Carboxylated block type nano-microsphere as well as preparation method and application thereof
Through the preparation method of carboxylated block nano microspheres, the problems of low light transmittance and low antibody coupling efficiency are solved, high light transmittance and high efficiency coupling are achieved, and latex enhancement immunity is enhanced Detection effect of turbidity reagent.
Patent Information
- Application Number
- CN202411316972.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-15
AI Technical Summary
The existing polystyrene nano microspheres have low light transmittance in in vitro detection reagents, which is difficult to meet the needs of reagent sensitivity and linear detection range at the same time. The coupling efficiency of antibodies and nano microspheres is low, which affects the latex-enhanced immune turbidity reagents. Development.
The preparation method of carboxylated block nano microspheres is adopted to initiate polymerization reaction through esterification, Fuke acylation and light irradiation, carboxylic active groups are introduced, the monomer ratio and photosensitive initiator dosage are adjusted, and excellent permeability is prepared. Nanomicrospheres with photoelectric and high carboxylic active group content were purified using heterogeneous wettable glass fiber separation membrane.
It improves the light transmittance and stability of nano microspheres, enhances the content of carboxylic active groups on the surface of nano microspheres, improves the efficiency of antibody coupling, and improves the detection effect of latex-enhanced immune turbidity reagent.
Smart Images

Figure CN118955783A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of immunoturbidimetric biochemical detection, in particular to carboxylation block type nano microspheres and a preparation method and application thereof. Background Art
[0002] In the field of immunodiagnosis, latex microspheres are closely related to the research and development of latex-enhanced immunoturbidimetric reagents. Modern scientific research has synthesized latex microspheres through different methods, such as emulsion polymerization, dispersion polymerization, suspension polymerization, solvent evaporation, etc., to prepare latex microspheres of different particle size ranges. At present, the materials used to prepare latex microspheres are mostly copolymers of polystyrene or its homologues. At the same time, with the advancement of modern science and technology, nano-microspheres with shell-core structures have gradually entered the field of vision of in vitro detection reagent developers. However, due to the limitations of the material of polystyrene nano-microspheres themselves, the transmittance is low, and nano-microspheres with the same particle size are difficult to meet the requirements of reagent sensitivity and linear detection range in the development of in vitro detection reagents. Therefore, it is necessary to continuously develop new polymerization monomers, or use different monomers to prepare nano-microspheres with special structures, such as nano-microspheres with shell-core structures.
[0003] In addition to the constraints of nano-microsphere materials on the development of latex-enhanced immunoturbidimetric reagents, the coupling efficiency of antibodies and nano-microspheres is another difficulty that affects the development of latex-enhanced immunoturbidimetric reagents. Due to the special structure of antibodies, modern research divides the binding between antibodies and nano-microspheres into two aspects: physical adsorption and chemical coupling. Physical adsorption is mainly because polystyrene nano-microspheres are hydrophobic microspheres that can adsorb and coordinate with proteins with hydrophobic groups, but hydrophobic adsorption is limited to hydrophobic microspheres. The interaction of chemical coupling is stronger than physical adsorption. Generally, the surface of nano-microspheres is modified to have active groups such as carboxyl, amino, and sulfonic acid groups on the surface. Generally, carboxyl groups are the most commonly used. By using EDC / NHS to activate latex microspheres, it can react chemically with the free primary amine at the Fc end of the antibody, so that the antibody can bind to the surface of the nano-microspheres in the correct direction. The binding of antibodies to nano-microspheres is related to the concentration of antibodies and the number of carboxyl active groups on the surface of nano-microspheres.
[0004] At present, the main methods for chemically modifying the surface of nanoparticles are: (1) synthesizing functional monomers with active groups and using them as preparation monomers to polymerize and generate surface functionalized nanoparticles; (2) using traditional methods to use monomers such as styrene to prepare nanoparticles and then chemically modifying their surfaces to introduce designed functional groups on the surface of the microspheres through special chemical reactions, such as: using benzene rings, using special functional groups, or for highly cross-linked polystyrene microspheres, using the residual pendant ethylene double bonds on the surface of the microspheres; (3) before the polymerization reaction, adding some monomers with functional groups to the polymerizing monomers to participate in the polymerization, thereby introducing specific functional groups on the surface of the nanoparticles. Although these three methods can prepare modified nano-microspheres with active groups on the surface, method (1) requires the preparation of monomers with functional groups in advance, and the preparation process is complicated. There are difficulties such as the stability of the prepared monomers is questionable and the polymerization conditions are difficult to control. Method (2) has certain requirements for latex microspheres and related chemical groups, and the reaction is difficult and the reaction conditions are harsh. Method (3) is relatively simple, but a large number of active groups will be embedded in the nano-microspheres, and the number of active functional groups exposed on the surface of the nano-microspheres is small and difficult to control accurately. Summary of the invention
[0005] In order to solve the problems of the prior art, the purpose of the present invention is to overcome the shortcomings of the prior art and provide carboxylated block nano-microspheres and a preparation method and application thereof.
[0006] One of the purposes of the present invention is to provide a method for preparing a carboxylated block nanosphere, comprising the following steps:
[0007] S1, performing an esterification reaction, and obtaining an ester compound after extraction;
[0008] S2, performing Friedel-Crafts acylation and ester condensation reaction, and obtaining a hydroxyalkyl phenone free radical photosensitive initiator after extraction;
[0009] S3, performing a photo-induced polymerization reaction to obtain an intermediate product;
[0010] S4, heating to initiate a polymerization reaction to obtain a product system;
[0011] S5, extracting the carboxylated block nanospheres in the product system;
[0012] in,
[0013] The reactants of the esterification reaction include a first catalyst, a hydroxyalkyl compound, and an organic polyacid;
[0014] The reactants of the Friedel-Crafts acylation and ester condensation reaction include the ester compound, an aldehyde substance and a second catalyst;
[0015] The reactants of the light-induced polymerization reaction include the photosensitive initiator, the dispersant and the first monomer;
[0016] The reactants for the heat-initiated polymerization reaction include the intermediate product, an emulsifier, a redox initiator, a third catalyst and a second monomer.
[0017] Preferably, the first monomer is one or more of acrylic acid, oleic acid, methyl methacrylate, acrylamide, vinyl naphthalene, and rosin acrylate, and the second monomer is one or more of styrene, 1,2-diphenylethylene, styrene sulfonyl chloride, and divinylbenzene.
[0018] In some preferred embodiments, the first monomer is methyl methacrylate, and the second monomer is styrene.
[0019] Preferably, the esterification reaction step in S1 is: adding the first catalyst, the hydroxyalkyl compound, and the organic polyacid into the first organic solution, heating the solution at a constant temperature for reaction, and then evaporating, concentrating, and filtering under reduced pressure to obtain the ester compound.
[0020] Further preferably, the parameters of the constant temperature heating reaction in S1 are: keeping warm at a temperature of 55 to 65° C. for 25 to 35 minutes.
[0021] In some preferred embodiments, the parameters of the constant temperature heating reaction in S1 are: keeping warm at 60° C. for 30 minutes.
[0022] Preferably, the first catalyst is selected from one or more of N,N-dicyclohexylcarbodiimide, 4-methylaminopyridine, and 4-arylpyridine.
[0023] In some preferred embodiments, the first catalyst is selected from N,N-dicyclohexylcarbodiimide and 4-methylaminopyridine.
[0024] In some more preferred embodiments, the first catalyst is selected from N,N-dicyclohexylcarbodiimide and 4-methylaminopyridine in a mass ratio of 1:1.
[0025] Preferably, the molar ratio of the hydroxyalkyl compound to the aldehyde substance is (1-2):1.
[0026] Preferably, the hydroxyalkyl compound is trimethylolpropane.
[0027] Preferably, the mass ratio of the first catalyst to the hydroxyalkyl compound is 0.5% to 1%.
