PLA-based heat shrink film

By designing compatibility agents and functional additives, combining the blending and bidirectional stretching process of PLA and PBAT, the problem of insufficient toughness and heat shrinkability of PLA-based heat shrink film is solved, and a high-performance PLA-based heat shrink film is achieved. Preparation, with excellent mechanical properties and high shrinkage, and maintains degradable properties.

CN118955784AInactive Publication Date: 2024-11-15PUSIWEI (SHANGHAI) BIOMATERIALS CO LTD

Patent Information

Application Number
CN202410991267.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing biodegradable heat shrinkable films have insufficient toughness and heat shrinkability, which limits its application promotion.

Method used

By designing compatibility agents and functional additives, including ring-opening reaction of lactic acid and epoxy olefins and modification of nanosilicon, combined with the blending and bidirectional stretching process of PLA and PBAT, excellent mechanical properties and high shrinkage rate were prepared by designing compatible agents and functional additives, including ring-opening reaction of lactic acid and epoxy olefins and modification of nanosilicon, combined with the blending and bidirectional stretching process of PLA and PBAT, the company has prepared a high shrinkage rate by designing compatibilities and functional additives, including ring-opening reaction of lactic acid and epoxy olefins and modification of nanosilicon, combined with the blending and bidirectional stretching process of PLA and PBAT, the company has a high mechanical properties and a high shrinkage rate. PLA-based heat shrink film.

Benefits of technology

The mechanical strength, toughness and heat shrinkability of the PLA-based heat shrink film are significantly improved, and its performance in applications is improved, and all materials are degradable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_11
    Figure SMS_11
  • Figure SMS_12
    Figure SMS_12
Patent Text Reader

Abstract

The invention belongs to the field of polymeric membranes. The invention relates to a PLA-based thermal shrinkage film and a preparation method thereof. The packaging film comprises the following raw materials in parts by weight: 65-85 parts of PLA; 15 to 35 parts of PBAT; 2.0 to 3.0 parts of a compatilizer; 4.0 to 6.0 parts of a functional auxiliary agent; 0.3 to 0.5 part of an antioxidant; 0.5 to 1.0 part of a lubricant; wherein the total mass of the PLA and the PBAT is 100 parts; the preparation method comprises the following steps: mixing the raw materials according to the formula, extruding, plasticizing, biaxially stretching, thermoforming, drawing, slitting, rolling and the like. According to the present invention, the defects of low toughness, low strength, poor thermal shrinkage and the like of the thermal shrinkage film prepared from the biodegradable material in the prior art can be effectively solved, and the main raw materials are the degradable materials so as to provide the great application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a PLA-based heat shrinkable film and a preparation method thereof, and belongs to the field of degradable films. Background Art

[0004] At present, there are relatively few studies on biodegradable heat shrinkable films. Among biodegradable materials, polylactic acid (PLA) is an aliphatic polyester that naturally decomposes into CO2 and water under composting conditions. It is a green and environmentally friendly bio-source material. It is also the only transparent biodegradable polymer and is used in the field of transparent packaging containers and daily necessities. However, its inherent brittleness limits its application and promotion.

[0005] In view of the above problems and the transparency advantage of PLA, it is of great significance to modify PLA to improve its processability, toughness and shrinkage. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a PLA-based heat shrinkable film, which is aimed at the defects of the heat shrinkable film prepared based on biodegradable materials in the prior art, such as low toughness and strength, poor heat shrinkage, etc. The compatibilizer and functional additive are prepared by molecular structure design, and are added to an extruder after formula design for extrusion and biaxial stretching. The technical solution adopted by the present invention to solve the technical problem is:

[0007] The present invention provides a method for preparing a compatibilizer, comprising the following steps:

[0008] S11, performing a ring-opening reaction between lactic acid and epoxyolefin A in the presence of a catalyst to obtain lactic acid ester;

[0009] S12, UV curing the lactate, aromatic acrylate, aliphatic acrylate, and epoxy olefin B under a photoinitiator to obtain a target product, namely a compatibilizer.

[0010] Furthermore, the lactic acid and epoxy olefins A are added in a molar ratio of carboxyl to epoxy of 1:1.

[0011] Further,

[0012] The usage ratio of the lactic acid ester, aromatic acrylate, aliphatic acrylate and epoxy olefin B is 0.2-0.4 mol: 0.2-0.3 mol: 0.2-0.3 mol: 0.2-0.3 mol.

[0013] The invention provides a compatibilizer, which is prepared by the preparation method of the compatibilizer.

[0014] Another object of the present invention is to provide a method for preparing a functional additive, comprising the following steps:

[0015] S21, placing nano-silicon and an aminosilane coupling agent in an alcohol solvent for silylation coupling reaction to obtain modified nano-silicon;

[0016] S22, performing a ring-opening reaction on the modified nano-silicon and the epoxy compound to obtain a target product, namely a functional additive.

[0017] Furthermore, the usage ratio of the nano-silicon, the aminosilane coupling agent and the alcohol solvent is 1g:3.5-5.5g:80mL.

[0018] Further,

[0019] The modified nano silicon and the epoxy compound are mixed in a molar ratio of amino group to epoxy group of 1:2-6; and

[0020] The molecular weight of the epoxy compound is 1000-3000.

[0021] Another object of the present invention is to provide a functional auxiliary agent prepared by the above-mentioned method for preparing the functional auxiliary agent.

[0022] Another object of the present invention is to provide a PLA-based heat shrinkable film, comprising the following raw materials in parts by weight:

[0023] PLA 65-85 parts;

[0024] PBAT 15-35 parts;

[0025] Compatibilizer 2.0-3.0 parts;

[0026] Functional additives 4.0-6.0 parts;

[0027] Antioxidant 0.3-0.5 parts;

[0028] Lubricant 0.5-1.0 part;

[0029] Among them, the total mass of PLA and PBAT is 100 parts.

