Flexible conductive composite material based on boron ester dynamic covalent bonds and preparation method and application thereof

By using flexible conductive composite materials based on the dynamic covalent bonds of boron esters, the problems of non-degradability and poor stability of flexible materials are solved, achieving self-healing and recyclability, and reducing environmental pollution.

CN118955853AActive Publication Date: 2024-11-15SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411249418.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-15
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

Existing flexible materials cannot be completely degraded, leading to environmental pollution and poor stability.

Method used

A flexible conductive composite material based on boron ester dynamic covalent bonds is used. By introducing dynamic covalent chemical bonds into the thermosetting network, an exchange reaction is initiated by external stimuli to achieve structural adhesion and shape reshaping of the material, which degrades during recycling.

Benefits of technology

The material is self-healing under heating conditions, maintaining its mechanical and sensing properties. After disposal, it is degradable in polar solvents, enabling efficient recycling and reducing the environmental impact of electronic waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955853A_ABST
    Figure CN118955853A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flexible sensors, and discloses a flexible conductive composite material based on boron ester dynamic covalent bonds and a preparation method and application thereof. The preparation method comprises the following steps: dissolving macromolecular dihydric alcohol, boron ester dihydric alcohol and diisocyanate in a polar organic solvent, adding a catalyst, stirring, carrying out a polyaddition reaction in an inert atmosphere to obtain a polymer solution, then adding a conductive material and micromolecular polyhydric alcohol, and carrying out ultrasonic stirring to obtain a polymer solution; and carrying out curing reaction and removing the solvent to obtain the flexible conductive composite material based on the boron ester dynamic covalent bond. The flexible conductive composite material provided by the invention has excellent mechanical properties, can be completely degraded in a water / organic solvent mixed solution, and solves the problem that the existing flexible material cannot be thoroughly degraded; when the flexible conductive composite material is used for preparing a flexible wearable strain sensor, the flexible conductive composite material has good electrochemical stability and signal response performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flexible sensors, and in particular to a flexible conductive composite material based on borate dynamic covalent bonds, and a preparation method and application thereof. Background Art

[0002] As human life becomes increasingly intelligent, flexible electronic devices have huge market prospects, especially in the biomedical field for wearable physiological monitoring devices, implantable medical electronic devices, electronic skin, etc. However, the rapid development of the electronics industry has also brought huge challenges to the management of electronic waste. According to the United Nations, tens of millions of tons of electronic waste are discarded every year around the world. Only a small amount of electronic waste is recycled, while most is sent directly to landfills or incinerators. The heavy metals in them will cause soil and groundwater pollution, leading to serious waste of resources and environmental pollution. Therefore, there is an urgent need for a degradable matrix material suitable for flexible electronic products to alleviate this problem.

[0003] The recyclable materials commonly used in traditional flexible electronics are mainly thermoplastic polymers, whose internal molecular chains are connected by non-covalent bonds. They soften and flow when heated, making them easy to repair, reshape and recycle. Their industrial production and manufacturing technology is also flexible and convenient, but their stability is poor. Unlike thermoplastic polymers, traditional thermosetting polymers are chemically cross-linked by covalent bonds. They have excellent mechanical properties, thermal stability and corrosion resistance, and are widely used in various fields. However, once traditional thermosetting resins are cured and formed, they cannot be processed again. The related welding, repair, recycling and other fields are difficult, so there are serious problems of resource waste and environmental pollution.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a flexible conductive composite material based on boron ester dynamic covalent bonds and a preparation method and application thereof, aiming to solve the problem that existing flexible materials cannot be completely degraded and pollute the environment and have poor stability.

[0006] In order to overcome the above problems of existing flexible materials, the inventors came up with the idea of ​​using glass-like polymer materials as matrix materials to prepare flexible conductive composite materials, and using their characteristics of introducing dynamic covalent chemical bonds in thermosetting networks to trigger exchange reactions through external stimuli while maintaining a constant crosslinking density. Glass-like polymer materials are no different from traditional thermosetting resins in normal conditions, but they can perform structural adhesion, shape reshaping, and material recycling when the reaction is activated, thus providing good prospects for constructing degradable and stable flexible composite materials and preparing flexible wearable sensors.