[0028] In some preferred embodiments, the mass ratio of the first catalyst to the hydroxyalkyl compound is 1%.
[0029] Preferably, the organic polyacid is selected from one or more of 2,3-dihydroxysuccinic acid, 3-carboxy-3-hydroxyglutaric acid, and succinic acid.
[0030] In some preferred embodiments, the organic polyacid is succinic acid.
[0031] Preferably, the first organic solution is methanol.
[0032] Preferably, the step of the Friedel-Crafts acylation and ester condensation reaction in S2 is: dissolving the ester compound and the aldehyde substance in a second organic solution, and carrying out a catalytic reaction under a weak alkaline environment and the action of a second catalyst, and then separating and purifying to obtain the photosensitive initiator.
[0033] Preferably, the aldehyde substance is p-hydroxymethylbenzaldehyde.
[0034] Preferably, the second organic solution is acetonitrile.
[0035] Preferably, the weak alkaline environment has a pH of 8.0 to 8.5.
[0036] Preferably, the second catalyst is zinc, titanium tetrachloride and lithium aluminum hydride.
[0037] Preferably, the mass ratio of the second catalyst to the aldehyde substance is 1% to 2%.
[0038] In some preferred embodiments, the mass ratio of the substances in the second catalyst is: zinc: titanium tetrachloride: lithium aluminum hydride = 1:2:2.
[0039] In some preferred embodiments, the mass ratio of the second catalyst to the aldehyde substance is 2%.
[0040] In some preferred embodiments, the photosensitive initiator has the structural formula:
[0041]
[0042] Preferably, the step of light-induced polymerization reaction in S3 is: the photosensitive initiator, dispersant and first monomer are mixed in a third organic solution to obtain a mixed solution containing the first monomer, and the mixed solution is irradiated under ultraviolet light to cause free radical cleavage of the photosensitive initiator, thereby initiating a free radical polymerization reaction of the first monomer.
[0043] Further preferably, the photosensitive initiator and the dispersant are first dissolved in a third organic solution to prepare a second solution, and after the solution is completely dissolved, the first monomer is added to obtain the mixed solution containing the first monomer.
[0044] Furthermore, the second solution is heated and stirred at 35-45° C. and 70-140 rpm to accelerate dissolution. After the second solution is completely dissolved, the first monomer is added and the heating and stirring are maintained until the light-induced polymerization reaction is completed.
[0045] In some preferred embodiments, the second solution is heated and stirred at 35-45° C. and 75-85 rpm to accelerate dissolution.
[0046] In some more preferred embodiments, the second solution is heated and stirred at 40°C and 80 rpm to accelerate dissolution. Preferably, the conditions for the light-induced polymerization reaction are: the irradiation light is: ultraviolet light with a wavelength of 300-350 nm, and the irradiation time is 5-8 hours.
[0047] In some preferred embodiments, the conditions for the light-induced polymerization reaction are: the irradiation light is ultraviolet light with a wavelength of 350 nm, and the irradiation time is 6-8 hours.
[0048] In some preferred embodiments, nitrogen is continuously introduced during the photo-induced polymerization reaction.
[0049] In some more preferred embodiments, the light-induced polymerization reaction further includes: stirring the mixed solution containing the first monomer at 35-45° C. and 90-110 rpm.
[0050] Preferably, the dispersant is selected from one or more of sodium styrene sulfonate, polyvinyl pyrrolidone, and polyvinyl alcohol;
[0051] In some preferred embodiments, the dispersant is polyvinyl pyrrolidone and sodium styrene sulfonate.
[0052] Preferably, the step of heating to initiate the polymerization reaction in S4 is: mixing the intermediate product, the emulsifier, the redox initiator and the third catalyst to obtain a third solution, and then adding the second monomer to the third solution.
[0053] More preferably, the third solution is heated and stirred at 45-55° C. and 95-105 rpm to accelerate dissolution.
[0054] In some preferred embodiments, the third solution is heated and stirred at 50° C. and 100 rpm to accelerate dissolution.
[0055] Preferably, the conditions for the heating-initiated polymerization reaction are: reaction temperature of 50-70° C., stirring speed of 150-200 rpm, and reaction time of 8-14 h.
[0056] In some preferred embodiments, the conditions for the heating-initiated polymerization reaction are: reaction temperature of 50-70° C., stirring speed of 150-200 rpm, and reaction time of 10-14 h.
[0057] In some preferred embodiments, nitrogen is continuously introduced during the heating-induced polymerization reaction.
[0058] Preferably, the emulsifier is selected from one or more of sodium lauryl sulfate, sodium alkylnaphthalene sulfonate, polyvinyl alcohol, steareth-21, PEG-100 stearate, sorbitan tristearate, N-dodecyldimethylamine, calcium dodecylbenzenesulfonate, and glyceryl monostearate.
[0059] In some preferred embodiments, the emulsifier is sodium dodecyl sulfate.
[0060] Preferably, the redox initiator is selected from one or more of benzoyl peroxide-sucrose, tert-butyl hydroperoxide-rongalite, tert-butyl hydroperoxide-sodium metabisulfite, sodium persulfate-ferrous sulfate, hydrogen peroxide-ferrous sulfate, benzoyl peroxide-N,N-diethylaniline, benzoyl peroxide-ferrous pyrophosphate, potassium persulfate-ferrous chloride.
[0061] In some preferred embodiments, the redox initiator is potassium persulfate-ferrous chloride.
[0062] Preferably, the third catalyst is selected from one or more of 2,2,6,6-tetramethylpiperidine-1-oxide, titanium zinc cyanine polyarylether nitrile, dicyanobenzene derivatives, bipyridine ruthenium, and cerium ethanol complex.
[0063] In some preferred embodiments, the third catalyst is titanium zinc cyanine poly (arylene ether nitrile).
[0064] In some preferred embodiments, the dispersant is polyvinyl pyrrolidone and sodium styrene sulfonate in a mass ratio of 5:1.
[0065] In some preferred embodiments, the third organic solution is an alcohol-water solution.
[0066] In some more preferred embodiments, the alcohol aqueous solution is a mixed solution of methanol and pure water.
[0067] In some more preferred embodiments, the alcohol aqueous solution is a mixed solution of methanol and pure water in a volume ratio of 2:1.
[0068] Preferably, the mass ratio of the photosensitive initiator to the first monomer is: (0.2-0.8):(10-20).
[0069] Preferably, the ratio of the mass of the emulsifier and the redox initiator to the mass of the second monomer is: (0.4-1):(10-30).
[0070] Preferably, the mass ratio of the first monomer to the second monomer is (1-2):(1-3).
[0071] In some preferred embodiments, the dosage ratio of the photosensitive initiator to the third organic solution is: (0.2-0.8) g:70 mL.
[0072] In some preferred embodiments, the mass ratio of the photosensitive initiator to the dispersant is: (2-8):3.
[0073] In some more preferred embodiments, the mass ratio of the photosensitive initiator to the dispersant is: (4-8):3.
[0074] Preferably, the mass ratio of the photosensitive initiator, the first monomer, the emulsifier, the redox initiator, the third catalyst and the second monomer is: (0.2-0.8):(10-20):(0.2-0.5):(0.2-0.6):(0.2-0.4):(10-30).
[0075] In some preferred embodiments, the mass ratio of the photosensitive initiator, the first monomer, the emulsifier, the redox initiator, the third catalyst and the second monomer is: (0.4-0.8):(10-20):(0.2-0.5):(0.2-0.5):(0.2-0.4):(10-20).
[0076] Preferably, the extraction in S5 is to obtain a precipitate by centrifuging the product system, and then drying the precipitate.
[0077] In some preferred embodiments, the carboxylated segmented nanospheres are extracted by multiple centrifugation followed by drying, that is, the precipitate after centrifugation is resuspended in ultrapure water and centrifuged once or multiple times to obtain a cleaner precipitate, which is then dried.