[0030] Another object of the present invention is to provide a method for preparing a PLA-based heat shrinkable film, comprising the following steps:

[0031] S31, mixing, plasticizing, casting, cooling, i.e.

[0032] Add the raw materials blended evenly into the extruder according to the proportion, heat and melt blend, extrude through the die head, and adhere the melt to the surface of the casting roll for cooling to obtain a cast sheet;

[0033] S32, biaxial stretching, heat setting, i.e.

[0034] Biaxially stretching the obtained cast sheet, and then heat-setting it to obtain a biaxially oriented film; and

[0035] S33, traction and winding, i.e.

[0036] The prepared biaxially oriented film is pulled and trimmed, and finally rolled up to obtain a PLA-based heat shrinkable film.

[0037] Further, the die temperature is 190-200°C; and

[0038] The biaxial stretching parameters are: stretching ratio of 3.0-4.0; temperature of 70-90° C.; and speed of 60-100 mm / s.

[0039] Beneficial effects of the present invention:

[0040] (1) The present invention provides a PLA-based heat shrinkable film, which is mainly composed of PLA and PBAT for blending and toughening, and can provide better mechanical strength and toughness. Both PLA and PBAT are degradable materials.

[0041] (2) The present invention provides a PLA-based heat shrinkable film, wherein the raw material formula contains a self-made compatibilizer, which is a linear macromolecular chain structure containing aromatic ring side groups, fatty structure side groups, lactic acid structure side groups and epoxy side groups. First, the aromatic ring side groups, fatty structure side groups and ester groups have good compatibility with PBAT; the fatty structure side groups and lactic acid structures have good compatibility with PLA, so the compatibilizer has a two-phase compatibilization effect with PLA and PBAT; second, the epoxy structure in the compatibilizer can react with the hydroxyl groups in PLA and PBAT, has an excellent chain extension effect, and can improve the optical properties of the heat shrinkable film; third, the lactic acid structure side groups in the compatibilizer also have terminal hydroxyl structures, which can have a certain plasticizing effect on PLA and PBAT; fourth, the side group structure in the compatibilizer is mainly a flexible chain, which has a positive effect on the shrinkage rate of the heat shrinkable film.

[0042] (3) The present invention provides a PLA-based heat shrinkable film, wherein the raw materials of the formula contain a self-made functional additive, which is a hyperbranched nano-silicon microsphere structure containing multiple epoxy groups. First, the nano-silicon has uniform light, which has a positive effect on light transmittance; second, the hyperbranched nano-silicon microsphere structure coated with an organic chain structure has excellent dispersibility; and can be used as a cross-linking point, has a chain extension effect, and can greatly improve the mechanical properties; third, the epoxy structure has a certain molecular weight, which can effectively improve the shrinkage rate of the shrinkable film during the heat treatment process.

[0043] (4) The present invention provides a method for preparing a PLA-based heat shrinkable film, which is prepared by a biaxial stretching process. After biaxial stretching orientation, the mechanical properties of the shrinkable film can be effectively improved, and after heat treatment, the oriented macromolecular chains will be deoriented and stretch to a free state, thereby obtaining a greater shrinkage rate. DETAILED DESCRIPTION

[0044] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.

[0045] The purpose of the present invention is to develop a PLA-based heat shrinkable film. The design idea is: PLA and the main resin, add a heat shrinkage-promoting additive and perform biaxial stretching to prepare. The problems faced are: 1. PLA toughening problem; 2. Preparation of functional additives that promote heat shrinkage. Solution: First, PLA toughening problem, PLA and PBAT are blended and modified, and considering the compatibility of PLA and PBAT, a compatibilizer containing lactic acid structure, benzene ring structure, etc. is prepared, and an epoxy structure with chain extension function and a long chain structure that can promote shrinkage are added. Second, the homemade functional additives, considering that the shrinkage mechanism of the heat shrinkable film is the deorientation of the macromolecular chain, a hyperbranched structure with a long-chain reactive functional group is designed, which can effectively improve the mechanical properties and promote heat shrinkage. The theoretical basis for the realization is: the self-made compatibilizer, firstly, lactic acid and epoxy olefins are subjected to a carboxyl and epoxy ring-opening reaction to form a lactate structure; then the lactate structure and the acrylate structure containing a benzene ring, an epoxy group, and a long-chain structure are cured by UV to efficiently form a compatibilizer macromolecular structure. The self-made functional additive is firstly subjected to a coupling reaction between nanosilicon and an aminosilane coupling agent to obtain aminosilane-modified nanosilicon; then the aminosilane-modified nanosilicon and a long-chain multifunctional epoxy structure are subjected to a ring-opening reaction to obtain a multi-epoxy long-chain hyperbranched structure. Finally, after formula design and taking into account the optical properties of the shrink film, PLA is mainly used and PBAT is supplemented, and the above-mentioned self-made ingredients are added to the various raw material components for blending, extrusion, and biaxial stretching process to obtain a PLA-based heat shrink film material with effectively improved properties including heat shrinkage. The components work synergistically with each other to effectively improve mechanical properties, etc. The embodiments of the present invention are as follows:

[0046] The embodiment of the present invention provides a method for preparing a compatibilizer, comprising the following steps:

[0047] S11, dissolve epoxy olefin A and hydroquinone in N,N-dimethylformamide A and place them in a constant pressure dropping funnel, place lactic acid, catalyst and N,N-dimethylformamide B in a three-necked flask, slowly add dropwise, stir at 100-105°C for 12-15h, cool to room temperature, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain lactic acid ester.

