresponding parts by mass of water and water reducing agent are added, and the mixture is evenly mixed by the third mixing to obtain the tunnel secondary lining concrete material.
[0013] According to an embodiment of the present application, in the first dry mixing step, the mixing time is 28 to 32 seconds.
[0014] In the second dry mixing step, the mixing time is 28 to 32 seconds.
[0015] In the third stirring step, the stirring time is 55 to 65 seconds.
[0016] The present application also provides an application of the above-mentioned tunnel secondary lining concrete material in tunnel secondary lining, including applying the tunnel secondary lining concrete material to form tunnel secondary lining.
[0017] According to the implementation mode of the present application, vibration is further performed after the application, and the vibration duration is 40 seconds.
[0018] In the above-mentioned tunnel secondary lining concrete, the amount and length of basalt fiber are reasonably set, and the type and content of concrete matrix materials, such as the gradation of coarse aggregate and the content of water reducer, are optimized. Under the condition that the basalt fiber content is 0.09~0.12%, the compressive strength, flexural strength and splitting strength of the above-mentioned tunnel secondary lining concrete are significantly improved. And because the tunnel secondary lining concrete includes a relatively large amount of coarse aggregate, compared with basalt fiber cement-based composite materials, the cost is greatly reduced, and it can be promoted and applied in the field of tunnel lining. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0020] Figure 1 is a flow chart of a method for preparing basalt fiber concrete according to one embodiment of the present application; Figure 2 It is a state diagram of concrete without fiber addition according to one embodiment of the present application; Figure 3 This is a state diagram of concrete with 12 mm fiber added according to one embodiment of the present application; Figure 4 This is a physical diagram of the slump of concrete without fiber added according to one embodiment of the present application; Figure 5 This is a physical diagram of the slump of the tunnel secondary lining concrete with a fiber content of 0.3% in one embodiment of the present application; Figure 6 This is a graph of compressive strength of fiber concrete of different lengths at 7 days of age according to an embodiment of the present application; Figure 7 This is a compressive strength diagram of fiber concrete of different lengths at 28 days of age according to an embodiment of the present application; Figure 8 This is a graph of the flexural strength of fiber concrete of different lengths at 7 days of age according to an embodiment of the present application; Fig. 9 This is a graph of the flexural strength of fiber concrete of different lengths at 28 days of age according to one embodiment of the present application; Fig.10 This is a splitting strength diagram of fiber concrete of different lengths at 7 days of age according to an embodiment of the present application; Fig.11 This is a splitting strength diagram of fiber concrete of different lengths at 28 days of age according to one embodiment of the present application.
[0021] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.
[0024] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0025] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0026] The present invention provides a tunnel secondary lining concrete material, comprising basalt fiber and a concrete matrix material, wherein the concrete matrix material comprises, by mass, 324-364 parts of cement, 28-32 parts of fly ash, 755-775 parts of fine aggregate, 1000-1300 parts of coarse aggregate, 150-170 parts of water and 5.10-5.30 parts of a water reducing agent; wherein the volume of the basalt fiber is 0.09-0.12% of the total volume of the concrete matrix material; and the length of the basalt fiber is 12 mm.
[0027] The coarse aggregate includes three grades of continuously graded crushed stone; Among them, the particle size range of the first-grade crushed stone is 4.75-9.5mm, and the apparent density is 2804kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.5%, mud content 0.8%, needle-like content 5.5%; The particle size range of the second-grade crushed stone is 9.5-19mm, and the apparent density is 2796kg / m 3 , Bulk density 1670kg / m 3 , porosity 40.3%, mud content 0.3%, needle-like content 4.5%; The particle size range of the third-grade crushed stone is 19-31.5mm, and the apparent density is 2801kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.8%, mud content 0.3%, needle-like content 5.9%; The mass ratio of the first-stage crushed stone, the second-stage crushed stone and the third-stage crushed stone is 1:3:1.
[0028] It should be noted that the role of the concrete matrix material is mainly to facilitate the description of the composition of various materials in the tunnel secondary lining concrete material, and it is not limited to the tunnel secondary lining concrete material must include a concrete composed of a concrete matrix material, on the basis of which basalt fiber is added.
[0029] Cement is an important component of cementitious materials in concrete. The quality and strength of cement will affect the performance of concrete. In this test, the grade of concrete is C30, and the cement selected is ordinary Portland cement (P•O42.5) produced by Quanjiao Conch Cement Co., Ltd., and there are certain requirements for cement: ①Use 42.5 grade ordinary Portland cement; ② The strength of cement must meet or exceed the standard and the performance indicators of cement must meet the national standards; The composition and performance indicators of cement are shown in Table 1.1.
[0030] Table 1 Cement performance indicators The selection of coarse aggregate is also very important for concrete, because it will directly affect the mechanical properties of concrete. The quality of the coarse aggregate selected for the test is required to comply with the "Standard for Quality and Inspection Methods of Sand and Stone for Ordinary Concrete". It must be clean, with relatively few needle-like particles, and the particle shape should be close to a cube. It must have good particle grading, preferably continuous grading, and on this basis, it must have a low water content. The strength of the coarse aggregate itself must also be higher than that of the concrete.
[0031] The coarse aggregate includes three grades of continuously graded crushed stone. The particle size of the first grade crushed stone ranges from 4.75 to 9.5 mm, and the apparent density is 2804 kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.5%, mud content 0.8%, needle-like content 5.5%. The particle size range of the second-grade crushed stone is 9.5-19mm, and the apparent density is 2796kg / m 3 , Bulk density 1670kg / m 3 , porosity 40.3%, mud content 0.3%, needle-like content 4.5%. The particle size range of the third-grade crushed stone is 19-31.5mm, and the apparent density is 2801kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.8%, mud content 0.3%, needle-like content 5.9%. The mass ratio of the first-grade crushed stone, the second-grade crushed stone and the third-grade crushed stone is 1:3:1.