[0007] The technical solution of the present invention is as follows:

[0008] The first aspect of the present invention provides a method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds, comprising the steps of:

[0009] S1, dissolving a macromolecular diol, a boron ester diol and a diisocyanate in a polar organic solvent to form a mixed solution, adding a catalyst to the mixed solution and stirring, and performing a polyaddition reaction under an inert atmosphere to obtain a polymer solution;

[0010] S2. Adding a conductive material and a small molecule polyol to the polymer solution, after ultrasonic stirring, pouring it into a mold for curing reaction, removing the solvent, and obtaining the flexible conductive composite material based on boron ester dynamic covalent bonds.

[0011] Optionally, the macromolecular diol includes one or more of polyethylene glycol, polyester polyol, polypropylene glycol, polytetramethylene glycol, polycarbonate polyol, polycaprolactone polyol, and hydroxy-terminated polydimethylsiloxane.

[0012] Optionally, the borate diol has any one of the chemical structural formulas shown in formula (I) to (XI):

[0013]

[0014] Optionally, the diisocyanate is one or more of an aromatic diisocyanate, an aliphatic diisocyanate and an alicyclic diisocyanate. Specifically, the diisocyanate may be selected from isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, etc., but is not limited thereto.

[0015] Optionally, the catalyst is selected from one or more of dimethylcyclohexylamine, dibutyltin dilaurate, a triazine trimerization catalyst, stannous octoate and dibutyltin maleate, but is not limited thereto.

[0016] Optionally, the conductive material includes one or more of polyacetylene, polypyrrole, polyaniline, polythiophene, graphene, metal nanowires, metal nanoparticles and carbon nanotubes, but is not limited thereto.

[0017] Optionally, the polyol small molecule includes one or more of glycerol, trimethylolpropane, hexanetriol and pentaerythritol, but is not limited thereto.

[0018] Optionally, the molar ratio of the total amount of alcoholic hydroxyl groups contained in the macromolecular diol, borate ester diol and small molecular polyol to the isocyanate groups contained in the diisocyanate is 1:(0.9-1.4).

[0019] Optionally, the mass of the catalyst accounts for 0.05-5% of the theoretical mass of the polymer, and the mass of the conductive material accounts for 1-25% of the theoretical mass of the polymer, wherein the theoretical mass of the polymer is equal to the sum of the masses of the macromolecular diol, the boron ester diol, the diisocyanate and the polyol small molecules.

[0020] In step S1, optionally, the step of adding a catalyst to the mixed solution and stirring, and performing a polyaddition reaction under an inert atmosphere comprises: adding the catalyst to the mixed solution and stirring evenly, placing it in a nitrogen or argon atmosphere at 60 to 90° C. for a polyaddition reaction for 2 to 12 hours.

[0021] In step S2, optionally, the ultrasonic stirring step includes: ultrasonic stirring at room temperature for 1 to 3 hours.

[0022] Optionally, the temperature of the curing reaction is 60 to 90° C., and the time of the curing reaction is 6 to 24 hours.

[0023] The second aspect of the present invention provides a flexible conductive composite material based on boron ester dynamic covalent bonds, which is prepared by the preparation method of the flexible conductive composite material based on boron ester dynamic covalent bonds.

[0024] The third aspect of the present invention provides an application of the flexible conductive composite material based on boron ester dynamic covalent bonds in the preparation of flexible wearable sensors.