[0048] The lactic acid and epoxy olefins A are added in a molar ratio of carboxyl group to epoxy group of 1:1;

[0049] The dosage ratio of the N,N-dimethylformamide A, lactic acid, and N,N-dimethylformamide B is 100 mL: 0.1 mol: 300 mL;

[0050] The amount of hydroquinone used is 1.0% of the mass of epoxy olefin A;

[0051] The amount of the catalyst used is 0.4% of the total mass of the reactants;

[0052] The catalyst may be triphenylphosphine or the like;

[0053] The epoxy olefins A may be glycidyl methacrylate, (glycidyloxy)ethyl methacrylate, allyl glycidyl ether, 1,2-epoxy-7-octene or 1,2-epoxy-9-decene, etc.; and glycidyl methacrylate is preferred.

[0054] S12, N2 protection, lactate, aromatic acrylate, aliphatic acrylate, epoxy olefin B, photoinitiator are dissolved in N,N-dimethylformamide C, stirred, placed under UV device for UV curing for 5-30 minutes; after the reaction is completed, the reaction device is removed, vacuum distillation is carried out, and vacuum drying is carried out at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer.

[0055] The dosage ratio of the lactic acid ester, aromatic acrylate, aliphatic acrylate, epoxy olefin B and N,N-dimethylformamide C is 0.2-0.4 mol: 0.2-0.3 mol: 0.2-0.3 mol: 0.2-0.3 mol: 500 mL.

[0056] The aromatic acrylate may be phenyl methacrylate, 2-phenoxyethyl acrylate, benzyl methacrylate, 4-(6-(acryloyloxy)hexyloxy)benzoic acid, etc.; and preferably benzyl methacrylate;

[0057] The aliphatic acrylate may be methyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, lauryl methacrylate, stearic methacrylate, etc.; and isooctyl methacrylate is preferred;

[0058] The epoxy olefin B may be glycidyl methacrylate, (glycidyloxy)ethyl methacrylate, allyl glycidyl ether, 1,2-epoxy-7-octene or 1,2-epoxy-9-decene, etc.; and preferably glycidyl methacrylate;

[0059] The epoxy olefins B and the epoxy olefins A in the present invention may be the same epoxy olefins or different epoxy olefins. To simplify the types of raw materials, the same epoxy olefins are selected in the embodiment of the present invention.

[0060] The amount of the photoinitiator is 1.0-4.0% of the total mass of the reactants;

[0061] The photoinitiator can be photoinitiator 184, photoinitiator 1173, photoinitiator 2959, photoinitiator TPO, etc.

[0062] The radiation energy intensity of the UV device can be 300-500 mW / cm 2 ; Specifically, it can be 300mW / cm 2 、350mW / cm 2 , 400mW / cm 2 、450mW / cm 2 , 500mW / cm 2 , or a range of any two values; and the radiation energy intensity of the UV device described in the following embodiments of the present invention is 400mW / cm 2 .

[0063] The present invention provides a method for preparing a functional additive, comprising the following steps:

[0064] S21, adding silicon dioxide and aminosilane coupling agent to an alcohol solvent, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 50-80° C. for 2-10 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain modified nano-silicon.

[0065] The dosage ratio of the nano-silicon, the aminosilane coupling agent and the alcohol solvent is 1g:3.5-5.5g:80mL.

[0066] The nano-silicon, with an average particle size of 50-100 nm, was purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.

[0067] The aminosilane coupling agent may be KH901, KH902, KH540, KH550, KH602, or KH792, and preferably KH550.

[0068] The alcohol solvent may be anhydrous methanol, anhydrous ethanol, anhydrous isopropanol, etc., and anhydrous ethanol is preferred.

[0069] S22, adding the modified nano-silicon to N,N-dimethylformyl D, ultrasonicating, dripping into the reaction kettle containing epoxy compound and N,N-dimethylformyl E through a peristaltic pump, heating to 40-60°C, stirring for 2-4h after the completion of the dripping, distilling under reduced pressure, and then drying in a vacuum oven at 40°C for 12h to obtain the target product, i.e., the functional additive.

[0070] The modified nano silicon and the epoxy compound are mixed in a molar ratio of amino group to epoxy group of 1:2-6;

[0071] The dosage ratio of the N,N-dimethylformyl D, the epoxy compound, and the N,N-dimethylformyl E is 200 mL: 0.1 mol: 600 mL;

[0072] The molecular weight of the epoxy compound is 1000-3000; it can be 1000, 1500, 2000, 2500, 3000, or a range consisting of any two values.

[0073] The epoxy compound can be epoxy soybean oil or epoxy-polyethylene glycol-epoxy, etc., wherein the molecular weight of the epoxy-polyethylene glycol-epoxy can be designed as required.

[0074] The embodiment of the present invention further provides a PLA-based heat shrinkable film, comprising the following raw materials in parts by weight:

[0075] PLA 65-85 parts;

[0076] PBAT 15-35 parts;

[0077] Compatibilizer 2.0-3.0 parts;

[0078] Functional additives 4.0-6.0 parts;

[0079] Antioxidant 0.3-0.5 parts;

[0080] Lubricant 0.5-1.0 part;

[0081] Among them, the total mass of PLA and PBAT is 100 parts.

[0082] The melt index of the PLA is 2.5-3.5 g / 10 min (190° C., 2.16 kg); the model of the PLA described in the following embodiments of the present invention is PT102, purchased from Pulisi Biotechnology Co., Ltd. PT102 PLA has self-nucleation ability and can crystallize quickly.

[0083] The brand of PBAT described in the following embodiments of the present invention is TH801T, which was purchased from Xinjiang Blue Mountain Tunhe Polyester Co., Ltd.