[0078] In some more preferred embodiments, the drying temperature is 50°C.
[0079] Further preferably, the extracted carboxylated block nanospheres are purified, and the purification process comprises: resuspending the carboxylated block nanospheres with ultrapure water, filtering with a heterogeneous wettability glass fiber separation membrane, and then drying.
[0080] The second object of the present invention is to provide a carboxylated block nanosphere prepared by the above-mentioned preparation method of carboxylated block nanosphere.
[0081] Preferably, the content of surface carboxyl active groups of the carboxylated segmented nanospheres is between 0.2 and 1.0 mmol / g.
[0082] Preferably, the particle size of the carboxylated segmented nanospheres is 50 to 500 nm.
[0083] In some preferred embodiments, the particle size of the carboxylated segmented nanospheres is 50-300 nm.
[0084] The third object of the present invention is to provide the application of the above-mentioned carboxylated segmented nano-microspheres, wherein the nano-microspheres are used for preparing latex enhanced immunoturbidimetric reagents.
[0085] Compared with the prior art, the present invention has the following beneficial effects:
[0086] First, the present invention provides a unique hydroxyalkyl phenone photosensitive initiator, and uses the photosensitive initiator to initiate a free radical polymerization reaction of a first monomer (such as methyl methacrylate monomer, etc.) under ultraviolet light irradiation, and uses styrene and methyl methacrylate as monomers to carry out a polymerization reaction to generate block polymer nanospheres, and nanospheres with excellent light transmittance are prepared by adjusting the usage ratio of styrene monomer and methyl methacrylate monomer.
[0087] Secondly, the hydroxyalkyl phenone photosensitive initiator introduced in the preparation of the carboxylated block nanospheres of the present invention can also serve as a donor of carboxyl active groups. Due to the special structure of the block polymer, the compound with the carboxyl group will be located at the interface of the block polymer, and after being polymerized into a spherical shape, it will be located on the surface of the nanospheres, and will be introduced into the surface of the nanospheres in a stable, effective and controllable manner.
[0088] Third, the present invention provides a method for preparing carboxylated block nanospheres, which adjusts the usage ratio of the first monomer and the second monomer to prepare nanospheres suitable for detection items with different light transmittance requirements; and controls the amount of carboxyl active groups on the surface of the nanospheres by controlling the usage of the photosensitive initiator.
[0089] Fourth, the carboxyl-block nano-microspheres provided by the present invention, by introducing a sufficient number of carboxyl groups on the surface of the nano-microspheres, enhance the ionic atmosphere on the surface of the nano-microspheres, thereby increasing the Zeta potential on the surface of the nano-microspheres, and improving the electrostatic stability of the nano-microspheres; and due to the increase in the number of carboxyl active groups on the surface of the nano-microspheres, the coupling efficiency of the downstream nano-microspheres and antibodies is improved, that is, when the nano-microspheres and antibodies are adsorbed to detect antigens, the number of antibodies that can be adsorbed is more, and the efficiency during detection is also higher; by the same token, it can be inferred that when the nano-microspheres and antigens are adsorbed to detect antibodies, the number of antigens that can be adsorbed is more, and the detection efficiency is improved due to the larger number of carboxyl active groups. In other words, the carboxyl-block nano-microspheres provided by the present invention, when applied to latex-enhanced immunoturbidimetric reagents, can further improve the detection effect of in vitro detection reagents.
[0090] Fifth, emulsion polymerization is the most commonly used method for preparing nano-microspheres in industry, but when using emulsion polymerization to prepare nano-microspheres, some emulsifiers will remain on the surface of the latex microspheres, and it is difficult to completely remove them through subsequent cleaning steps. The present invention purifies the obtained nano-microspheres by creatively using a heterogeneous wettability glass fiber separation membrane. The heterogeneous wettability glass fiber separation membrane consists of a strongly hydrophilic SB region and a weakly hydrophilic SiO2 / PVA region. The two regions have different affinities for water and oil, and the diffusion and penetration rates of hydrophilic substances in the two regions are significantly different. Compared with the weakly hydrophilic region component SiO2 / PVA, the hydrophilic molecules in the strongly hydrophilic SB region will have a more obvious wetting and spreading rate. When the nano-microspheres prepared by the emulsion polymerization method pass through this interface, the hydrophilic surfactant adsorbed on the surface of the nano-microspheres will be captured by the hydrophilic SB region, so that the hydrophilic emulsifier remaining on the surface of the nano-microspheres is adsorbed in the hydrophilic SB region, and the hydrophobic latex microspheres are captured and aggregated by the weakly hydrophilic region to achieve separation, thereby obtaining nano-microspheres with high neatness and good optical properties, eliminating the influence of the residual emulsifier on the surface of the nano-microspheres on the coupling efficiency of the downstream microspheres and antibodies, so as to further improve the coupling efficiency of the carboxylated block nano-microspheres and antibodies. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] Figure 1 The SEM image (a) and particle size distribution diagram (b) of the carboxylated block nanospheres prepared in Example 7 of the present invention;
[0092] Figure 2 The SEM image (a) and particle size distribution diagram (b) of the carboxylated segmented nanospheres prepared in Example 8 of the present invention;
[0093] Figure 3 The SEM image (a) and particle size distribution diagram (b) of the carboxylated segmented nanospheres prepared in Example 9 of the present invention;
[0094] Figure 4 The SEM image (a) and particle size distribution diagram (b) of the carboxylated segmented nanospheres prepared in Example 5 of the present invention;
[0095] Figure 5 The standard curve is drawn by using the BCA kit in the present invention with the standard protein concentration and the measured absorbance. DETAILED DESCRIPTION
[0096] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0097] First, this specific embodiment provides a method for preparing carboxylated segmented nanospheres, the steps are:
[0098] S1, using a first catalyst to catalyze an esterification reaction between trimethylolpropane and an organic polyacid to generate an ester compound;
[0099] S2, adding the ester compound obtained in step S1, aldehydes and a strong base substance into an organic solvent, and then adding a second catalyst to carry out a catalytic reaction, so as to cause Friedel-Crafts acylation and ester condensation reactions, and obtaining a photosensitive initiator after separation and purification;
[0100] S3, mixing the photosensitive initiator, dispersant and first monomer obtained in step S2, and performing a light-induced polymerization reaction to induce a free radical polymerization reaction of the first monomer to obtain an intermediate product;
[0101] S4, adding an emulsifier, a redox initiator, a third catalyst and a second monomer to the intermediate product, heating and initiating a polymerization reaction, to obtain a product mixture containing carboxylated block nanospheres;
[0102] S5. Extracting the solid matter from the product mixture to obtain carboxylated block nanospheres, which may also be called polystyrene-polymethyl methacrylate block nanospheres.
[0103] The following is a detailed introduction to the preparation method of carboxylated segmented nanospheres through examples.