[0025] Beneficial effects:

[0026] The present invention uses a polyurethane glass body based on a boron ester dynamic covalent bond as a matrix material, and prepares the flexible conductive composite material based on a boron ester dynamic covalent bond by filling a conductive material, which effectively improves the stability between the conductive material and the matrix material and the uniformity of the conductive material distribution. The flexible conductive composite material has extremely strong self-healing ability and mechanical properties. When the material is broken, the self-healing under heating conditions hardly affects the original mechanical properties and sensing properties, and can be well adapted to application scenarios that require frequent stretching; when the material is discarded, it has a good degradation rate in a mixed solution of water and a polar solvent, and can efficiently and easily recycle the polyurethane glass body and the conductive material under mild conditions, and can realize efficient recycling and recycling of the resin matrix and the conductive material. Therefore, the recyclability of the flexible conductive composite material prepared by the present invention can greatly reduce electronic waste and its impact on the environment, and reduce manufacturing costs. At the same time, when the flexible conductive composite material is used to prepare a flexible wearable strain sensor, it has good electrochemical stability and signal response performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1This is a macroscopic picture of the flexible conductive composite material based on boron ester dynamic covalent bonds prepared in Example 1 of the present invention.

[0028] Figure 2 The relative resistance change of the flexible conductive composite material based on boron ester dynamic covalent bonds prepared in Example 1 of the present invention under different strains. DETAILED DESCRIPTION

[0029] The present invention provides a flexible conductive composite material based on boron ester dynamic covalent bonds and a preparation method and application thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] Unless otherwise defined, all technical terms and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0031] The embodiment of the present invention provides a method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds, comprising the steps of:

[0032] S1, dissolving a macromolecular diol, a boron ester diol and a diisocyanate in a polar organic solvent to form a mixed solution, adding a catalyst to the mixed solution and stirring, and performing a polyaddition reaction under an inert atmosphere to obtain a polymer solution;

[0033] S2. Adding a conductive material and a small molecule polyol to the polymer solution, after ultrasonic stirring, pouring it into a mold for curing reaction, removing the solvent, and obtaining the flexible conductive composite material based on boron ester dynamic covalent bonds.

[0034] In some embodiments, the macromolecular diol includes one or more of polyethylene glycol, polyester polyol, polypropylene glycol, polytetramethylene glycol, polycarbonate polyol, polycaprolactone polyol, and hydroxy-terminated polydimethylsiloxane.

[0035] In some embodiments, the borate diol has any one of the chemical structural formulas shown in Formulas (I) to (XI):

[0036]

[0037] In some embodiments, the diisocyanate is one or more of an aromatic diisocyanate, an aliphatic diisocyanate, and an alicyclic diisocyanate. Specifically, the diisocyanate may be selected from isophorone diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, etc., but is not limited thereto.

[0038] In some embodiments, the catalyst is selected from one or more of dimethylcyclohexylamine, dibutyltin dilaurate, a triazine trimerization catalyst, stannous octoate, and dibutyltin maleate, but is not limited thereto.

[0039] In some embodiments, the conductive material includes one or more of polyacetylene, polypyrrole, polyaniline, polythiophene, graphene, metal nanowires, metal nanoparticles, and carbon nanotubes, but is not limited thereto.

[0040] In some embodiments, the polyol small molecule includes one or more of glycerol, trimethylolpropane, hexanetriol, and pentaerythritol, but is not limited thereto.

[0041] In some embodiments, the molar ratio of the total amount of alcoholic hydroxyl groups contained in the macromolecular diol, borate ester diol and small molecular polyol to the isocyanate groups contained in the diisocyanate is 1:(0.9-1.4).

[0042] In some embodiments, the mass of the catalyst accounts for 0.05-5% of the theoretical mass of the polymer, and the mass of the conductive material accounts for 1-25% of the theoretical mass of the polymer, wherein the theoretical mass of the polymer is equal to the sum of the masses of the macromolecular diol, the boron ester diol, the diisocyanate and the polyol small molecule. The raw material components and their proportions involved in the process of preparing the flexible composite material in the embodiment of the present invention can be controlled and adjusted, so that the performance of the prepared flexible conductive composite material is controllable.