[0084] The antioxidant is a hindered phenol; it can be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, etc.; and the antioxidant described in the following embodiments of the present invention is antioxidant 1010.

[0085] The lubricant may be erucamide, oleamide, ethylene bisstearamide, etc.; and, the lubricant described in the following embodiments of the present invention is erucamide and ethylene bisstearamide mixed and added in a mass ratio of 2 / 1.

[0086] The embodiment of the present invention also provides a method for preparing a PLA-based heat shrinkable film, comprising the following steps:

[0087] S31, mixing, plasticizing, casting, cooling, i.e.

[0088] Add the uniformly blended raw materials into a twin-screw extruder according to the proportion, heat and melt blend, extrude through a die head, and adhere the melt to the surface of a casting roll for cooling to obtain a cast sheet;

[0089] The twin-screw extruder is set with the temperature of each zone at 150-190°C, the die head temperature at 190-200°C, and the casting temperature at 30-50°C.

[0090] S32, biaxial stretching, heat setting, i.e.

[0091] The obtained cast sheet is subjected to biaxial stretching, and then heat-set at 90-100° C. for 10-20 minutes to obtain a biaxially oriented film;

[0092] The biaxial stretching parameters are: stretching ratio of 3.0-4.0; temperature of 70-90° C.; and speed of 60-100 mm / s.

[0093] S33, traction and winding, i.e.

[0094] The prepared biaxially oriented film is pulled and trimmed, and finally rolled up to obtain a PLA-based heat shrinkable film with a thickness of 15-40 μm.

[0095] The PLA-based heat shrinkable film can be designed according to needs, and can be 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, or a range value consisting of any two values.

[0096] In order to further understand the present invention, a PLA-based heat shrinkable film provided by the present invention is described in detail below in conjunction with specific embodiments, and the protection scope of the present invention is not limited by the following embodiments.

[0097] Example 1

[0098] A method for preparing a compatibilizer comprises the following steps:

[0099] S11, dissolve glycidyl methacrylate and hydroquinone in N,N-dimethylformamide A and place in a constant pressure dropping funnel, place lactic acid, triphenylphosphine and N,N-dimethylformamide B in a three-necked flask, slowly add dropwise, stir at 100°C for 15h, cool to room temperature, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain lactic acid ester.

[0100] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1;

[0101] The dosage ratio of the N,N-dimethylformamide A, lactic acid, and N,N-dimethylformamide B is 100 mL: 0.1 mol: 300 mL;

[0102] The amount of hydroquinone used is 1.0% of the mass of glycidyl methacrylate;

[0103] The amount of triphenylphosphine used is 0.4% of the total mass of the reactants.

[0104] Its infrared data are as follows: 3364cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group exists.

[0105] S12, N2 protection, lactate, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, photoinitiator 184 were dissolved in N,N-dimethylformamide C, stirred, and placed under UV device for UV curing for 15 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer

[0106] The dosage ratio of the lactic acid ester, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, and N,N-dimethylformamide C is 0.3 mol: 0.2 mol: 0.25 mol: 0.25 mol: 500 mL.

[0107] The amount of the photoinitiator 184 used is 2.0% of the total mass of the reactants.

[0108] Its infrared data are as follows: 3364cm -1 :-OH exists; 3011cm-1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- does not exist; 1265cm -1 、893cm -1 、825cm -1 : Epoxy group exists.

[0109] A method for preparing a functional additive comprises the following steps:

[0110] S21, adding silica and aminosilane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 70° C. for 6 h, filtering, taking the insoluble matter, and drying at 60° C. for 12 h to obtain modified nano-silicon.

[0111] The usage ratio of the nano-silicon, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL.

[0112] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists.

[0113] S22, adding modified nano silicon to N,N-dimethylformyl D, ultrasonicating, dripping into the reaction kettle containing epoxy compound and N,N-dimethylformyl E through a peristaltic pump, heating to 50°C, stirring for 2.5h after the completion of dripping, distilling under reduced pressure, and drying in a vacuum oven at 40°C for 12h to obtain the target product, i.e., the functional additive.

[0114] The modified nano-silicon and the epoxy compound are mixed in a molar ratio of 1:2 between the amino group and the epoxy group;

[0115] The dosage ratio of the N,N-dimethylformyl D, the epoxy compound, and the N,N-dimethylformyl E is 200 mL: 0.1 mol: 600 mL;

[0116] The epoxy compound is epoxy-polyethylene glycol-epoxy (molecular weight is 2000).

[0117] Its infrared data is as follows: 3378cm -1 :-OH exists and is enhanced; 1560cm -1: -NH peak exists and weakens; 1109cm -1 、801cm -1 :-Si-O- exists; 1261cm -1 、892cm -1 、824cm -1 : Epoxy group exists.

[0118] A PLA-based heat shrinkable film comprises the following raw materials in parts by weight:

[0119] PLA 75 copies;

[0120] PBAT 25 copies;

[0121] 2.5 parts of compatibilizer;

[0122] Functional additives 5.0 parts;

[0123] 0.4 parts of antioxidant;

[0124] 0.7 parts of lubricant.

[0125] A method for preparing a PLA-based heat shrinkable film comprises the following steps:

[0126] S31, mixing, plasticizing, casting, cooling, i.e.

[0127] Add the uniformly blended raw materials into a twin-screw extruder according to the proportion, heat and melt blend, extrude through a die head, and adhere the melt to the surface of a casting roll for cooling to obtain a cast sheet;

[0128] The twin-screw extruder is set with the temperature of zone 1 at 160°C, zone 2 at 170°C, zone 3 at 180°C, zone 4 at 190°C, die head temperature at 195°C, and casting temperature at 40°C.