[0104] Example 1
[0105] This embodiment introduces a method for preparing carboxylated segmented nanospheres, wherein:
[0106] The specific steps of the esterification reaction in S1 are:
[0107] The first catalyst, trimethylolpropane and organic polyacid are added to the first organic solution, and the mixture is heated at a constant temperature for reaction, and then evaporated, concentrated and filtered under reduced pressure to obtain an ester compound, wherein:
[0108] The first catalyst is N, N-dicyclohexylcarbodiimide DCC (dosage is 0.025g) and 4-methylaminopyridine (dosage is 0.025g), trimethylolpropane (dosage is 5g), the organic polyacid is succinic acid (dosage is 3g), the first organic solution is pure methanol (dosage is 10mL), the reaction conditions are 60℃ water bath heating reaction for 30min, esterification reaction occurs to generate succinic acid-(2-methyl), (2-hydroxymethyl)-propylene glycol, and then evaporation concentration and reduced pressure filtration are carried out in sequence to obtain ester compound succinic acid-(2-methyl), (2-hydroxymethyl)-propylene glycol solid product, the reaction formula is as follows:
[0109]
[0110] The specific steps of the reaction of Friedel-Crafts acylation and ester condensation in S2 are:
[0111] The ester compound and aldehyde substance prepared in S1 are dissolved in a second organic solution, and catalytically reacted under a weak alkaline environment and the action of a second catalyst, and then separated and purified to obtain a photosensitive initiator, wherein:
[0112] The amount of ester compound is 1g, the aldehyde is p-hydroxymethylbenzaldehyde (the amount is 1g), the second organic solution is pure acetonitrile (the amount is 10mL), the pH of the reaction system is adjusted to the range of 8.0 to 8.5 by adding a strong base substance, the second catalyst is zinc (the amount is 0.004g), titanium tetrachloride (the amount is 0.008g) and lithium aluminum hydride (the amount is 0.008g), the catalytic reaction is 20min, and the separation and purification is carried out by evaporation concentration recrystallization. The obtained photosensitive initiator is a hydroxyalkyl phenone photosensitive initiator, and the reaction formula is as follows:
[0113]
[0114] The aldehyde group of p-hydroxymethylbenzaldehyde undergoes electron transfer under alkaline conditions, and the carbon to which the aldehyde group belongs is transformed from electrically neutral to a carbon anion, and under the catalytic action of the combined catalyst, it attacks the ester bond to produce a β-hydroxydicarbonyl nine-membered ring intermediate. This intermediate has poor stability. Under the continuous attack of the carbon anion, electron rearrangement occurs, the ring breaks and recombine to form a stable carbonyl compound.
[0115] In this embodiment, potassium hydroxide (dosage: 0.05 g) is used as the strong alkaline substance.
[0116] In order to make the reaction more complete, the ester compound, aldehydes and strong alkaline substances are added to the second organic solution to obtain a first solution. After the first solution is mixed evenly, the second catalyst is added.
[0117] The specific steps of the light-induced polymerization reaction in S3 are:
[0118] The photosensitive initiator, dispersant and first monomer prepared in S2 are mixed in a third organic solution, and the photosensitive initiator is subjected to free radical cleavage under ultraviolet light, thereby initiating a free radical polymerization reaction of the first monomer, wherein the free radical cleavage reaction formula of the photosensitive initiator is as follows:
[0119]
[0120] Specifically, the dosage of each reaction substance is: the dosage of the photosensitive initiator is 0.2g, the dispersant is polyvinylpyrrolidone PVP (the dosage is 0.25g) and sodium styrene sulfonate (the dosage is 0.05g), the third organic solution is an alcohol aqueous solution (the dosage is 70mL), and the first monomer is methyl methacrylate monomer (the dosage is 10g).
[0121] In this embodiment, the alcohol aqueous solution uses a solvent system composed of methanol and water in a volume ratio of 2:1. Specifically, the conditions for the light-induced polymerization reaction are: irradiation with 350nm wavelength ultraviolet light for 6 hours, continuous nitrogen flow during the illumination period, and continuous stirring at 40°C and 100rpm, so that the photosensitive initiator undergoes free radical cleavage and then initiates free radical polymerization of the methyl methacrylate monomer to obtain an intermediate product.
[0122] In order to make the reaction more complete, the photosensitive initiator and the dispersant are dissolved in an alcohol aqueous solution to prepare a second solution, and the first monomer is added after the solution is completely dissolved.
[0123] In order to accelerate the dissolution rate of the second solution, the second solution was heated and stirred at 40° C. and 80 rpm.
[0124] In S4, the specific steps of heating to initiate the polymerization reaction are:
[0125] The intermediate product prepared in S3, the emulsifier, the redox initiator, and the third catalyst are mixed to obtain a third solution, and the second monomer is added to the third solution, wherein:
[0126] The emulsifier is sodium dodecyl sulfate (dosage 0.2g), the redox initiator is potassium persulfate-ferrous chloride system (the mass ratio of potassium persulfate and ferrous chloride is 2:1, and the total dosage is 0.2g), the third catalyst is titanium zinc cyanine polyarylether nitrile (dosage 0.2g), and the second monomer is styrene monomer (dosage 10g).
[0127] The conditions for the heat-initiated polymerization reaction are as follows: nitrogen is continuously introduced during the reaction, and the reaction is carried out at 50° C. and 150 rpm with continuous stirring for 10 hours to obtain a product mixture.
[0128] In this embodiment, the emulsifier, the redox initiator and the third catalyst are first mixed to obtain a third solution, the dissolution of the third solution is accelerated under stirring conditions of 50° C. and 100 rpm, and then the second monomer is added to the completely dissolved third solution.
[0129] It is worth noting that in the experiment of preparing nano-microspheres by emulsion polymerization, the role of the redox initiator is to initiate the polymerization reaction. However, since sodium persulfate itself has a strong initiation effect, using it alone will make the initiation rate too fast and cause uneven particle size of the nano-microspheres. Therefore, ferrous chloride is used to limit the initiation rate, not to use sodium persulfate to react with ferrous chloride.
[0130] The extraction method of carboxylated block nanospheres in S5 is the following three steps:
[0131] S5-1. Separate the solid from the liquid to obtain a precipitate.
[0132] The solid-liquid separation was performed by multiple centrifugation to obtain a precipitate. Specifically, after centrifugation at 4°C and 10,000 rpm for 15 min, the precipitate was resuspended in 10 mL of ultrapure water and centrifuged again, and the resuspension and centrifugation operations were repeated twice.
[0133] In this embodiment, the resuspended mixed solution is also subjected to ultrasonic treatment, the ultrasonic power is 300 W, and the ultrasonic time is 2 min.
[0134] S5-2. Purification
[0135] First, the precipitate obtained from S5-1 was resuspended in 10 mL of ultrapure water, and then the resuspended liquid was purified by nanospheres using a heterogeneous wettability glass fiber separation membrane, so that the hydrophilic emulsifier remaining on the surface of the nanospheres could be separated from the nanospheres, thereby achieving the purpose of removing the residual emulsifier on the surface of the nanospheres.
[0136] The heterogeneous wettability glass fiber separation membrane in this example was purchased from Maiborui Biomembrane Technology Co., Ltd., with the product number MSGFF100300N.
[0137] S5-3, drying to obtain carboxylated block nanoparticles.
[0138] In this embodiment, the purified nanospheres obtained in S5-2 are dried in an oven at 50°C.
[0139] The carboxylated block nanospheres prepared in this example have a particle size distribution in the range of about 200 to 250 nm.
[0140] It should be noted that the dried carboxylated block nanospheres were stored by resuspending in 30 mM phosphate buffer at pH 7.2-7.4 and sonicating in an ice-water bath for 2 min to completely disperse them, wherein the mass dispersion of the carboxylated block nanospheres was 10 wt.%.
[0141] The power of ultrasound in the ice water bath was 300 W, and the ultrasound time was 2 min.
[0142] Example 2
[0143] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 1, except that:
[0144] The amount of the third catalyst used was 0.4 g, and the amount of the second monomer used was 20 g.
[0145] The carboxylated block nanospheres prepared in this example have a particle size distribution in the range of about 200 to 250 nm.
[0146] Example 3
[0147] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 1, except that:
[0148] The amount of the third catalyst used was 0.6 g, and the amount of the second monomer used was 30 g.
[0149] The carboxylated block nanospheres prepared in this example have a particle size distribution in the range of about 200 to 250 nm.
[0150] Example 4
[0151] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 1, except that:
[0152] The amount of photosensitive initiator used was 0.3 g.
[0153] The carboxylated block nanospheres prepared in this example have a particle size distribution in the range of about 200 to 250 nm.