[0043] In step S1, in some embodiments, the step of adding a catalyst to the mixed solution and stirring, and performing a polyaddition reaction under an inert atmosphere includes: adding the catalyst to the mixed solution and stirring evenly, placing it in a nitrogen or argon atmosphere at 60 to 90° C. for a polyaddition reaction for 2 to 12 hours.

[0044] In step S2, in some embodiments, the ultrasonic stirring step includes: ultrasonic stirring at room temperature for 1 to 3 hours.

[0045] In some embodiments, the curing reaction temperature is 60 to 90° C., and the curing reaction time is 6 to 24 hours. Usually, the curing reaction is carried out in a polytetrafluoroethylene mold.

[0046] The embodiment of the present invention provides a flexible conductive composite material based on boric ester dynamic covalent bonds, which is prepared by the preparation method of the flexible conductive composite material based on boric ester dynamic covalent bonds. The flexible conductive composite material has extremely strong self-healing ability and mechanical properties. When the material is broken, it can self-heal under heating conditions, and almost does not affect the original mechanical properties and sensing properties, and can be well adapted to application scenarios that require frequent stretching; when discarded, the flexible conductive composite material has a good degradation rate in a water / polar solvent mixed solution, and can efficiently and easily recycle polyurethane glass and its conductive materials under mild conditions, thereby realizing efficient recycling and recycling of resin matrix and conductive materials. When used to prepare flexible wearable strain sensors, it has good electrochemical stability and signal response performance. Therefore, the recyclability of the flexible conductive composite material prepared by the present invention can greatly reduce electronic waste and its impact on the environment, and can also reduce manufacturing costs.

[0047] The embodiment of the present invention provides an application of the flexible conductive composite material based on boron ester dynamic covalent bonds in the preparation of a flexible wearable sensor. The flexible wearable sensor can be used as a strain or pressure sensor to monitor human breathing, heartbeat or movement.

[0048] The following describes it in detail through specific embodiments.

[0049] Example 1

[0050] 397 mg of borate diol (as shown in Formula VII), 600 mg of polyethylene glycol (PEG) (Mn=600) and 1167 g of isophorone diisocyanate were dissolved in 10 ml of N,N-dimethylformamide, 6 mg of dibutyltin dilaurate was added, and the mixture was stirred thoroughly to form a uniform solution, and the mixture was reacted at 70° C. under a nitrogen atmosphere for 6 hours to obtain a polyurethane solution;

[0051] 120 mg of carbon nanotubes and 221 mg of trimethylolpropane were added to the polyurethane solution, and ultrasonic stirring was performed at room temperature for 2 h to obtain a uniform solution; the uniform solution was poured into a polytetrafluoroethylene mold, and the reaction was continued at 80° C. for 6 h; and then the solvent was removed in vacuum at 90° C. for 12 h to obtain a flexible conductive composite material based on boron ester dynamic covalent bonds, such as Figure 1 As shown in Figure 2, the flexible conductive composite material has excellent mechanical properties after bending and stretching. The relative resistance change of the flexible conductive composite material under different strains was tested, and the results are shown in Figure 2. Figure 2 As shown, it can be concluded that the resistance / original resistance of the flexible conductive composite material increases with the increase of strain.

[0052] The prepared flexible conductive composite material was cut open and molded at 130℃ / 2MPa for 40 minutes. It was found that the damaged conductive composite material healed again, restoring its complete sensing ability and mechanical integrity. At the same time, the relative resistance change of the self-healed conductive composite material under different strains was tested, and the results were consistent with the original sample.

[0053] Recycling of flexible conductive composites

[0054] Immerse 2g of the material in 10ml DMF / H2O (v / v, 5:1), heat and stir at 120℃ for 3h, and the polymer matrix can be degraded into oligomers soluble in the degradation solution, and the carbon nanotubes sink to the bottom of the solution. Then the degraded solution and carbon nanotubes are mixed and transferred to the mold, heated in an oven at 100℃, and the solvent is completely removed after 3h to obtain a recycled conductive composite material sample. The relative resistance change of the recycled flexible conductive composite material under different strains is tested, and the results are consistent with the original sample.