[0129] S32, biaxial stretching, heat setting, i.e.

[0130] The obtained cast sheet was subjected to biaxial stretching and then heat-set at 95°C for 15 minutes to obtain a biaxially oriented film;

[0131] The biaxial stretching parameters are: stretching ratio of 3.5; temperature of 80° C.; and speed of 80 mm / s.

[0132] S33, traction and winding, i.e.

[0133] The prepared biaxially oriented film was pulled and trimmed, and finally rolled up to obtain a PLA-based heat shrinkable film with a thickness of 30 μm.

[0134] Example 2

[0135] The rest is the same as in Example 1, except that:

[0136] A method for preparing a compatibilizer comprises the following steps:

[0137] S11, dissolve glycidyl methacrylate and hydroquinone in N,N-dimethylformamide A and place in a constant pressure dropping funnel, place lactic acid, triphenylphosphine and N,N-dimethylformamide B in a three-necked flask, slowly add dropwise, stir at 105°C for 12h, cool to room temperature, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain lactic acid ester.

[0138] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1;

[0139] The dosage ratio of the N,N-dimethylformamide A, lactic acid, and N,N-dimethylformamide B is 100 mL: 0.1 mol: 300 mL;

[0140] The amount of hydroquinone used is 1.0% of the mass of glycidyl methacrylate;

[0141] The amount of triphenylphosphine used is 0.4% of the total mass of the reactants.

[0142] Its infrared data are as follows: 3364cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group exists.

[0143] S12, N2 protection, lactate, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, photoinitiator 184 were dissolved in N,N-dimethylformamide C, stirred, and placed under UV device for UV curing for 10 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer

[0144] The dosage ratio of the lactic acid ester, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, and N,N-dimethylformamide C is 0.2 mol: 0.3 mol: 0.2 mol: 0.3 mol: 500 mL.

[0145] The amount of the photoinitiator 184 used is 3.0% of the total mass of the reactants.

[0146] Its infrared data are as follows: 3364cm -1 :-OH exists; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- does not exist; 1265cm -1 、893cm -1 、825cm -1 : Epoxy group exists.

[0147] A method for preparing a functional additive comprises the following steps:

[0148] S21, adding silica and aminosilane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 80° C. for 2 h, filtering, taking the insoluble matter, and drying at 60° C. for 12 h to obtain modified nano-silicon.

[0149] The usage ratio of the nano-silicon, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL.

[0150] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists.

[0151] S22, adding the modified nano-silicon to N,N-dimethylformyl D, ultrasonicating, dripping into the reaction kettle containing epoxy compound and N,N-dimethylformyl E through a peristaltic pump, heating to 40°C, stirring for 4 hours after the completion of the dripping, distilling under reduced pressure, and then drying in a vacuum oven at 40°C for 12 hours to obtain the target product, i.e., the functional additive.

[0152] The modified nano-silicon and the epoxy compound are mixed in a molar ratio of 1:2 between the amino group and the epoxy group;

[0153] The dosage ratio of the N,N-dimethylformyl D, the epoxy compound, and the N,N-dimethylformyl E is 200 mL: 0.1 mol: 600 mL;

[0154] The epoxy compound is epoxy-polyethylene glycol-epoxy (molecular weight is 2000).

[0155] Its infrared data is as follows: 3378cm -1:-OH exists and is enhanced; 1560cm -1 : -NH peak exists and weakens; 1109cm -1 、801cm -1 :-Si-O- exists; 1261cm -1 、892cm -1 、824cm -1 : Epoxy group exists.

[0156] Example 3

[0157] The rest is the same as in Example 1, except that:

[0158] A method for preparing a compatibilizer comprises the following steps:

[0159] S11, dissolve glycidyl methacrylate and hydroquinone in N,N-dimethylformamide A and place in a constant pressure dropping funnel, place lactic acid, triphenylphosphine and N,N-dimethylformamide B in a three-necked flask, slowly add dropwise, stir at 100°C for 15h, cool to room temperature, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain lactic acid ester.

[0160] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1;

[0161] The dosage ratio of the N,N-dimethylformamide A, lactic acid, and N,N-dimethylformamide B is 100 mL: 0.1 mol: 300 mL;

[0162] The amount of hydroquinone used is 1.0% of the mass of glycidyl methacrylate;

[0163] The amount of triphenylphosphine used is 0.4% of the total mass of the reactants.

[0164] Its infrared data are as follows: 3364cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group exists.

[0165] S12, N2 protection, lactate, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, photoinitiator 184 were dissolved in N,N-dimethylformamide C, stirred, and placed under UV device for UV curing for 30 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer

[0166] The dosage ratio of the lactic acid ester, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, and N,N-dimethylformamide C is 0.4 mol: 0.2 mol: 0.2 mol: 0.2 mol: 500 mL.

[0167] The amount of the photoinitiator 184 used is 1.0% of the total mass of the reactants.

[0168] Its infrared data are as follows: 3364cm -1 :-OH exists; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- does not exist; 1265cm -1 、893cm -1 、825cm -1 : Epoxy group exists.

[0169] A method for preparing a functional additive comprises the following steps:

[0170] S21, adding silica and aminosilane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 50° C. for 10 h, filtering, taking the insoluble matter, and drying at 60° C. for 12 h to obtain modified nano-silicon.

[0171] The usage ratio of the nano-silicon, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL.

[0172] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm- 1 :-Si-O- exists.

[0173] S22, adding the modified nano-silicon to N,N-dimethylformyl D, ultrasonicating, dripping into the reaction kettle containing epoxy compound and N,N-dimethylformyl E through a peristaltic pump, heating to 60°C, stirring for 2h after the addition is completed, distilling under reduced pressure, and then drying in a vacuum oven at 40°C for 12h to obtain the target product, i.e., the functional additive.