[0032] Correspondingly, in the concrete matrix material, 1100 parts by mass of crushed stone include 220 parts of first-grade crushed stone, 660 parts of second-grade crushed stone, and 220 parts of third-grade crushed stone. For example, the present application selects the third-grade continuously graded crushed stone of Hexian Hengshan (Hexian Hengshan Mining Co., Ltd.), and its performance indicators are shown in Tables 2 and 3 below.
[0033] Table 2 Coarse aggregate performance indicators Table 3 Coarse aggregate screening results This application studies the specific length of basalt fiber, admixtures, coarse aggregate and other factors, and makes full use of the coordination relationship between the above raw materials. The details are as follows: The tunnel secondary lining concrete material of the present application also includes a water reducing agent. On the one hand, the water reducing agent can increase the fluidity of the concrete, making it difficult for the basalt fibers therein to agglomerate, and evenly mix with the concrete matrix material to form a dense material with low porosity, thereby reducing the impact of the basalt fibers on the fluidity of the concrete and improving the performance of the concrete material in various aspects.
[0034] On the other hand, while maintaining the strength of concrete, water reducers can reduce the amount of cement in concrete, thereby reducing the amount of water used. This helps to improve the durability and impermeability of concrete.
[0035] The tunnel secondary lining concrete material of the present application also optimizes the coarse aggregate. The three-stage continuous grading crushed stone proposed in the present application is conducive to the formation of a uniform and dense structure of concrete. Under the grading of the present application, the fluidity and plasticity of the tunnel secondary lining concrete material are improved, so that the basalt fiber therein is not easy to agglomerate and is evenly mixed with the concrete matrix material, thereby reducing the influence of basalt fiber on fluidity and improving the performance of concrete materials in all aspects.
[0036] Moreover, under this gradation, the porosity in the concrete can be reduced, thereby improving the density and strength of the tunnel secondary lining concrete material.
[0037] After comprehensive consideration and optimization of the above factors, under the condition of basalt fiber dosage of 0.09~0.12%, a tunnel secondary lining concrete material with higher compressive strength, flexural strength and splitting tensile strength was obtained, achieving unexpected beneficial effects.
[0038] In the above-mentioned tunnel secondary lining concrete, the amount and length of basalt fiber are reasonably set, and the type and content of concrete matrix materials, such as the gradation of coarse aggregate and the content of water reducer, are optimized. Under the condition that the basalt fiber content is 0.09~0.12%, the compressive strength, flexural strength and splitting strength of the above-mentioned tunnel secondary lining concrete are significantly improved. And because the tunnel secondary lining concrete includes a relatively large amount of coarse aggregate, compared with basalt fiber cement-based composite materials, the cost is greatly reduced, and it can be promoted and applied in the field of tunnel lining.
[0039] Fine aggregate also plays an important role in concrete. According to the principle of sand and gravel grading, the role of fine aggregates such as sand is to fill the gaps between coarse aggregates such as gravel and pebbles to increase the strength of concrete. Therefore, choosing the right sand (such as river sand) also has an important impact on the test. This test also has a series of standard requirements for sand. First of all, the sand must meet the technical standards, the surface must be clean, and meet the standard requirements. Secondly, the concrete with a C30 ratio must be medium sand, and the modulus coefficient must be controlled between 2.3-3.0, and the sand ratio must also meet the requirements.
[0040] In some embodiments, the river sand in the present application meets the following conditions: its performance indicators are shown in Table 4 and Table 5. The river sand used in the test is from Jiangxi Fujian Sand and Gravel Trading Company.
[0041] Table 4 Performance indexes of fine aggregate Table 5 Fine aggregate screening results Adding admixtures to concrete, without changing the ratio of various raw materials, adding concrete high-efficiency water reducing agent will not change the strength of concrete, and at the same time can greatly improve the rheology and plasticity of concrete. Without changing the ratio of various raw materials (except cement) and the strength of concrete, the amount of cement can be reduced. Adding 0.2%~0.5% of concrete water reducing agent by cement mass can save more than 15~30% of cement. And adding concrete water reducing agent at the same time can increase the life of concrete by more than double. This test uses JSPC-2 admixture from Anhui Jinshi Concrete Admixture Co., Ltd.
[0042] Usually, an appropriate amount of fly ash is added to the concrete mix because fly ash can play an active role in concrete and can make the gap between cement and fly ash smaller. Secondly, it can also play a filling role and increase the structural density.
[0043] The test used Class F II fly ash from Huainan Changhua Electric Power Industry Corporation, and its physical properties are shown in Table 6.
[0044] Table 6 Physical properties of fly ash The fiber added in this test is basalt fiber, which has the following advantages compared to other fibers: the elastic modulus of basalt fiber is also in the same order of magnitude as the elastic modulus of the concrete matrix material, and the two have good deformation coordination ability, and the tensile strength of basalt fiber is at least two orders of magnitude higher than that of the concrete matrix, so it has a higher tensile capacity. In addition, the price of basalt fiber is lower than that of carbon fiber, glass fiber, etc., and its application in concrete engineering has a cost-effective advantage. In particular, basalt fiber itself has no toxic side effects and will not cause any harm to the human body during construction and use, so this test focuses on the effect of basalt fiber on the mechanical properties of concrete.