[0154] Example 5
[0155] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 1, except that:
[0156] The amount of photosensitive initiator used was 0.4 g.
[0157] The carboxylated block nanospheres prepared in this example have a particle size distribution of about 200 to 250 nm. The SEM image and particle size distribution diagram are shown in FIG. Figure 4 shown.
[0158] Example 6
[0159] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 1, except that:
[0160] The amount of photosensitive initiator used is 0.5g.
[0161] The carboxylated block nanospheres prepared in this example have a particle size distribution in the range of about 200 to 250 nm.
[0162] Example 7
[0163] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 1, except that:
[0164] The amount of photosensitive initiator is 0.8g, the amount of the first monomer is 20g, the amount of emulsifier is 0.5g, the total amount of redox initiator is 0.5g, the amount of the third catalyst is 0.4g, the amount of the second monomer is 20g,
[0165] In S3, the conditions for the light-induced polymerization reaction are: irradiation with ultraviolet light of 350 nm wavelength for 8 h, continuous nitrogen flow during the irradiation period, and continuous stirring at 50° C. and 150 rpm;
[0166] In S4, the conditions for the heating-initiated polymerization reaction are: nitrogen is continuously introduced during the reaction, and the reaction is maintained at 70° C. and stirred at 200 rpm for 14 hours to obtain a product mixture.
[0167] The carboxylated block nanospheres prepared in this example have a particle size distribution of about 50 to 100 nm. The SEM image and particle size distribution diagram are shown in FIG. Figure 1 shown.
[0168] Example 8
[0169] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 7, except that:
[0170] The amount of emulsifier used was 0.4 g, and the total amount of redox initiator used was 0.4 g;
[0171] In S3, the conditions for the light-induced polymerization reaction are: irradiation with ultraviolet light of 350 nm wavelength for 8 h, continuous nitrogen flow during the irradiation period, and continuous stirring at 50° C. and 120 rpm;
[0172] In S4, the conditions for the heating-initiated polymerization reaction are: nitrogen is continuously introduced during the reaction, and the reaction is maintained at 70° C. and 180 rpm with continuous stirring for 14 hours to obtain a product mixture.
[0173] The carboxylated block nanospheres prepared in this example have a particle size distribution of about 100 to 150 nm. The SEM image and particle size distribution diagram are shown in FIG. Figure 2 shown.
[0174] Example 9
[0175] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 7, except that:
[0176] The amount of photosensitive initiator is 0.6 g, the amount of the first monomer is 15 g, the amount of emulsifier is 0.3 g, the total amount of redox initiator is 0.3 g, the amount of the third catalyst is 0.3 g, and the amount of the second monomer is 15 g;
[0177] In S3, the conditions for the light-induced polymerization reaction are: irradiation with ultraviolet light of 350 nm wavelength for 8 h, continuous nitrogen flow during the irradiation period, and continuous stirring at 40° C. and 100 rpm;
[0178] In S4, the conditions for the heating-initiated polymerization reaction are: nitrogen is continuously introduced during the reaction, and the reaction is maintained at 60° C. and 180 rpm with continuous stirring for 14 hours to obtain a product mixture.
[0179] The carboxylated block nanospheres prepared in this example have a particle size distribution of about 150 to 200 nm. The SEM image and particle size distribution diagram are shown in FIG. Figure 3 shown.
[0180] Example 10
[0181] This example introduces a method for preparing carboxylated block nanospheres, and the steps are basically the same as those in Example 5, except that:
[0182] There is no S5-2 step in S5.
[0183] In this example, unpurified carboxylated block nanospheres were obtained, and the particle size distribution was approximately in the range of 200 to 250 nm.
[0184] Embodiment 11
[0185] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 2, except that:
[0186] There is no S5-2 step in S5.
[0187] In this example, unpurified carboxylated block nanospheres were obtained, and the particle size distribution was approximately in the range of 200 to 250 nm.
[0188] Example 12
[0189] This example introduces a method for preparing carboxylated block nanospheres, and the steps are basically the same as those in Example 3, except that:
[0190] There is no S5-2 step in S5.
[0191] In this example, unpurified carboxylated block nanospheres were obtained, and the particle size distribution was approximately in the range of 200 to 250 nm.
[0192] Embodiment 13
[0193] This example introduces a method for preparing carboxylated segmented nanospheres, and the steps are basically the same as those in Example 8, except that:
[0194] The amount of the photosensitive initiator is 0.4g;
[0195] There is no S5-2 step in S5.
[0196] In this example, unpurified carboxylated block nanospheres were obtained, and the particle size distribution was about 100-150 nm.
[0197] Comparative Example 1
[0198] Carboxylated polystyrene nanospheres with a particle size distribution range of 50-100 nm were purchased from Beijing Boerma Biotechnology Co., Ltd.
[0199] Comparative Example 2
[0200] Carboxylated polystyrene nanospheres with a particle size distribution range of 100-150 nm were purchased from Beijing Boerma Biotechnology Co., Ltd.
[0201] Comparative Example 3
[0202] Carboxylated polystyrene nanospheres with a particle size distribution range of 150-200 nm were purchased from Beijing Boerma Biotechnology Co., Ltd.
[0203] Comparative Example 4
[0204] Carboxylated polystyrene nanospheres with a particle size distribution range of 200-250 nm were purchased from Beijing Boerma Biotechnology Co., Ltd.
[0205] The test analysis of the above-mentioned embodiments and comparative examples is introduced below, which is as follows:
[0206] 1. Morphology and particle size
[0207] The electron microscope images and particle size distribution test results of the nano-microspheres prepared in Examples 5 and 7 to 9 are shown in FIG. Figures 1 to 4 As shown, it can be seen that the prepared nanoparticles are spherical with uniform morphology.
[0208] 2. Transmittance
[0209] The transmittance of the carboxylated segmented nanospheres obtained in Examples 1-3, 5, 10-12 and the nanospheres of Comparative Example 4 was determined using a 722S spectrophotometer (Shanghai Lingguang Technology Co., Ltd.) according to the following experimental steps. Each sample was measured 3 times, the average value was calculated, and the transmittance of the nanospheres was evaluated.
[0210] (1) Turn on the power of 722S spectrophotometer (Shanghai Lingguang Technology Co., Ltd.), preheat the instrument for 20 minutes, and enter the setting interface after the self-test is completed;
[0211] (2) Select the wavelength to be set to 290nm and save the setting parameters;
[0212] (3) Wash the quartz cuvette three times with pure water and wipe it clean with a clean paper towel;
[0213] (4) Calibration: Place the quartz cuvette in the spectrophotometer after shielding it with a light shield, and set the transmittance at this time to 0.0%. Then, add 1 ml of ultrapure water to the quartz cuvette and place it in the spectrophotometer, and set the transmittance at this time to 100.0%.
[0214] (5) After calibration, the transmittance of the sample nanospheres was measured. 0.5 g of nanospheres were suspended in 5 ml of pure water. After resuspending and mixing in an ice-water bath ultrasound (300 W power, ultrasound for 2 min), 1 ml of the emulsion sample was taken out for transmittance testing. Each sample was tested three times.
[0215] The test results are shown in Table 1, and it can be seen that:
[0216] Comparative analysis of Examples 1 to 5, Example 10 and Comparative Example 4 revealed that the light transmittance of the carboxylated segmented nanospheres prepared by the present invention was superior to the light transmittance of the commercially available carboxylated polystyrene nanospheres of the same particle size;
[0217] By comparing and analyzing Examples 1 to 3, it was found that the transmittance of the nano-microspheres prepared by the present invention is related to the usage ratio of the first monomer and the second monomer in the preparation process, and decreases with the increase of the usage ratio of the two monomers. In subsequent applications, the usage ratio of styrene and methyl methacrylate monomers in the segmented nano-microspheres can be changed according to the requirements of the in vitro detection reagent project of latex enhanced immunoturbidimetry to prepare nano-microspheres with adapted transmittance.