[0174] The modified nano-silicon and the epoxy compound are mixed in a molar ratio of 1:2 between the amino group and the epoxy group;

[0175] The dosage ratio of the N,N-dimethylformyl D, the epoxy compound, and the N,N-dimethylformyl E is 200 mL: 0.1 mol: 600 mL;

[0176] The epoxy compound is epoxy-polyethylene glycol-epoxy (molecular weight is 2000).

[0177] Its infrared data is as follows: 3378cm -1 :-OH exists and is enhanced; 1560cm -1 : -NH peak exists and weakens; 1109cm -1 、801cm -1 :-Si-O- exists; 1261cm -1 、892cm -1 、824cm -1 : Epoxy group exists.

[0178] Example 4

[0179] The rest is the same as in Example 1, except that:

[0180] A method for preparing a compatibilizer comprises the following steps:

[0181] S11, dissolve glycidyl methacrylate and hydroquinone in N,N-dimethylformamide A and place in a constant pressure dropping funnel, place lactic acid, triphenylphosphine and N,N-dimethylformamide B in a three-necked flask, slowly add dropwise, stir at 100°C for 15h, cool to room temperature, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain lactic acid ester.

[0182] The lactic acid and glycidyl methacrylate are added in a molar ratio of carboxyl group to epoxy group of 1:1;

[0183] The dosage ratio of the N,N-dimethylformamide A, lactic acid, and N,N-dimethylformamide B is 100 mL: 0.1 mol: 300 mL;

[0184] The amount of hydroquinone used is 1.0% of the mass of glycidyl methacrylate;

[0185] The amount of triphenylphosphine used is 0.4% of the total mass of the reactants.

[0186] Its infrared data are as follows: 3364cm -1 :-OH exists; 1710cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group exists.

[0187] S12, N2 protection, lactate, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, photoinitiator 184 were dissolved in N,N-dimethylformamide C, stirred, and placed under UV device for UV curing for 5 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer

[0188] The dosage ratio of the lactic acid ester, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, and N,N-dimethylformamide C is 0.3 mol: 0.25 mol: 0.2 mol: 0.25 mol: 500 mL.

[0189] The amount of the photoinitiator 184 used is 4.0% of the total mass of the reactants.

[0190] Its infrared data are as follows: 3364cm -1 :-OH exists; 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- does not exist; 1265cm -1 、893cm -1 、825cm -1 : Epoxy group exists.

[0191] A method for preparing a functional additive comprises the following steps:

[0192] S21, adding silicon dioxide and aminosilane coupling agent KH550 to anhydrous ethanol, ultrasonically oscillating for 0.5 h, standing at room temperature for 2 h, reacting at 60° C. for 8 h, filtering, taking insoluble matter, and drying at 60° C. for 12 h to obtain modified nano-silicon.

[0193] The usage ratio of the nano-silicon, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:4.5g:80mL.

[0194] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1560cm -1 : -NH peak exists; 1109cm -1 、801cm -1 :-Si-O- exists.

[0195] S22, adding modified nano silicon to N,N-dimethylformyl D, ultrasonicating, dripping into the reaction kettle containing epoxy compound and N,N-dimethylformyl E through a peristaltic pump, heating to 50°C, stirring for 2.5h after the completion of dripping, distilling under reduced pressure, and drying in a vacuum oven at 40°C for 12h to obtain the target product, i.e., the functional additive.

[0196] The modified nano-silicon and the epoxy compound are mixed in a molar ratio of 1:2 between the amino group and the epoxy group;

[0197] The dosage ratio of the N,N-dimethylformyl D, the epoxy compound, and the N,N-dimethylformyl E is 200 mL: 0.1 mol: 600 mL;

[0198] The epoxy compound is epoxy-polyethylene glycol-epoxy (molecular weight is 2000).

[0199] Its infrared data is as follows: 3378cm -1 :-OH exists and is enhanced; 1560cm -1 : -NH peak exists and weakens; 1109cm -1 、801cm -1 :-Si-O- exists; 1261cm -1 、892cm -1 、824cm -1 : Epoxy group exists.

[0200] Example 5

[0201] The rest is the same as in Example 1, except that:

[0202] The usage ratio of the nano-silicon, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:3.5g:80mL.

[0203] Example 6

[0204] The rest is the same as in Example 1, except that:

[0205] The usage ratio of the nano-silicon, aminosilane coupling agent KH550 and anhydrous ethanol is 1g:5.5g:80mL.

[0206] Example 7

[0207] The rest is the same as in Example 1, except that:

[0208] The epoxy compound is epoxy-polyethylene glycol-epoxy (molecular weight is 1000).

[0209] Example 8

[0210] The rest is the same as in Example 1, except that:

[0211] The epoxy compound is epoxy-polyethylene glycol-epoxy (molecular weight is 3000).

[0212] Example 9

[0213] The rest is the same as in Example 1, except that:

[0214] The modified nano silicon and the epoxy compound are mixed in a molar ratio of amino group to epoxy group of 1:5; and the epoxy compound is epoxy soybean oil.

[0215] Example 10

[0216] The rest is the same as in Example 1, except that:

[0217] The modified nano silicon and the epoxy compound are mixed in a molar ratio of amino group to epoxy group of 1:6; and the epoxy compound is epoxy soybean oil.