[0045] In some embodiments, the basalt fiber has a diameter of 16.1 μm and a density of 2650 kg / m 3 , the breaking strength is 1723MPa, the breaking elongation is 2.7%, the elastic modulus is 8100GPa, and the water content is 0.02%.
[0046] For example, the experiment in this application uses basalt fiber produced by Jiangsu Tianlong Basalt Continuous Fiber Co., Ltd., and its physical and mechanical properties are shown in Table 7 below.
[0047] Table 7 Physical and mechanical properties of basalt fiber When preparing basalt fiber concrete, the mix ratio of concrete without fiber is tested many times. However, with the addition of fiber, the fiber will absorb the mixing water inside the concrete. At this time, based on the unchanged mix ratio and water-binder ratio, the amount of admixture used is appropriately changed to ensure the performance of the concrete. The addition of admixture has basically no effect on the strength of concrete, but at the same time, the amount of admixture added must be controlled within an appropriate range to prevent it from bleeding and segregation, which will affect the test data.
[0048] The present application also provides a method for preparing the above-mentioned tunnel secondary lining concrete material, comprising the following steps: After the corresponding mass parts of cement, fly ash, fine aggregate and coarse aggregate are uniformly mixed by the first dry mixing, the corresponding volume of basalt fiber is added and uniformly mixed by the second dry mixing; After the mixture is obtained by the second dry mixing, corresponding parts by mass of water and water reducing agent are added, and the mixture is evenly mixed by the third mixing to obtain the tunnel secondary lining concrete material.
[0049] In some embodiments, in the first dry mixing step, the mixing time is 28 to 32 seconds.
[0050] In the second dry mixing step, the mixing time is 28 to 32 seconds.
[0051] In the third stirring step, the stirring time is 55 to 65 seconds.
[0052] For example, the coarse aggregate, fine aggregate, cement, and fly ash prepared in advance are weighed in turn and poured into the concrete mixer, and then the mixer is started for dry mixing. After 30 seconds of dry mixing, the weighed basalt fiber is evenly sprinkled (the purpose is to prevent uneven distribution of fiber agglomeration), and then dry mixed for another 30 seconds; then water and weighed admixtures are added for full mixing, and the mixing time is 60 seconds. The prepared tunnel secondary lining concrete material is obtained. Specifically, the mixing speed is related to the type of mixer, such as the speed of a self-falling mixer is generally 14-~33r / min; the speed of a forced mixer is generally 20~36r / min, and the speed is not mandatory.
[0053] The applicant adopted other mixing methods in some experiments. Basalt fiber was added after cement, fly ash, fine aggregate and coarse aggregate were evenly mixed, and then water and admixtures were added. At this time, the concrete mixer was already completely wet with water. After the fiber was added and contacted with the aggregate, the fiber could not be fully expanded due to the presence of water, and the fiber might also clump due to the water and could not be evenly distributed.
[0054] The present application also provides an application of the above-mentioned tunnel secondary lining concrete material in tunnel secondary lining, including applying the tunnel secondary lining concrete material to form tunnel secondary lining.
[0055] The composite lining structure of the mountain tunnel based on the basalt fiber concrete mainly includes eight types: S5a, S5b, S5c, S4a, S4b, S4c, S3a, and S3b. Different types of lining structures are selected according to the different geological conditions of the tunnel.
[0056] The S5a lining is mainly used for the shallow buried section of the tunnel entrance and the structural fracture zone that has a greater impact on the stability of the tunnel body. The S5a lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 26cm thick C25 shotcrete, Steel mesh (single layer with spacing of 20cm×20cm), 20a I-beam (vertical spacing of 60cm). The reserved deformation is a reserved deformation with a thickness of 12cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 45cm thick basalt fiber reinforced concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 50cm thick C30 reinforced concrete secondary lining.
[0057] The S5b lining is mainly used for shallow buried sections of tunnels with grade V surrounding rock, deep buried soft rock sections and local structural fracture zones with little impact on tunnel stability. The S5b lining mainly includes initial support, reserved deformation, waterproof layer and secondary lining along the radial direction of the tunnel from outside to inside. The initial support mainly includes 24cm thick C25 shotcrete, Steel mesh (single layer with spacing of 20cm×20cm), 18 I-beam (vertical spacing of 75cm). The reserved deformation is a reserved deformation with a thickness of 10cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing coil. The secondary lining is 45cm thick basalt fiber reinforced concrete.
[0058] The S5c lining is mainly used for the deep buried hard rock section of the tunnel body with grade V surrounding rock. The S5c lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 24cm thick C25 shotcrete, Steel mesh (single layer with spacing of 20cm×20cm), 18 I-beam (vertical spacing of 80cm). The reserved deformation is a reserved deformation with a thickness of 10cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 40cm thick basalt fiber reinforced concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 45cm thick C30 reinforced concrete secondary lining.
[0059] The S4a lining is mainly used for the shallow buried section of the tunnel entrance and the broken zone of the tunnel body. The S4a lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 22cm thick C25 shotcrete, Steel mesh (single layer with spacing of 25cm×25cm), 16 I-beams (vertical spacing of 100cm). The reserved deformation is a reserved deformation with a thickness of 8cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 35cm thick basalt fiber concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 40cm thick C30 cast concrete.
[0060] The S4b lining is mainly used for deep buried soft rock sections of tunnels with Class IV surrounding rock. The S4b lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 20cm thick C25 shotcrete, Steel mesh (single layer with spacing of 25cm×25cm), 14 I-beams (vertical spacing of 100cm). The reserved deformation is a reserved deformation with a thickness of 7cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 35cm thick basalt fiber concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 40cm thick C30 cast concrete.
