Preparation method of antistatic polyester film
By introducing nickel-plated carbon nanotubes and aluminum units doped with zinc oxide nanopowders into the polyester film, a conductive layer and current network is formed, which solves the problem of easy damage to the electrostatic layer and improves the anti-static performance of the polyester film and long-term stability.
Patent Information
- Application Number
- CN202411046028.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing anti-static polyester film is prone to damage during long-term use, resulting in a gradual decrease in the anti-static effect and lack of long-term use performance.
Carbon nanotubes are used as matrix material, and blended with polyester material after electroless nickel plating layer, and combined with aluminum units doped with zinc oxide nanopowder to form a modified nanopowder, and a conductive layer is formed through swelling liquid treatment. Three-dimensional current network to improve conductivity and antistatic properties.
The stable conductivity and anti-static properties of the polyester film are achieved, ensuring the stability of the conductive layer during long-term use, and avoiding the substantial impact of the damage to the anti-static properties.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester film processing, in particular to a method for preparing an antistatic polyester film. Background Art
[0002] Polyester film has good comprehensive properties and is widely used in the fields of electronics, optics, etc. However, as a polymer insulating material, polyester film has a high resistivity and is prone to static electricity due to friction during production and use, which brings many inconveniences to the application of polyester film, especially when it is used in the field of electronics and electrical appliances. The electrostatic discharge phenomenon will cause semiconductor failure and affect product performance. Therefore, the antistatic modification of polyester film has very important practical significance. The antistatic property represents the property of discharging the charges accumulated on the surface of the insulating material by appropriate methods. In order to improve the antistatic properties of the polyester film, generally speaking, an antistatic layer or a conductive layer can be formed on the surface of the polyester film, or a conductive or antistatic substance (such as metal, carbon powder, antistatic agent, etc.) can be added to the polyester material matrix to effectively discharge the charges accumulated on the surface.
[0003] For example, the invention patent with announcement number CN116041770A discloses a method for preparing an antistatic polyester film, which adopts a suspended interface assembly method to achieve single-sided enrichment of conductive TiO2 and improve the utilization rate of conductive TiO2. The suspended interface assembly method achieves single-sided enrichment of conductive TiO2 particles, greatly improving the utilization efficiency of conductive TiO2, and its surface resistance can be reduced to 10 6 Ω / sq, under the same conductive TiO2 addition amount, it is reduced by 5 orders of magnitude compared with the melt blending method and the surface coating method. In addition, the surface hydrophilicity of the antistatic PET film is also greatly improved by the suspended interface modification, and the surface contact angle is reduced to 25°. The polyester film prepared by this method has excellent antistatic properties; since the technical solution is to form an electrostatic layer on the surface of the polyester film to achieve the antistatic effect, but the polyester film is not resistant to water washing, and in the long-term use process, it is affected by various factors, and the surface electrostatic layer is easily damaged and lost, which causes the antistatic effect of the polyester film to become worse and worse over time, and it does not have long-term performance. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a method for preparing an antistatic polyester film.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing an antistatic polyester film specifically comprises the following steps:
[0007] S1, blending the polyester matrix with the modified nano powder, and granulating to obtain a polyester masterbatch;
[0008] S2, melt-blending the polyester masterbatch, casting the sheet with a die head, longitudinally stretching, transversely stretching, and winding to obtain a semi-finished polyester film;
[0009] S3. Immerse the semi-finished polyester film in the swelling liquid at 80-90℃ for 20-50min. After taking it out, spray the treatment liquid evenly on the surface, place it in an oven, dry it at 95-98℃, and control the total air volume in the oven to 25000-30000m 3 / h, dry for 90-120s.
[0010] As a further preferred embodiment of the present invention, the mass ratio of the polyester matrix to the modified nanopowder is (75-85):(15-25).