[0218] Embodiment 11

[0219] The rest is the same as in Example 1, except that:

[0220] A PLA-based heat shrinkable film comprises the following raw materials in parts by weight:

[0221] PLA 65 copies;

[0222] PBAT 35 copies;

[0223] 3.0 parts of compatibilizer;

[0224] 4.0 parts of functional additives;

[0225] 0.3 parts of antioxidant;

[0226] Lubricant 1.0 part

[0227] A method for preparing a PLA-based heat shrinkable film comprises the following steps:

[0228] S31, mixing, plasticizing, casting, cooling, i.e.

[0229] Add the uniformly blended raw materials into a twin-screw extruder according to the proportion, heat and melt blend, extrude through a die head, and adhere the melt to the surface of a casting roll for cooling to obtain a cast sheet;

[0230] The twin-screw extruder is set with the temperatures of zone 1 at 150°C, zone 2 at 160°C, zone 3 at 170°C, zone 4 at 185°C, die head temperature at 190°C, and casting temperature at 30°C.

[0231] S32, biaxial stretching, heat setting, i.e.

[0232] The obtained cast sheet was subjected to biaxial stretching and then heat-set at 90°C for 20 minutes to obtain a biaxially oriented film;

[0233] The biaxial stretching parameters are: stretching ratio of 4.0; temperature of 90° C.; and speed of 60 mm / s.

[0234] S33, traction and winding, i.e.

[0235] The prepared biaxially oriented film was pulled and trimmed, and finally rolled up to obtain a PLA-based heat shrinkable film with a thickness of 30 μm.

[0236] Example 12

[0237] The rest is the same as in Example 1, except that:

[0238] A PLA-based heat shrinkable film comprises the following raw materials in parts by weight:

[0239] PLA 85 copies;

[0240] PBAT 15 copies;

[0241] 2.0 parts of compatibilizer;

[0242] Functional additives 6.0 parts;

[0243] 0.5 parts of antioxidant;

[0244] 0.5 parts of lubricant.

[0245] S31, mixing, plasticizing, casting, cooling, i.e.

[0246] Add the uniformly blended raw materials into a twin-screw extruder according to the proportion, heat and melt blend, extrude through a die head, and adhere the melt to the surface of a casting roll for cooling to obtain a cast sheet;

[0247] The twin-screw extruder has set temperatures of 165°C in zone 1, 175°C in zone 2, 185°C in zone 3, 190°C in zone 4, 200°C in die head temperature, and 50°C in casting temperature.

[0248] S32, biaxial stretching, heat setting, i.e.

[0249] The obtained cast sheet was subjected to biaxial stretching and then heat-set at 100°C for 10 minutes to obtain a biaxially oriented film;

[0250] The biaxial stretching parameters are: stretching ratio of 3.0; temperature of 70° C.; and speed of 100 mm / s.

[0251] S33, traction and winding, i.e.

[0252] The prepared biaxially oriented film was pulled and trimmed, and finally rolled up to obtain a PLA-based heat shrinkable film with a thickness of 30 μm.

[0253] The following comparative examples are compared with specific embodiment 1:

[0254] Comparative Example 1

[0255] The rest is the same as in Example 1, except that:

[0256] No compatibilizer is added to the raw material formula of the PLA-based heat shrinkable film.

[0257] Comparative Example 2

[0258] The rest is the same as in Example 1, except that:

[0259] A method for preparing a compatibilizer comprises the following steps:

[0260] Under N2 protection, methyl methacrylate, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate, and photoinitiator 184 were dissolved in N,N-dimethylformamide C, stirred, and placed under UV device for UV curing for 15 minutes; after the reaction, the reaction device was removed, vacuum distilled, and vacuum dried at 40°C for 12 hours to obtain the target product, i.e., the compatibilizer

[0261] The usage ratio of methyl methacrylate, benzyl methacrylate, isooctyl methacrylate, glycidyl methacrylate and N,N-dimethylformamide C is 0.3 mol: 0.2 mol: 0.25 mol: 0.25 mol: 500 mL.

[0262] The amount of the photoinitiator 184 used is 2.0% of the total mass of the reactants.

[0263] Its infrared data are as follows: 3011cm -1 、1595cm -1 、1498cm -1 : benzene ring exists; 1735cm -1 :-C=O (ester group) exists and is enhanced; 1606cm -1 、811cm -1 :-C=C- does not exist; 1265cm -1 、893cm -1 、825cm -1 : Epoxy group exists.

[0264] Comparative Example 3

[0265] The rest is the same as in Example 1, except that:

[0266] The isooctyl methacrylate was replaced with methyl methacrylate.

[0267] Comparative Example 4

[0268] The rest is the same as in Example 1, except that:

[0269] The glycidyl methacrylate in S12 is replaced by butyl methacrylate.

[0270] Comparative Example 5

[0271] The rest is the same as in Example 1, except that:

[0272] No functional additives are added to the raw material formula of the PLA-based heat shrinkable film.

[0273] Comparative Example 6

[0274] The rest is the same as in Example 1, except that:

[0275] The epoxy-polyethylene glycol-epoxy (molecular weight 2000) was replaced with epoxy-polyethylene glycol-hydroxyl (molecular weight 2000).

[0276] Comparative Example 7

[0277] The rest is the same as in Example 1, except that:

[0278] The epoxy-polyethylene glycol-epoxy (molecular weight 2000) was replaced with neopentyl glycol diglycidyl ether.

[0279] Comparative Example 8

[0280] The rest is the same as in Example 1, except that:

[0281] The method for preparing the PLA-based heat shrinkable film does not involve a biaxial stretching process.

[0282] The physical properties of the PLA-based heat shrinkable films in the embodiments of the present invention and the comparative examples are respectively measured and the results are shown in Table 1.

[0283] Table 1 Physical test performance of each embodiment

[0284]

[0285]

[0286] First, it can be concluded from Examples 1-12 in Table 1 that the PLA-based heat shrinkable film of the present invention has excellent mechanical properties and a high shrinkage rate.