[0061] The S4c lining is mainly used for deep buried hard rock sections of tunnels with Class IV surrounding rock. The S4c lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 20cm thick C25 shotcrete, Steel mesh (single layer with spacing of 25cm×25cm), 14 I-beams (vertical spacing of 120cm). The reserved deformation is a reserved deformation with a thickness of 7cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 35cm thick basalt fiber concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 40cm thick C30 cast concrete.
[0062] The S3a lining is mainly used for reinforcing the lining within 10m before and after the emergency parking zone of Class III surrounding rock. It is also used in the actual construction process for Class III surrounding rock with obvious layered structure. The surrounding rock strength and hardness are relatively high, but some sections have long-distance vertical joints and fissures in the arch, and there is a high risk of potential block falling and small collapse. The S3a lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 20cm thick C25 shotcrete, Steel mesh (single layer with spacing of 25cm×25cm), grid steel arch frame (vertical distance of 120cm). The reserved deformation is a reserved deformation with a thickness of 5cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 30cm thick basalt fiber concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 35cm thick C30 cast concrete.
[0063] The S3b lining is mainly used in general areas of Grade III surrounding rock. The S3b lining mainly includes initial support, reserved deformation, waterproof layer, and secondary lining along the radial direction of the tunnel from the outside to the inside. The initial support mainly includes 10cm thick C25 shotcrete, Steel mesh (single layer with spacing of 25cm×25cm). The reserved deformation is a reserved deformation with a thickness of 5cm set along the circumferential direction of the tunnel. The waterproof layer mainly includes 400g / m 2 Non-woven fabric, 1.5mm thick EVA waterproofing membrane. The secondary lining is 30cm thick basalt fiber concrete, which saves concrete usage and improves the lining's crack resistance and durability compared to the traditional 35cm thick C30 cast concrete.
[0064] The composite lining structure of the tunnel described in this application is based on the principle of the New Austrian Tunneling Method. The initial support consists of system anchors, single-layer steel mesh, shotcrete, and I-beam steel arch frames (if any), combined with advance reinforcement measures such as pipe sheds, double-layer small ducts or advanced small ducts as auxiliary construction measures. The secondary lining adopts molded basalt fiber reinforced concrete, and a waterproof layer is laid between the initial support and the secondary lining. The support parameters can be adjusted appropriately according to the measurement information. During the construction process, the principles of "pipe advance, strict slurry injection, short advance, weak blasting, strong support, early ring formation, and frequent measurement" should be strictly followed, and the process should be strictly controlled to ensure construction safety and structural stability.
[0065] In some embodiments, vibration is further performed after the application, and the vibration duration is 40 seconds.
[0066] In the process of making the test piece, pour out the mold after stirring. After the mold is completed, put the mold on the vibration table and vibrate for 40 seconds (the best time selected after many tests). Finally, put the surface and put it in the curing room at a temperature of 20±2℃ and a relative humidity of about 95%. The curing period is 7d and 28d respectively.
[0067] Preferably, a vibration table is used for vibration. The effect of manual tamping is not as good as that of a vibration table. There will be a large number of bubbles in the concrete specimens produced by manual vibration, which seriously affects the strength of the concrete specimens. The reason for this phenomenon is that fibers are added to the concrete. The fibers are bonded to the concrete, which increases the resistance to vibration and also produces certain gaps, resulting in many bubbles in the concrete that have not been discharged after vibration. This makes it impossible for the concrete to bond well with each other, thereby affecting the strength of the concrete.
[0068] The technical solution of the present application is described below in conjunction with specific embodiments.
[0069] Example 1 According to Table 8, multiple groups of concrete are configured. The specific preparation method includes: the coarse aggregate, fine aggregate, sand, cement, and fly ash prepared in advance are weighed in sequence and poured into the concrete mixer, and then the mixer is started for dry mixing. After 30 seconds of dry mixing, the weighed basalt fiber is evenly sprinkled (the purpose is to prevent the fiber from clumping and uneven distribution), and then dry mixing is continued for 30 seconds; then water and weighed admixtures are added for full mixing, and the mixing time is 60 seconds. After mixing, pour out the mold. After the mold is filled, put the mold on the vibration table and vibrate for 40 seconds (the best time selected after many tests). Finally, the surface is smoothed and put into the curing room. The temperature is 20±2℃ and the relative humidity is about 95%. The ages are 7d and 28d respectively for curing. Among them, B1-12 is the mix ratio of this application and meets the tunnel secondary lining concrete material ratio of this application.
[0070] Table 8 Basalt fiber concrete mix ratio Note: B0 means no basalt fiber, B1-12 means fiber content is 0.1%, length is 12mm, and so on.
[0071] Each group of concrete and the resulting specimens were tested.
[0072] Slump Slump is a method and index for determining the workability of concrete. On construction sites and in laboratories, slump tests are usually performed to determine the fluidity of the mixture, and to assess cohesion and water retention by intuitive experience. Slump is a quantitative index to measure the degree of concrete workability, and is used to determine whether construction can proceed normally.
[0073] Fluidity is an important indicator for evaluating the working performance of concrete. The test is mainly carried out with reference to the method of "Standard for Test Methods of Ordinary Concrete Mixture Performance" (GB / T 50080-2002). The test sample is fresh basalt fiber concrete. The test steps are as follows: (1) To prevent the instruments from taking away some of the moisture in the concrete, the inner wall of the slump cone and other tools should be wetted with a damp cloth before testing. The cone should be placed on a moist and non-absorbent steel plate, and the pedals on both sides of the cone should be stepped on to prevent the cone from moving during loading.