[0218] Comparative analysis of Example 2 and Example 11, Example 3 and Example 12, and Example 5 and Example 10 revealed that the use of a heterogeneous wettability glass fiber separation membrane to separate and purify the nanosphere product can improve the light transmittance of the nanosphere product.
[0219] Table 1 Test results of light transmittance of nano-microspheres in Examples and Comparative Examples
[0220]
[0221] 2. Carboxyl active group content
[0222] The carboxyl active group content on the surface of the carboxyl block nanospheres prepared in Examples 1 and 4 to 9 and the carboxyl polystyrene nanospheres purchased in Comparative Examples 1 to 4 was determined by chemical titration with reference to the following experimental steps. The reagents used were methanol, 0.1% phenolphthalein indicator, and 0.05 mol / L KOH standard solution. The test steps were:
[0223] (1) Weigh 0.5 g of nanospheres into a 50 ml conical flask, add 10 ml of methanol, and disperse them in an ice-water bath with ultrasonic waves (300 W power, 3 min);
[0224] (2) Use a rubber-tipped dropper to add 2 drops of 0.1% phenolphthalein indicator into the conical flask;
[0225] (3) Titrate with 0.05 mol / L KOH standard solution until the solution turns light pink (does not fade within 15-30 seconds). Measure the pH value of the solution at this time with a pH meter = 8.5, which is the reaction endpoint;
[0226] (4) Use the same method to titrate the blank methanol reagent (titrate to pH = 8.5 reaction endpoint);
[0227] (5) According to the formula Calculate the content of carboxyl active groups on the surface of nanospheres of each sample, where V and V 0are the volumes of KOH standard solution consumed in sample titration and blank methanol titration respectively (in ml), c is the concentration of KOH standard solution (in mol / L), m is the mass of nanosphere sample (in g), and ACOOH is the content of carboxyl active groups on the surface of nanosphere (in mmol / g).
[0228] The test results of the carboxyl active group content of the nano-microspheres prepared under different photosensitive initiator dosages are shown in Table 2, and it can be seen that:
[0229] The content of carboxyl active groups on the surface of the carboxylated segmented nano-microspheres with a particle size range of 200-250 nm prepared by the present invention is related to the amount of the photosensitive initiator used during preparation. The content of the carboxyl active groups increases with the increase in the amount of the photosensitive initiator used, and there is a maximum value of the carboxyl active group content within the particle size range, that is, within the particle size range of 200-250 nm, when the mass ratio of the photosensitive initiator to the first monomer is 4:100, the content of the carboxyl active groups on the surface of the nano-microspheres prepared by the present invention is the highest, and further increasing the amount of the photosensitive initiator used cannot significantly increase the content of the carboxyl active groups on the surface of the nano-microspheres.
[0230] Table 2 Surface carboxyl active group content of nanoparticles in Examples and Comparative Examples
[0231]
[0232] The test results of the content of carboxyl active groups on the surface of nano-microspheres with different particle sizes are shown in Table 3. It can be seen that:
[0233] Comparative analysis of Example 5 and Examples 7 to 9 revealed that the content of carboxyl active groups introduced into the small-particle nano-microspheres prepared by the present invention is higher than that introduced into the large-particle nano-microspheres. This is due to the differences in the concentration of the polymerization monomer, the concentration of the photosensitive initiator in the reaction system, and the polymerization conditions.
[0234] Comparative analysis was performed within the same particle size range, namely: Example 1, Example 3 and Comparative Example 4, Example 7 and Comparative Example 1, Example 8 and Comparative Example 2, Example 9 and Comparative Example 3. It was found that within the same particle size range, the content of carboxyl active groups on the surface of the nano-microspheres prepared by the present invention was 1.4-3.5 times higher than that of commercially available nano-microspheres, indicating that the polystyrene-polymethyl methacrylate block nano-microspheres prepared by the preparation method of carboxylated block nano-microspheres provided by the present invention can increase the content of carboxyl active groups on the surface of the nano-microspheres.
[0235] Table 3 Content of carboxyl active groups on the surface of nanoparticles with different particle sizes
[0236]
[0237] 3. Stability
[0238] Charged particles adsorb particles of opposite charge in the dispersion system, and the ions on the surface of the particles are strongly bound, while the ions farther away form a relatively loose electron cloud. The potential difference between the inside and outside of the electron cloud is the Zeta potential. Zeta potential is an important indicator for characterizing the stability of the dispersion system. Zeta potential (unit mV) of the carboxylated block nanospheres prepared in Example 3, Example 7-9 and the nanospheres of Comparative Examples 1-4 was measured using a Zeta potential analyzer (Shanghai Powerchip Scientific Instrument Co., Ltd.) with reference to the following experimental steps and the average value was calculated.
[0239] (1) Turn on the power: let it stand for 30 minutes, and then turn on the computer to perform a self-check on the instrument;
[0240] (2) Establish the measurement procedure: select the material name and the dispersed medium (water), set the measurement temperature to 4°C, measure each sample 3 times, set the sample volume to 1 ml, and measure the sample after the settings are completed;
[0241] (3) Accurately weigh 0.5 g of nanospheres and resuspend them in 5 ml of deionized water and mix them evenly by ultrasonication for 10 min. Take out 1 ml to measure the Zeta potential.
[0242] The measurement results are shown in Table 4, and it can be seen that:
[0243] The Zeta potential of the nano-microspheres prepared by the present invention is higher than that of the commercially available nano-microspheres, indicating that the sample prepared by the preparation method of the carboxylated block nano-microspheres provided by the present invention has higher stability;
[0244] By comparing the Zeta potential of the nanosphere surface, it is shown that the Zeta potential of the nanosphere surface is related to the amount of the photosensitive initiator used. Compared with Example 1, the amount of photosensitive initiator used in Example 5 is larger, the content of carboxyl active groups on the surface of the nanosphere is more, the surface Zeta potential is also larger, and the stability is stronger.
[0245] The comparison results between Examples 5 and 7 to 9 and the measurement results between Examples 10 and 13 can all illustrate that the stability of small-diameter nano-microspheres is better than that of large-diameter nano-microspheres.
[0246] The measurement results between Example 5 and Example 10, and between Example 8 and Example 13 show that whether or not a heterogeneous wettability glass fiber separation membrane is used to separate and purify the nanospheres has no significant effect on the level of Zeta on the surface of the nanospheres, that is, the effect of the heterogeneous wettability glass fiber separation membrane on the stability of the nanospheres is not obvious.
[0247] Table 4 Zeta potential measurement results of nano-microspheres in Examples and Comparative Examples
[0248]
[0249] 4. Antibody Coupling Efficiency on Nanosphere Surface
[0250] A key point that determines the performance of latex enhanced immunoturbidimetric reagents is the amount of antibody that is chemically coupled to the surface of the nanospheres. The traditional method is to detect the residual antibody protein in the supernatant after coupling through enzyme-linked immunosorbent reaction (ELISA) or protein quantification method (Bradford, BCA method, etc.), and evaluate the efficiency of antibody coupling to the microsphere surface based on the residual amount of antibody in the supernatant.
[0251] In the present invention, the nanosphere samples obtained in Examples 5, 8, 10 and 13 and Comparative Examples 2 and 4 are first used to prepare antibody-coupled nanospheres (as shown in Examples 14 to 17 and Comparative Examples 5 to 6), and the supernatant after coupling is extracted and detected using the BCA method.