[0287] Second, it can be observed from Example 1 and Comparative Examples 1-4 that the PLA-based heat shrinkable film of the present invention uses a self-made compatibilizer, which has a significant effect on improving mechanical properties, optical properties, etc.; at the same time, it can be found that the lactate structure has the effect of improving the compatibilizer and plasticizing, and the long-chain side group structure and the reactive epoxy group structure have the function of improving compatibility and shrinkage, which is of great significance to improving the compatibility of the two phases, and can improve the shrinkage to a certain extent;

[0288] It can be observed from Example 1 and Comparative Examples 5-7 that the self-made functional additives in the PLA-based heat shrinkable film of the present invention have a positive effect on improving the mechanical properties and optical properties, especially on improving the heat shrinkage rate; at the same time, it can be found that the long-chain and reactive structure has a better effect on the shrinkage rate;

[0289] It can be observed from Examples 1 and 1-7 that the compatibilizer and the functional additive have a synergistic effect, which is of great significance for improving the mechanical properties, optical properties and shrinkage rate.

[0290] It can be observed from Example 1 and Comparative Example 8 that the PLA-based heat shrinkable film of the present invention has better mechanical properties after biaxial stretching, and the shrinkage rate is significantly improved.

[0291] In summary, the PLA-based heat shrinkable film provided by the present invention, on the one hand, is prepared by molecular design to prepare a highly reactive compatibilizer and a functional additive; on the other hand, it is prepared by formula design through extrusion and biaxial stretching processes, and has excellent performance; and the main raw materials used have the advantage of being completely degradable and widely used.

[0292] The test method is as follows:

[0293] The heat shrinkable films in the above embodiments and comparative examples were tested with reference to the provisions of GB / T 13529-2016, wherein the shrinkage rate was tested at 100° C. / 10 s.

[0294] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A method for preparing a compatibilizer, characterized in that: The following steps are involved: S11, performing a ring-opening reaction between lactic acid and epoxyolefin A in the presence of a catalyst to obtain lactic acid ester; S12, UV curing the lactate, aromatic acrylate, aliphatic acrylate, and epoxy olefin B under a photoinitiator to obtain a target product, namely a compatibilizer.

2. The method for preparing a compatibilizer according to claim 1, characterized in that: The lactic acid and epoxy olefins A are added in a molar ratio of carboxyl to epoxy of 1:

1.

3. The method for preparing a compatibilizer according to claim 1, characterized in that: The usage ratio of the lactic acid ester, aromatic acrylate, aliphatic acrylate and epoxy olefin B is 0.2-0.4 mol: 0.2-0.3 mol: 0.2-0.3 mol: 0.2-0.3 mol.

4. A compatibilizer, characterized in that: The compatibilizer is prepared by the preparation method of any one of claims 1 to 3.

5. A method for preparing a functional additive, characterized in that: The following steps are involved: S21, placing nano-silicon and an aminosilane coupling agent in an alcohol solvent for silylation coupling reaction to obtain modified nano-silicon; S22, performing a ring-opening reaction on the modified nano-silicon and the epoxy compound to obtain a target product, namely, a functional additive.

6. The method for preparing the functional additive according to claim 5, characterized in that: The dosage ratio of the nano-silicon, the aminosilane coupling agent and the alcohol solvent is 1g:3.5-5.5g:80mL.

7. The method for preparing the functional additive according to claim 5, characterized in that: The modified nano-silicon and the epoxy compound are mixed in a molar ratio of amino group to epoxy group of 1:2-6; and The molecular weight of the epoxy compound is 1000-3000.

8. A functional additive, characterized in that: Prepared by the preparation method of the functional auxiliary agent as claimed in any one of claims 5-7.

9. A PLA-based heat shrinkable film, characterized in that: The invention comprises the following raw materials in parts by weight: PLA 65-85 parts; PBAT 15-35 parts; Compatibilizer 2.0-3.0 parts; Functional additives 4.0-6.0 parts; Antioxidant 0.3-0.5 parts; Lubricant 0.5-1.0 part; Among them, the total mass of PLA and PBAT is 100 parts.

10. A method for preparing a PLA-based heat shrinkable film, characterized in that: The steps include: S31, mixing, plasticizing, casting, cooling, i.e. Add the raw materials blended evenly according to the proportion into the extruder, heat and melt blend, extrude through the die head, and adhere the melt to the surface of the casting roll for cooling to obtain a cast sheet; S32, biaxial stretching, heat setting, i.e. Biaxially stretching the obtained cast sheet, and then heat-setting it to obtain a biaxially oriented film; and S33, traction and winding, i.e. The prepared biaxially oriented film is pulled and trimmed, and finally rolled up to obtain a PLA-based heat shrinkable film.

11. The method for preparing a PLA-based heat shrinkable film according to claim 10, characterized in that: The die temperature is 190-200°C; and The biaxial stretching parameters are: stretching ratio of 3.0-4.0; temperature of 70-90° C.; and speed of 60-100 mm / s.

Citation Information

Patent Citations

  • Biodegradable polyester heat shrink film and preparation method thereof

    CN113789039A

  • High-temperature-resistant release PVA (Polyvinyl Alcohol) demolding film for artificial stone

    CN118978746A

  • Low-carbon high-barrier biodegradable mulching film and preparation method thereof

    CN118978747A

  • BOPLA (Biaxially Oriented Polylactic Acid) film with high stretching rate and preparation method thereof

    CN119639202A

  • Fluffy soft polyester fiber and preparation method thereof

    CN119824569A

Cited By

  • Bio-based compatilizer modified full-biodegradable two-way stretching heat shrinkage film and preparation method thereof

    CN121991409A