[0074] (2) Load the material in layers according to 1 / 3 of the height of the cylinder. Use a tamping rod to tamp each layer evenly from the outside to the inside along the spiral direction 25 times. The tamping rod should penetrate the layer. When tamping along the edge of the cylinder, the tamping rod should be slightly tilted inward. After the last layer is filled and tamped, let the concrete slightly protrude from the cylinder mouth, then scrape it off with a spatula and smooth it.
[0075] (3) After clearing the concrete from the side of the cone, lift the slump cone vertically and steadily within 5 to 10 seconds. The whole process from loading to lifting the cone should be completed within 150 seconds.
[0076] (4) Measure the distance between the highest point of the concrete mixture and the cylinder height after collapse, which is the slump value of the concrete mixture, in millimeters. Slump tests were conducted on fiber concrete with different dosages. The slump test results are shown in Table 3.9: Table 9 Slump results of basalt fiber concrete Note: B0 means no basalt fiber, B1-12 means fiber content is 0.1%, length is 12mm, and so on.
[0077] See also Figure 2 and 3 The state of fiber concrete and the state of concrete without fiber are as follows Figure 2 and Figure 3 As shown. As can be seen from Table 9, the addition of fiber has a significant effect on the slump of concrete. As the fiber content increases, the slump of the concrete gradually decreases. The reason is that the gradual addition of fiber into concrete will cause some fibers to be mixed unevenly, clump together, and entangled together, which will hinder the flow of concrete aggregate; at the same time, when basalt fiber is added to the mixture, it is immediately stirred and dispersed into extremely fine flocculent fiber filaments, and part of the cement slurry that originally wrapped the aggregate is transferred to wrap the fiber filaments. A certain amount of mixing water will be absorbed between the fiber cement slurry, resulting in poor fluidity of the concrete. The slump of concrete without fiber reaches 190mm. Figure 4 As shown in the figure, the higher the dosage, the greater the impact on the slump of concrete. Based on the comprehensive test results, the dosage of about 0.1% is the most appropriate. With this dosage, after the concrete is formed and hardened, the surface is smooth, and the fiber distribution is not very obvious to the naked eye; when the dosage is 0.3%, the surface of the molded specimen is rough, and a few fibers can be clearly seen on the surface. The slump reaches 170mm. Figure 5 shown.
[0078] Compressive strength test The concrete compressive strength test was based on the “Standard for Test of Mechanical Properties of Ordinary Concrete” (GB / T50081-2002), and the specimens used were 150mm×150mm×150mm.
[0079] The test was conducted using a digital press with a maximum load of approximately 2000kN. The test steps are as follows: (1) Take out the test piece from the curing room and clean the test piece and the upper and lower pressure plates of the testing machine; (2) The center of the specimen is aligned with the center of the lower pressure plate of the testing machine, and the side of the specimen when it is formed is used as the pressure-bearing surface. Start the testing machine. When the upper pressure plate approaches the specimen, adjust the ball seat so that the specimen and the upper pressure plate are in balanced contact; (3) Apply load continuously and evenly at a loading speed of 0.5-0.8 MPa / s. When the specimen is close to failure, stop adjusting the throttle until the specimen fails. Record the maximum load with an accuracy of 0.1 MPa.
[0080] (4) Calculation of compressive strength of concrete cube: Where: f cu —Concrete cube compressive strength (MPa) F —Ultimate compressive load (N) A —Test piece pressure area (mm²) This test studied the compressive strength of basalt fiber concrete specimens at different ages of 7d and 28d with fiber content of 0.1%, 0.2%, 0.3% and length of 12mm, 18mm, 24mm. The test data are as follows.
[0081] Table 10 Compressive strength of basalt fiber concrete at different ages It can be seen from Table 10 that the addition of basalt fiber has a significant improvement on the compressive strength of concrete. The changes in concrete strength for different dosages and different lengths of fibers are also different. From the table, we can see that when the fiber volume dosage is 0.1%, the concrete strength improvement is higher than other dosages, and also higher than concrete without fiber. When the fiber length is 12mm and the volume dosage is 0.1%, the performance is optimal. The compressive strength of 7d and 28d reached 38.35MPa and 47.01MPa, respectively, an increase of 11% and 16%. However, as the fiber dosage increases, the three lengths of fibers do not significantly improve the compressive strength of concrete and even show a downward trend. It can be seen that an appropriate amount of fiber can enhance the compressive strength, while excessive fiber will be counterproductive.
[0082] from Figure 6 and Figure 7 It can be seen that the fiber concrete with a volumetric dosage of 0.1% and a length of 12 mm has the highest strength, which is higher than other dosages. The fiber with a length of 12 mm is shorter and easier to disperse. It can be intuitively seen that the dispersion is the best among the three fibers during mixing. Basalt fiber can improve the strength of concrete because an appropriate amount of fiber is evenly mixed into the concrete. After being dispersed by mixing, the internal strength of the matrix is still in the growth stage in the early stage of concrete forming. The fiber can be connected between the matrix and can hinder the development of cracks under the action of external force, thereby improving the early strength. However, when the fiber is excessive, there will be a large number of unevenly dispersed fibers, and there is no bonding force between these fibers. They cannot resist large loads in the early stage of concrete hydration. Therefore, when the volume dosage is 0.2%~0.3%, the strength of fiber concrete is much lower than that of ordinary concrete. This is because as the fiber dosage increases, its agglomeration phenomenon becomes more serious, which reduces the effective contact area between the fiber and the concrete, thereby increasing the internal pores and reducing the compressive strength of the concrete.