[0055] Example 2

[0056] 520 mg of borate diol (as shown in Formula IV), 1000 mg of PEG (Mn=1000) and 882 g of hexamethylene diisocyanate were added to 12 ml of N,N-dimethylformamide, and 7 mg of dibutyltin dilaurate was added. The mixture was stirred thoroughly to form a uniform solution, and the mixture was reacted at 70° C. under a nitrogen atmosphere for 7 hours to obtain a polyurethane solution.

[0057] 200 mg of silver nanoparticles and 18.4 mg of glycerol were added to the polyurethane solution, and ultrasonic stirring was performed at room temperature for 2 h to obtain a uniform solution; the uniform solution was poured into a polytetrafluoroethylene mold, and the reaction was continued at 70°C for 8 h; then the solvent was removed in vacuum at 90°C for 18 h to obtain the flexible conductive composite material based on boron ester dynamic covalent bonds. The relative resistance change of the conductive composite material under different strains was tested.

[0058] The above-mentioned flexible conductive composite material was cut open and molded at 120℃ / 2.55MPa for 60 minutes. The damaged conductive composite material healed again and restored its complete sensing ability and mechanical integrity. At the same time, the relative resistance change of the self-healed conductive composite material under different strains was tested, and the results were consistent with the original sample.

[0059] Recycling of flexible conductive composites

[0060] Immerse 2g of flexible conductive composite material in 15ml DMF / H2O (v / v, 2:1), heat and stir at 125℃ for 2.5h, the polymer matrix can be degraded into oligomers soluble in the degradation solution, and the silver nanoparticles sink to the bottom of the solution. Then the degraded solution and silver nanoparticles are mixed and transferred to the mold, heated in an oven at 110℃, and the solvent is completely removed after 3h to obtain a recycled conductive composite material sample. At the same time, the relative resistance change of the recycled flexible conductive composite material under different strains is tested, and the results are consistent with the original sample.

[0061] Example 3

[0062] 397 mg of borate diol (as shown in Formula VII), 1000 mg of PEG (M n =1000) and 1167g of isophorone diisocyanate were dissolved in 15ml of N,N-dimethylformamide, 10mg of stannous octoate was added, and the mixture was stirred thoroughly to form a uniform solution, and the mixture was reacted at 80°C in a nitrogen atmosphere for 6h to obtain a polyurethane solution;

[0063] 210 mg of poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) and 170 mg of pentaerythritol were added to the polyurethane solution, and ultrasonic stirring was performed at room temperature for 2 hours to obtain a uniform solution; the uniform solution was poured into a polytetrafluoroethylene mold, and the reaction was continued at 80°C for 6 hours; then the solvent was removed in vacuum at 90°C for 12 hours to obtain the flexible conductive composite material based on boron ester dynamic covalent bonds. The relative resistance change of the flexible conductive composite material under different strains was tested.

[0064] The prepared flexible conductive composite material was cut open and molded at 120℃ / 1.5MPa for 60 minutes. The damaged conductive composite material healed again and restored its complete sensing ability and mechanical integrity. The relative resistance change of the self-healed conductive composite material under different strains was tested, and the results were consistent with the original sample.

[0065] Recycling of flexible conductive composites

[0066] Immerse 2g of the material in 10ml DMF / H2O (v / v, 4:1), heat and stir at 120℃ for 2h, and the polymer matrix can be degraded into oligomers soluble in the degradation solution. Then transfer the degraded solution to the mold and heat it to 90℃ in an oven. After 5h, the solvent is completely removed to obtain a recycled conductive composite material sample. The relative resistance change of the recycled conductive composite material under different strains is consistent with that of the original sample.

[0067] The flexible conductive composite material based on boron ester dynamic covalent bond prepared in Examples 1 to 3 is cut into rectangular strips, conductive silver paste is applied to both ends of the strips, and they are assembled with copper wires to obtain a wearable sensor. The flexible wearable sensor can be used as a strain or pressure sensor to monitor human breathing, heartbeat or movement.