[0252] Embodiment 14
[0253] This embodiment provides a method for preparing modified antibody-sensitized polystyrene-polymethyl methacrylate block nanospheres from the nanospheres of Example 5, comprising the following steps:
[0254] (1) Add 500 μL of the carboxylated segmented nanospheres prepared in Example 5 and 8.0 mL of phosphate buffer with a pH of 7.2-7.4 into a 20 mL centrifuge tube, mix well, add 100 μL of a 10 mg / mL EDC solution and 100 μL of a 10 mg / mL NHS solution, and incubate and activate on a shaker at 60 rpm for 30 min at room temperature to obtain a first emulsion;
[0255] (2) slowly adding the antibody buffer (adding 100 μL of the antibody buffer at a time within 2 to 4 minutes, while continuously stirring to ensure uniform mixing) into the first emulsion, and then incubating on a shaker at 60 rpm for 3 hours at room temperature to obtain a first incubation solution, wherein the antibody buffer is prepared by adding 150 μL of troponin I (CTNI) antibody (purchased from Nanjing Oukai Biotechnology Co., Ltd.) into 5 mL of activation buffer (30 mM phosphate buffer + 2% sodium chloride (w / v), pH = 7.2-7.4), and mixing evenly;
[0256] (3) The first incubation solution was centrifuged at 4°C, 10,000 rpm, and 10 min. The supernatant was collected and the precipitate was resuspended in 6 mL of blocking solution (30 mM phosphate buffer + 1.5% BSA (w / v) + 1% sodium chloride (w / v), pH = 7.2-7.4), sonicated in an ice water bath, and then incubated on a shaker at 60 rpm for 1 h at room temperature to obtain a second incubation solution, wherein the ultrasonic parameters were: at 300 W power, sonicated for 2 s, rested for 1 s, sonicated for 2 min, then rested for 1 min, and repeated the above sonication for 2 min and rested for 1 min three times;
[0257] (4) The second incubation solution was centrifuged at 4°C, 10,000 rpm, and 5 min. The precipitate was resuspended in 20 mL of R2 buffer (10 mM phosphate buffer + 1% sucrose (w / v) + 0.1% Proclin 300 (v / v)). After sonication in an ice-water bath, CTNI antibody-sensitized nanospheres were obtained and stored at 4°C. The sonication method was the same as that in (3) above.
[0258] Embodiment 15
[0259] This example provides a method for preparing modified antibody-sensitized polystyrene-polymethyl methacrylate block nanospheres from the nanospheres of Example 8. The steps are basically the same as those of Example 14, except that:
[0260] The nanospheres are replaced with the carboxylated block nanospheres prepared in Example 8;
[0261] The antibody in the antibody buffer was replaced with C-reactive protein (CRP) antibody (purchased from Nanjing Okey Biotechnology Co., Ltd.).
[0262] Example 16
[0263] This example provides a method for preparing modified antibody-sensitized polystyrene-polymethyl methacrylate block nanospheres from the nanospheres of Example 10. The steps are basically the same as those of Example 14, except that:
[0264] The nanospheres were replaced with the carboxylated block nanospheres prepared in Example 10.
[0265] Embodiment 17
[0266] This example provides a method for preparing modified antibody-sensitized polystyrene-polymethyl methacrylate block nanospheres from the nanospheres of Example 13. The steps are basically the same as those of Example 15, except that:
[0267] The nanospheres were replaced with the carboxylated block nanospheres prepared in Example 13.
[0268] Comparative Example 5
[0269] This embodiment provides a method for preparing modified antibody-sensitized nanoparticles from the nanoparticles of Comparative Example 2. The steps are basically the same as those of Example 15, except that:
[0270] The nanospheres are replaced with the carboxylated polystyrene nanospheres of Comparative Example 2.
[0271] Comparative Example 6
[0272] This embodiment provides a method for preparing modified antibody-sensitized nanoparticles from the nanoparticles of Comparative Example 4. The steps are basically the same as those of Example 14, except that:
[0273] The nanospheres are replaced with the carboxylated polystyrene nanospheres of Comparative Example 4.
[0274] The following is a method for detecting the antibody protein remaining in the supernatant after coupling in Examples 14 to 17 and Comparative Examples 5 to 6, comprising the following steps:
[0275] The supernatants collected in step (3) of Examples 14 to 17 and Comparative Examples 5 to 6 were each detected for residual CTNI antibody protein using a BCA kit (Shanghai Biotech Co., Ltd.) and a Read Max 1000F absorbance microplate reader (Shanghai Shanpu Biotechnology Co., Ltd.) according to the steps described in the BCA kit manual, specifically:
[0276] ① Take 1.2ml of standard protein preparation solution and add it to 30mg BSA. After fully dissolving, prepare a 25mg / ml standard protein solution; take 20ul of 25mg / ml standard protein solution and add 980ul of PBS diluent to prepare a 0.5mg / ml protein standard solution;
[0277] ② Prepare BCA working solution according to the number of samples (mix reagent A and reagent B in a volume ratio of 50:1 and mix thoroughly);
[0278] ③ Add 0.5 mg / ml protein standard solution to the sample wells of the 96-well plate at the order of 0, 1, 2, 4, 8, 12, 16, and 20 ul, and add standard diluent to make up to 20 ul, that is, the concentrations of the standard are 0, 0.025, 0.05, 0.1, 0.2, 0.3, 0.4, and 0.5 mg / ml, respectively;
[0279] ④ Take out 20ul of sample from the corresponding supernatant of Example 5, Example 8, Example 10, Example 13, Comparative Example 2, and Comparative Example 4 respectively and add them to the sample wells of a 96-well plate;
[0280] ⑤ Add 200ul BCA working solution to each well, perform three parallel experiments on each standard and experimental sample, and incubate in a 37℃ constant temperature incubator for 20-30min;
[0281] ⑥ Determine A562 using Read Max 1000F microplate reader, collect and organize the absorbance values of each standard and sample, such as Figure 4 and as shown in Table 5;
[0282] ⑦ Draw a standard curve based on the determination results of the standard, calculate the remaining antibody concentration in the supernatant according to the absorbance of the experimental sample and the sample volume used, and then evaluate the coupling efficiency of the antibody and nanoparticles in each sample.
[0283] Table 5 Absorbance values measured in each well
[0284]
[0285]
[0286] With the concentration of each standard as the X-axis and the absorbance as the Y-axis, the linear regression equation was fitted using the mean absorbance of each standard, y=Ax+B, and then the amount of protein in the sample was calculated based on the absorbance value of the measured sample, thereby evaluating the coupling efficiency of the antibody and nanospheres in each sample.
[0287] like Figure 4 As shown, the standard curve obtained from the experiment is: y = 0.0002x + 0.1293 (R 2 =0.9978). Since the volumes used for each sample are consistent, the residual antibody concentrations in the supernatants of the corresponding samples of each embodiment and comparative example can be calculated according to the absorbance values measured in each embodiment and comparative example, and are listed in Table 5. It can be seen that the relationship between the residual antibody concentrations of each sample in the CTNI project is: comparative example 6> embodiment 16> embodiment 14, and the coupling efficiency of CTNI antibody binding to each nanosphere is: embodiment 14> embodiment 16> comparative example 6; the relationship between the residual antibody concentrations of each sample in the CRP project is: comparative example 5> embodiment 17> embodiment 15, and the coupling efficiency of CRP antibody binding to each nanosphere is: embodiment 15> embodiment 17> comparative example 5. The results showed that the coupling efficiency of antibody-nanospheres was related to the content of carboxyl active groups on the surface of nanospheres. The more active groups on the surface of nanospheres, the higher the coupling efficiency with antibodies. It is worth noting that after the nanospheres were separated and purified using a heterogeneous wettable glass fiber separation membrane, the residual emulsifier on the surface of the nanospheres was removed, eliminating the effect of the emulsifier on the coupling of nanospheres with antibodies and improving the coupling efficiency of nanospheres with antibodies.