[0083] In the concrete compression test, it can be found that when the specimen without fiber reaches the cracking load, some vertical cracks will appear at the four corners of the specimen. After continuing to bear the load, the cracks will develop into cracks and expand the gaps between them, accompanied by slight peeling of concrete on the surface. When the load continues to increase, the cracks continue to develop and a small amount of concrete blocks fall off.
[0084] The number of cracks in the concrete specimens mixed with basalt fibers is significantly reduced compared to ordinary concrete, with only a small amount of concrete peeling and a small amount of vertical cracks on the edge of the specimens. The extent of the cracks is not as large as that of ordinary concrete specimens because the fibers are distributed in three dimensions in the concrete specimens, which can effectively reduce the stress concentration at the tips of the microcracks and limit the development of the cracks. When the load continues to increase, the cracks on the specimens will gradually develop inward, and some of the fibers dispersed in the matrix are just located between the cracks, effectively transmitting the force from the cracks and delaying the destruction of the concrete.
[0085] Bending tensile strength test The concrete compressive strength test was based on the “Test Standard for Mechanical Properties of Ordinary Concrete” (GB / T50081-2002), and the specimens used were 150mm×150mm×550mm.
[0086] The test was conducted using a universal testing machine with a maximum load of 300kN. The test steps are as follows: (1) After taking out the test piece from the curing room, clean it and inspect its appearance. There should be no obvious defects on the test piece; (2) The side surface of the specimen during molding shall be used as the pressure-bearing surface. The deviation of all installation dimensions shall not exceed 1 mm. The contact surface between the support and the pressure-bearing surface and the cylinder shall be smooth and uniform, otherwise it shall be leveled; (3) Start the testing machine and load evenly at a loading speed of 0.05-0.08 MPa / s. When the specimen is close to failure, stop adjusting the throttle until the specimen fails. Record the failure load and the fracture position of the lower edge of the specimen. The flexural strength should be accurate to 0.01 MPa.
[0087] The flexural strength formula of concrete specimens is: Where: —Concrete flexural strength (MPa) F—Specimen failure load (N) L—span between supports (mm) b,h—specimen section width and height (mm) This part of the test also studied the compressive strength of basalt fiber concrete specimens at different ages of 7d and 28d with fiber content of 0.1%, 0.2%, 0.3% and length of 12mm, 18mm, 24mm respectively. The test data are as follows.
[0088] Table 11 Flexural strength of basalt fiber concrete at different ages From the data in Table 11, it can be seen that the addition of basalt fiber has a significant improvement on the flexural strength of concrete. From the chart, we can see that with the increase of age, the improvement of strength by fiber becomes more and more obvious. At 28 days, 0.1%~0.3% fiber basically improves the flexural strength of concrete, which is better than the strength at 7 days. At the same time, we can also know that when the volume content is 0.1%, the improvement of concrete flexural strength is better than 0.2%, 0.3% and the strength of concrete without fiber. When the volume content is 0.1% and the fiber length is 12mm, the flexural strength of this ratio is the largest, the strength at 7 days is increased by 28%, and the effect is the best at 28 days. With the increase of fiber volume content, there are more uneven dispersion of internal fibers after stirring, which leads to weakened bonding with the matrix and a decrease in overall bending strength.
[0089] from Figure 8 and Fig. 9It can be further understood that the addition of fiber does enhance the flexural strength of concrete. From the figure, we can first intuitively see that the volume content of 0.1% shows higher strength than other content, especially the basalt fiber with a length of 12mm and a volume content of 0.1%, which shows the highest flexural strength, much higher than other content. Moreover, as the fiber content increases, the 7d and 28d flexural strengths also decrease, and are even lower than the strength without adding fiber.
[0090] The fiber itself has toughness. In concrete, it can not only improve the mechanical properties of concrete, but also significantly improve the plastic deformation capacity of the concrete matrix. In the flexural test, basalt fiber concrete is significantly different from ordinary concrete in terms of the crack development rate and fracture morphology. In the flexural strength test, when the specimen is subjected to the load and reaches the point of cracking, the initial crack will appear in the tensile part of the specimen between the two concentrated loads, and cracks will appear in the middle area at the bottom of each specimen. As the load continues to increase, the cracks will soon extend to the upper part of the specimen after they appear, causing the specimen to break into two parts. The time from the appearance of the crack to the splitting of the concrete without fiber is very short, and the fracture is mostly straight.
[0091] Under the action of load, the crack development speed of basalt fiber concrete is obviously slower than that of ordinary concrete, which delays the time for the specimen to split and increases the ultimate load that the specimen can withstand. Since basalt fibers are distributed in three-dimensional random directions inside the concrete matrix, when cracks develop in the bending specimen, the fibers in the middle of the cracks play a bridging role and bear a certain tensile stress. The presence of fibers will inhibit the development of cracks. Even if the fibers are broken by force, when the load continues to increase, the stress inside the specimen is redistributed, and the addition of fibers changes the extension path of the cracks and delays the destruction of the concrete. Therefore, the fracture position of basalt fiber concrete is generally not straight, and has a certain concave and convex section.