[0011] As a further preferred embodiment of the present invention, the preparation method of the modified nanopowder is as follows:
[0012] 1) adding carbon nanotubes to a mixed solution of tin chloride and hydrochloric acid solution at 93-98° C. for sensitization for 45-60 min, adjusting the pH value to 2.0-2.5 with urea, filtering and washing, and drying to constant weight at 85-90° C., then placing in a nickel sulfate solution, soaking at room temperature for 10-30 min, washing with water, and reducing with potassium borohydride for 15-30 min, then immersing in a chemical plating solution, plating at 85-89° C. and pH 6.0-6.5 for 3-7 h, and drying to obtain modified carbon nanotubes;
[0013] 2) Dissolve zinc chloride and aluminum nitrate in deionized water, then add polyethylene glycol, stir at 300-500 r / min for 30-50 min to obtain a mixed solution, prepare a mixed alkali solution according to sodium hydroxide and sodium carbonate, and then add the mixed alkali solution dropwise to the mixed solution under magnetic stirring to ensure that the pH value is 7.5-8.5 during the reaction process, react at 60-65° C. for 2-5 h, after the reaction is completed, let the product stand for aging for 2-5 h, repeatedly wash with deionized water and dry to obtain a precursor powder;
[0014] 3) The precursor powder is placed in a tube furnace, kept at 300-350°C for 2-4 hours, then heated to 800-860°C, and kept for 2-4 hours. After naturally cooling to room temperature, the product is mixed with modified carbon nanotubes in a mass ratio of 1: (2-6) and ball milled for 2-5 hours to obtain modified nanopowder.
[0015] As a further preferred embodiment of the present invention, in step 1), the mass ratio of the tin chloride to the hydrochloric acid solution is 1:(3-5);
[0016] The concentration of the hydrochloric acid solution is 1-3 mol / L;
[0017] The concentration of the nickel sulfate solution is 0.2-0.5 mol / L;
[0018] The chemical plating solution consists of 25-30 g / L nickel sulfate, 20-26 g / L sodium dihydrogen phosphate, 15-18 g / L sodium citrate and 5-8 g / L sodium acetate.
[0019] As a further preferred embodiment of the present invention, in step 2), in the mixed solution, the ratio of zinc chloride, aluminum nitrate, deionized water, and polyethylene glycol is (10-16) g: (0.1-0.2) g: (80-130) mL: (0.2-0.5) g;
[0020] In the mixed alkaline solution, the molar ratio of sodium hydroxide to sodium carbonate is (2.0-2.6):1.
[0021] As a further preferred embodiment of the present invention, in step 3), the rotation speed of the ball mill is 120-180 r / min.
[0022] As a further preferred embodiment of the present invention, the swelling liquid is composed of toluene, p-xylene, m-xylene and 1,1,2,2-tetrachloroethane in a mass ratio of 1:(0.5-1.2):(0.2-0.7):(0.5-1.8).
[0023] As a further preferred embodiment of the present invention, the preparation method of the treatment liquid is as follows:
[0024] 1) adding multi-walled carbon nanotubes, a dispersant and ethyl acetate into a ball kettle and milling for 45-50 hours, then centrifuging in a centrifuge at a speed of 8000-10000 r / min for 5-10 minutes, taking the supernatant to obtain a multi-walled carbon nanotube dispersion;
[0025] 2) Add the silicone resin to toluene, stir and disperse evenly, then add the platinum catalyst and the multi-walled carbon nanotube dispersion, stir and disperse evenly.
[0026] As a further preferred embodiment of the present invention, in step 1), the ratio of the multi-walled carbon nanotubes, the dispersant, and ethyl acetate is (4-9) g: (4.5-9.8) g: (400-600) mL;
[0027] The dispersant is composed of dispersant BYK-2155 and dispersant BYK-9076 in a mass ratio of (4-9): (0.5-0.8);
[0028] The centrifugal speed is 8000-10000r / min.