[0068] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds, characterized in that: Includes steps: S1, dissolving a macromolecular diol, a boron ester diol and a diisocyanate in a polar organic solvent to form a mixed solution, adding a catalyst to the mixed solution and stirring, and performing a polyaddition reaction under an inert atmosphere to obtain a polymer solution; S2. Adding a conductive material and a small molecule polyol to the polymer solution, after ultrasonic stirring, pouring it into a mold for curing reaction, removing the solvent, and obtaining the flexible conductive composite material based on boron ester dynamic covalent bonds.

2. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to claim 1, characterized in that: The macromolecular diol includes one or more of polyethylene glycol, polyester polyol, polypropylene glycol, polytetramethylene glycol, polycarbonate polyol, polycaprolactone polyol, and hydroxy-terminated polydimethylsiloxane.

3. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to claim 1, characterized in that: The borate diol has any one of the chemical structural formulas shown in formula (I) to (XI):

4. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to claim 1, characterized in that: The diisocyanate is one or more of aromatic diisocyanate, aliphatic diisocyanate and alicyclic diisocyanate; the catalyst is one or more of dimethylcyclohexylamine, dibutyltin dilaurate, triazine trimerization catalyst, stannous octoate and dibutyltin maleate.

5. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to claim 1, characterized in that: The conductive material includes one or more of polyacetylene, polypyrrole, polyaniline, polythiophene, graphene, metal nanowires, metal nanoparticles and carbon nanotubes; the polyol small molecules include one or more of glycerol, trimethylolpropane, hexanetriol and pentaerythritol.

6. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to any one of claims 1 to 5, characterized in that: The molar ratio of the total amount of alcoholic hydroxyl groups contained in the macromolecular diol, the boric ester diol and the small molecule polyol to the isocyanate groups contained in the diisocyanate is 1:(0.9-1.4); the mass of the catalyst accounts for 0.05-5% of the theoretical mass of the polymer, and the mass of the conductive material accounts for 1-25% of the theoretical mass of the polymer, wherein the theoretical mass of the polymer is equal to the sum of the masses of the macromolecular diol, the boric ester diol, the diisocyanate and the small molecules of the polyol.

7. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to claim 1, characterized in that: In step S1, the step of adding a catalyst to the mixed solution and stirring, and performing a polyaddition reaction under an inert atmosphere comprises: adding the catalyst to the mixed solution and stirring evenly, placing the mixed solution in a nitrogen or argon atmosphere at 60 to 90° C. for a polyaddition reaction for 2 to 12 hours.

8. The method for preparing a flexible conductive composite material based on boron ester dynamic covalent bonds according to claim 1, characterized in that: In step S2, the ultrasonic stirring step includes: ultrasonic stirring at room temperature for 1 to 3 hours; and / or, the temperature of the curing reaction is 60 to 90° C., and the time of the curing reaction is 6 to 24 hours.

9. A flexible conductive composite material based on boron ester dynamic covalent bonds, characterized in that: The flexible conductive composite material is prepared by the preparation method of the boron ester dynamic covalent bond-based flexible conductive composite material according to any one of claims 1 to 8.

10. Use of the flexible conductive composite material based on boron ester dynamic covalent bonds as claimed in claim 9 in the preparation of flexible wearable sensors.

Citation Information

Patent Citations

  • Renewable polyurea-urethane based on dynamic covalent crosslinking of stable borate bonds, and preparation method and application thereof

    CN109897148A

  • Ultrafast self-healing polysaccharide-based hydrogel strain sensor and manufacturing method thereof

    CN112066866A

  • Preparation method of self-repairing thermosetting film based on multi-component Ugi polymerization reaction and dynamic oxime urethane bond exchange

    CN113121781A

  • Preparation method, regeneration method and application of linear boron ester bond polyurethane elastomer composite material

    CN115322324A

  • High-toughness cross-linked polyurethane capable of being reprocessed at room temperature and preparation method of high-toughness cross-linked polyurethane

    CN116396463A