[0092] That is, the failure morphology of the specimens without fiber or with insufficient fiber content is brittle fracture, and the failure morphology of the specimens with reasonable fiber content is ductile fracture. Generally speaking, brittle fracture is sudden, the fracture surface is straight, and the stress-strain curve of the material shows a steep drop when the material is damaged; ductile fracture is slow, and there are certain signs before the fracture, such as the appearance of many fine cracks, the fracture surface of the specimen is mostly fine serrated, and the stress-strain curve of the material shows a slow drop when the material is damaged.
[0093] 3.3.5 Splitting strength test The method of “Test Standard for Mechanical Properties of Ordinary Concrete” (GB / T50081-2002) was adopted, and the specimens used were 150mm×150mm×150mm.
[0094] The instrument used in the test is the same universal testing machine as the flexural test. The test steps are as follows: (1) After the specimen is taken out, clean the surface and the upper and lower pressure plates of the testing machine. Draw the cleavage surface position line perpendicular to the top surface in the middle of the side surface of the specimen when it is formed; (2) The specimen is placed in a standard fixture. A wooden pad is added between the upper and lower arc-shaped steel pads and the specimen. The center lines of the pads and the splitting surface of the specimen are aligned. The whole is placed at the center of the lower pressure plate of the testing machine.
[0095] (3) Start the testing machine and load evenly at a loading speed of 0.05-0.08 MPa / s. When the specimen is close to failure, stop adjusting the throttle until the specimen fails and record the failure load.
[0096] (4) Splitting tensile strength formula: — Splitting tensile strength of concrete cube specimens F—Specimen failure load (N) A—Split surface area of specimen (mm2) The test studied the splitting strength of basalt fiber concrete specimens at different ages of 7d and 28d with fiber content of 0.1%, 0.2%, 0.3% and length of 6mm, 12mm, 18mm, 24mm. The splitting strength of specimens at different ages is as follows: Table 12 Splitting strength of basalt fiber concrete at different ages From Table 12, we can see that the addition of fiber also has a certain effect on the splitting strength of concrete. Like compression and flexural strength, the concrete has the best performance when the addition amount is 0.1%. The splitting strength is the best when the fiber length is 12mm and the addition amount is 0.1%, reaching 3.46MPa and 3.70MPa at 7d and 28d respectively, which is much higher than the strength without fiber. When the fiber addition amount is 0.2%, the strength at 7d is still improved, but when the addition amount is increased to 0.3%, the splitting strength of concrete is not only reduced without fiber addition.
[0097] from Fig.10 and Fig.11As we know, the splitting strength of concrete increases first and then decreases. The fiber strength of 0.1% dosage is still higher than other dosages, and the trend remains the same. The splitting strength of the fiber length of 12mm and the dosage of 0.1% is the best among these proportions. Compared with the case without adding fibers, the improvement rate is higher than 14%, and then the dosage increases. Regardless of the length of the fiber, the splitting strength is decreasing, and even lower than the strength without adding fibers. The downward trend of splitting strength is because after the fiber is excessive, the fiber agglomeration phenomenon becomes more serious, and the micropores between the fibers cause the bonding force between the internal cement binder to decrease. The pores and holes in the middle of the matrix increase. When the dosage is 0.1%, the internal pores and holes are relatively small, while when the dosage is 0.3%, the internal pores and holes increase. When testing the splitting strength, the pad applies an external force to the middle of the specimen, the pores increase, and the load capacity weakens. Therefore, the larger the dosage, the lower the splitting strength of the concrete.
[0098] With the increase of fiber content, the splitting strength decreases because after the fiber is excessive, the fiber agglomeration phenomenon becomes more serious, and the micropores between the fibers cause the bonding force between the internal cement binder to decrease. The pores and holes in the middle of the matrix increase. When the content is 0.1%, the internal pores and holes are relatively small. When the content is 0.2%, the internal pores and holes increase. When testing the splitting strength, the pad applies an external force to the middle of the specimen, the pores increase, and the load capacity weakens. Therefore, the larger the content, the lower the splitting strength of the concrete.
[0099] In the splitting test, longitudinal cracks will appear at the upper and lower wooden pads at the beginning of the load application. As the load increases, the cracks gradually develop and penetrate along the middle of the specimen. When the specimen reaches the ultimate load, the specimen is split into two halves. The process from cracks to cracks and then to splitting is very fast. Ordinary concrete is directly split into two halves under the action of the ultimate load. Concrete mixed with basalt fiber will delay the formation of initial cracks in the specimen, and when the internal cracks develop, the fibers bear part of the tensile stress. When the cracks develop, the force can be transmitted to both sides through the fibers between the cracks, delaying the destruction time of the concrete, and when the ultimate load is reached, the destruction morphology is more complete than that of ordinary concrete. If there are more fibers that can transmit force between the two sides of the crack, the improvement of concrete will be more obvious.
[0100] Based on this experimental study and result analysis, the following conclusions were obtained: (1) The gradual addition of basalt fiber to concrete will affect the fluidity of concrete to a certain extent. As the fiber content increases, the fluidity of the three basalt fiber concrete mixtures with different lengths and diameters gradually decreases, and the slump gradually decreases. Taking the fiber length of 12 mm as an example, the fluidity of the concrete with 0.3% fiber content is much lower than that of the concrete without fiber, and the concrete with fiber has almost no fluidity. The larger the fiber content and the longer the length, the greater the loss of fluidity, and the slump gradually decreases.
[0101] (2) Basalt fiber significantly improves the compressive strength of concrete. The optimal volume content is 0.1%. When the volume content is 0.1%, the compressive strength of concrete is improved by the three different lengths of fibers. Among them, when the volume content is 0.1%, the fiber with a length of 12 mm has the best compressive strength for concrete. However, as the content increases and the fiber length becomes longer, the strength of basalt fiber concrete will decrease to a certain extent, and even be lower than the strength of concrete without fiber.