[0288] Therefore, when coupled to the same concentration of antibodies, the coupling efficiency of the carboxylated block nano microspheres prepared by the present invention is higher, even when not purified by a heterogeneous wettability glass fiber separation membrane, it is possible to prepare nano microspheres that are better than products on the market, especially after removing the residual emulsifier on the surface of the nano microspheres through a heterogeneous wettability glass fiber separation membrane, so that the effect of the emulsifier on the nano microsphere coupling antibody is eliminated, and the surface of the obtained nano microspheres contains more carboxyl active groups, which has a higher efficiency when coupling antibodies. It can be inferred that when the carboxylated block nano microspheres prepared by the present invention are applied to latex enhanced immunoturbidimetric reagents, they can couple more antibodies, and have a higher detection sensitivity and a better detection effect when detecting antigen content.
[0289] Similarly, it can be concluded that when the carboxylated block nanoparticles are coupled with antigens to detect the presence of antibodies, since the nanoparticles prepared by the present invention have a higher content of functional groups on the surface, they will also have a better ability to couple with antigens, thereby having a higher detection sensitivity and a better detection effect when detecting the antibody content.
[0290] In summary, the polystyrene-polymethyl methacrylate block nanospheres prepared by the preparation method of carboxylated block nanospheres provided by the present invention have good light transmittance, and can introduce a large number of carboxyl active groups into the surface of the nanospheres, while ensuring that the nanospheres have good stability, while ensuring the coupling efficiency between the downstream nanospheres and antibodies, thereby providing certain beneficial effects for the research and development of latex enhanced immunoturbidimetry in vitro detection reagents.
[0291] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is limited by the attached embodiments and their equivalents.
Claims
1. A method for preparing carboxylated block nanospheres, characterized in that: The steps include: S1, adding a first catalyst, a hydroxyalkyl compound, and an organic polyacid into a first organic solution, and performing a constant temperature heating reaction to obtain an ester compound; S2, dissolving the ester compound and the aldehyde substance in a second organic solution, and carrying out a catalytic reaction under a weak alkaline environment and the action of a second catalyst, and then separating and purifying to obtain a hydroxyalkyl phenone free radical photosensitive initiator; S3, subjecting the photosensitive initiator, the dispersant and the first monomer to a light-induced polymerization reaction to obtain an intermediate product; S4, heating the intermediate product, the emulsifier, the redox initiator and the second monomer under the catalysis of a third catalyst to initiate a polymerization reaction to obtain a product system; S5, extracting the carboxylated segmented nanospheres from the product system.
2. The method for preparing carboxylated segmented nanospheres according to claim 1, characterized in that: It also includes one or more of the following technical features: A. The first monomer is one or more of acrylic acid, oleic acid, methyl methacrylate, acrylamide, vinyl naphthalene, and rosin acrylate; B. The second monomer is one or more of styrene, 1,2-diphenylethylene, styrene sulfonyl chloride, and divinylbenzene; C. The mass ratio of the photosensitive initiator to the first monomer is (0.2-0.8):(10-20); D. The mass ratio of the first monomer to the second monomer is (1-2):(1-3).
3. The method for preparing carboxylated block nanospheres according to claim 1, characterized in that: It also includes one or more of the following technical features: A. The first catalyst is selected from one or more of N,N-dicyclohexylcarbodiimide, 4-methylaminopyridine, and 4-arylpyridine; B. The hydroxyalkyl compound is trimethylolpropane; C. The organic polyacid is selected from one or more of 2,3-dihydroxysuccinic acid, 3-carboxy-3-hydroxyglutaric acid, and succinic acid; D. The molar ratio of the hydroxyalkyl compound to the aldehyde substance is (1-2):1; E. The mass ratio of the first catalyst to the hydroxyalkyl compound is 0.5% to 1%; F. The mass ratio of the second catalyst to the aldehyde substance is 1% to 2%; G. The weak alkaline environment has a pH of 8.0 to 8.5; H. The aldehyde substance is p-hydroxymethylbenzaldehyde; I. The second catalyst is zinc, titanium tetrachloride and lithium aluminum hydride.
4. The method for preparing carboxylated block nanospheres according to claim 1, characterized in that: It also includes one or more of the following technical features: A. The emulsifier is selected from one or more of sodium lauryl sulfate, sodium alkylnaphthalene sulfonate, polyvinyl alcohol, steareth-21, PEG-100 stearate, sorbitan tristearate, N-dodecyl dimethylamine, calcium dodecylbenzene sulfonate, and glyceryl monostearate; B. The redox initiator is selected from one or more of benzoyl peroxide-sucrose, tert-butyl hydroperoxide-rongalite, tert-butyl hydroperoxide-sodium metabisulfite, sodium persulfate-ferrous sulfate, hydrogen peroxide-ferrous sulfate, benzoyl peroxide-N,N-diethylaniline, benzoyl peroxide-ferrous pyrophosphate, potassium persulfate-ferrous chloride; C. The third catalyst is selected from one or more of 2,2,6,6-tetramethylpiperidine-1-oxide, phthalocyanine zinc polyarylether nitrile, dicyanobenzene derivatives, bipyridine ruthenium, and cerium ethanol complex; D. The mass ratio of the emulsifier, the redox initiator and the second monomer is (0.4-1):(10-30); E. The mass ratio of the photosensitive initiator, the first monomer, the emulsifier, the redox initiator, the third catalyst and the second monomer is: (0.2-0.8):(10-20):(0.2-0.5):(0.2-0.6):(0.2-0.4):(10-30).
5. The method for preparing carboxylated block nanospheres according to claim 1, characterized in that: It also includes one or more of the following technical features: A. The step of initiating the polymerization reaction by light is as follows: the photosensitive initiator, the dispersant and the first monomer are mixed in a third organic solution, and the mixed solution is irradiated under ultraviolet light to cause free radical cleavage of the photosensitive initiator, thereby initiating a free radical polymerization reaction of the first monomer; B. The step of heating to initiate the polymerization reaction is: mixing the intermediate product, emulsifier, redox initiator and third catalyst to obtain a third solution, and then adding the second monomer to the third solution.
6. The method for preparing carboxylated segmented nanospheres according to claim 5, characterized in that: In step A, the photosensitive initiator and the dispersant are dissolved in the third organic solution to prepare a second solution, the second solution is heated and stirred at 35-45° C. and 70-140 rpm, and after the second solution is completely dissolved, the first monomer is added, and the heating and stirring are maintained until the light-induced polymerization reaction is completed; the conditions for the light-induced polymerization reaction are: the irradiation light is: ultraviolet light with a wavelength of 300-350 nm, and the irradiation time is 5-8 hours; In step B, the third solution is heated and stirred at 45-55° C. and 95-105 rpm; the conditions for the heating to initiate the polymerization reaction are: reaction temperature of 50-70° C., stirring speed of 150-200 rpm, and reaction time of 8-14 h.
7. The method for preparing carboxylated block nanospheres according to claim 1, characterized in that: In S5, the extraction is to obtain a precipitate by centrifuging the product system, and then drying the precipitate.
8. The method for preparing carboxylated segmented nanospheres according to any one of claims 1 to 7, characterized in that: The method further comprises purifying the extracted carboxylated block nano-microspheres. The purification process comprises: resuspending the carboxylated block nano-microspheres with ultrapure water, filtering them with a heterogeneous wettability glass fiber separation membrane, and then drying them.
9. A carboxylated block nanosphere, characterized in that: The nanospheres are prepared according to the method for preparing carboxylated block nanospheres according to any one of claims 1 to 8, and the content of surface carboxyl active groups of the nanospheres is between 0.2 and 1.0 mmol / g.
10. The use of the carboxylated segmented nanospheres according to claim 9, characterized in that: The nano-microspheres are used for preparing latex enhanced immunoturbidimetric reagents.
Citation Information
Cited By
Red modified microsphere immunochromatography test strip for detecting ochratoxin A in wine and application of red modified microsphere immunochromatography test strip
CN119667149A