[0102] (3) Similarly, the addition of basalt fiber also significantly improves the flexural strength of concrete. When the fiber content is 0.1% and the length is 12 mm, the flexural strength of concrete is the best, which is much higher than the strength of concrete without fiber. When the fiber content exceeds 0.2%, the flexural strength of basalt fiber concrete decreases significantly, which is lower than the strength without fiber.
[0103] (4) The splitting strength of basalt fiber concrete also changes with the addition of fibers. When the fiber content is 0.1% and 0.2%, the splitting strength of concrete is also significantly improved, especially when the content is 0.1%, the improvement rate is the highest, which is higher than the strength of concrete without fiber. At the same 0.1% content, the splitting strength of the 12mm length reaches the maximum value. However, when the fiber content reaches 0.3%, the splitting strength of all fiber concrete is lower than the strength without fiber.
[0104] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the protection scope of the present invention.
Claims
1. A tunnel secondary lining concrete material, characterized in that: It comprises basalt fiber and concrete matrix material, wherein the concrete matrix material comprises, by weight, 324-364 parts of cement, 28-32 parts of fly ash, 755-775 parts of fine aggregate, 1000-1300 parts of coarse aggregate, 150-170 parts of water and 5.10-5.30 parts of water reducing agent; wherein the volume of the basalt fiber is 0.09-0.12% of the total volume of the concrete matrix material; and the length of the basalt fiber is 12 mm; The coarse aggregate includes three grades of continuously graded crushed stone; Among them, the particle size range of the first-grade crushed stone is 4.75-9.5mm, and the apparent density is 2804kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.5%, mud content 0.8%, needle-like content 5.5%; The particle size range of the second-grade crushed stone is 9.5-19mm, and the apparent density is 2796kg / m 3 , Bulk density 1670kg / m 3 , porosity 40.3%, mud content 0.3%, needle-like content 4.5%; The particle size range of the third-grade crushed stone is 19-31.5mm, and the apparent density is 2801kg / m 3 , Bulk density 1630kg / m 3 , porosity 41.8%, mud content 0.3%, needle-like content 5.9%; The mass ratio of the first-stage crushed stone, the second-stage crushed stone and the third-stage crushed stone is 1:3:
1.
2. The tunnel secondary lining concrete material according to claim 1, characterized in that: The concrete matrix material includes, by mass, 344 parts of cement, 30 parts of fly ash, 765 parts of fine aggregate, 1100 parts of coarse aggregate, 161 parts of water and 5.23 parts of water reducing agent; the volume of the basalt fiber is 0.1% of the total volume of the concrete matrix material; and the length of the basalt fiber is 12 mm.
3. The tunnel secondary lining concrete material according to claim 1, characterized in that: The diameter of the basalt fiber is 16.1 μm and the density is 2650 kg / m 3 , the breaking strength is 1723MPa, the breaking elongation is 2.7%, the elastic modulus is 8100GPa, and the water content is 0.02%.
4. The tunnel secondary lining concrete material according to claim 1, characterized in that: The fine aggregate is sand, and the apparent density of the sand is 2784 kg / m 3 , Bulk density 1660kg / m 3 , porosity 40.4%, mud content 0.2%, mud content 1.1%, and fineness modulus 2.88Mx.
5. The tunnel secondary lining concrete material according to claim 4, characterized in that: The particle size of the sand satisfies: the cumulative residue rate at the sieve hole of 4.75 mm is 8.4%, the cumulative residue rate at the sieve hole of 2.36 mm is 28.4%, the cumulative residue rate at the sieve hole of 1.18 mm is 35.8%, the cumulative residue rate at the sieve hole of 0.6 mm is 60.5%, the cumulative residue rate at the sieve hole of 0.3 mm is 82.1%, and the cumulative residue rate at the sieve hole of 0.15 mm is 98.8%.
6. A method for preparing a tunnel secondary lining concrete material according to any one of claims 1 to 5, characterized in that: The following steps are involved: After the corresponding mass parts of cement, fly ash, fine aggregate and coarse aggregate are uniformly mixed by the first dry mixing, the corresponding volume of basalt fiber is added and uniformly mixed by the second dry mixing; After the mixture is obtained by the second dry mixing, water and a water reducing agent in corresponding parts by mass are added, and the mixture is evenly mixed through the third mixing treatment to obtain a tunnel secondary lining concrete material.
7. The preparation method according to claim 6, characterized in that: In the first dry mixing step, the mixing time is 28 to 32 seconds; In the second dry mixing step, the mixing time is 28 to 32 seconds; In the third stirring step, the stirring time is 55 to 65 seconds.
8. Use of the tunnel secondary lining concrete material according to any one of claims 1 to 5 in tunnel secondary lining, characterized in that: The method comprises applying the tunnel secondary lining concrete material to form the tunnel secondary lining.
9. The use according to claim 8, characterized in that: After the application, vibration is also performed, and the vibration time is 40 seconds.
Citation Information
Patent Citations
Tunnel sprayed concrete and preparation method thereof
CN110590258A
Method for preventing and treating large deformation of tunnel soft rock by adopting basalt fiber concrete
CN118030128A
Basalt fiber reinforced excavation material aggregate concrete and preparation method thereof
CN118145938A
Arch wall lining structure suitable for hidden hole of mountain tunnel and construction method
CN118601615A
Concrete composition for tunnel lining
KR1020090036952A
Cited By
Soft rock tunnel backfill area mass concrete pouring method
CN120906591A