[0029] As a further preferred embodiment of the present invention, in step 2), the usage ratio of the silicone resin, toluene, platinum catalyst, and multi-walled carbon nanotube dispersion is (5-10) g: (5-10) mL: (0.1-0.3) g: (2-5) mL.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] In the present invention, carbon nanotubes are used as a matrix material, and a nickel layer is plated on the surface thereof by chemical plating to obtain modified carbon nanotubes. The plated metal nickel layer gives the matrix material stable electrical conductivity, and is introduced into the polyester material, so that the polyester material has good electrical conductivity. At the same time, since the filled modified carbon nanotubes have a large aspect ratio, the percolation threshold of the polyester material is reduced, so that it has good antistatic properties. Moreover, the modified carbon nanotubes form three-dimensional contact in the polyester material, construct a conductive network, and form a parallel structure with the polyester material. The current will preferentially flow along the modified carbon nanotubes with low resistance and bypass the polyester material matrix with high resistance. The modified carbon nanotubes The three-dimensional current network chain formed plays a controlling role in the conductivity of the overall system, thereby greatly improving the conductivity of the polyester material and making it have a good antistatic effect; at the same time, in the present invention, a chemical coprecipitation method is also used to obtain a nano powder of aluminum unit doped zinc oxide, and it is physically combined with the modified carbon nanotubes by ball milling. By doping aluminum units in zinc oxide, the nano powder presents a hexagonal wurtzite structure with good crystallinity, and with the appropriate increase in the doping amount of aluminum units, the electrical properties of the nano powder are improved, so that after being combined with the modified carbon nanotubes, it can present more excellent electrical properties and be introduced into the polyester material to significantly improve its antistatic performance.
[0032] At the same time, in order to further enhance the antistatic properties of polyester materials, in the present invention, a small-diameter multi-walled carbon nanotube dispersion is used as a conductive functional body, and a silicone resin is used as a matrix material to prepare a treatment liquid. After the surface of the polyester film is swelled by a swelling agent, the substances in the treatment liquid can penetrate into the surface layer of the polyester film to form a conductive layer, thereby reducing the surface resistance of the polyester film and achieving an antistatic effect, so that the polyester film has a more excellent antistatic effect.
[0033] In the present invention, modified nanopowders with conductivity are introduced into the polyester material, and a conductive layer is formed in the surface layer thereof, so that the formed polyester film has good conductivity and low resistance, thereby having an antistatic effect. Moreover, during long-term use, even if the conductive layer on the surface is damaged or lost, it will not have a substantial impact on the antistatic property, and the polyester film can still be used normally. DETAILED DESCRIPTION
[0034] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] A method for preparing an antistatic polyester film specifically comprises the following steps:
[0037] S1. Blending the polyester matrix and the modified nano powder in a mass ratio of 75:25, and granulating to obtain a polyester masterbatch;
[0038] S2, melt-blending the polyester masterbatch, casting the sheet with a die head, longitudinally stretching, transversely stretching, and winding to obtain a semi-finished polyester film;
[0039] S3. Immerse the semi-finished polyester film in the swelling liquid at 80°C for 20 minutes. After taking it out, spray the treatment liquid evenly on the surface, place it in an oven, dry it at 95°C, and control the total air volume in the oven to 25000m 3 / h, dry for 90s;
[0040] The swelling liquid is composed of toluene, p-xylene, m-xylene and 1,1,2,2-tetrachloroethane in a mass ratio of 1:0.5:0.2:0.5.
[0041] The preparation method of the modified nanopowder is as follows:
[0042] 1) Add carbon nanotubes to a mixed solution of tin chloride and 1 mol / L hydrochloric acid solution at 93°C for sensitization for 45 minutes, wherein the mass ratio of tin chloride to hydrochloric acid solution is 1:3, and urea is used to adjust the pH value to 2.0. After filtering, washing, and drying to constant weight at 85°C, the carbon nanotubes are placed in a 0.2 mol / L nickel sulfate solution and soaked at room temperature for 10 minutes. After washing with water, the carbon nanotubes are reduced with potassium borohydride for 15 minutes, and then immersed in a chemical plating solution. The carbon nanotubes are plated at 85°C and pH 6.0 for 3 hours, and then dried to obtain modified carbon nanotubes;
[0043] The chemical plating solution is composed of 25 g / L nickel sulfate, 20 g / L sodium dihydrogen phosphate, 15 g / L sodium citrate and 5 g / L sodium acetate;
[0044] 2) Dissolve 10g zinc chloride and 0.1g aluminum nitrate in 80mL deionized water, then add 0.2g polyethylene glycol, stir at 300r / min for 30min to obtain a mixed solution, prepare a mixed alkali solution according to the molar ratio of sodium hydroxide to sodium carbonate of 2:1, and then add the mixed alkali solution dropwise to the mixed solution under magnetic stirring to ensure that the pH value is 7.5 during the reaction, react at 60°C for 2h, and after the reaction is completed, let the product stand for 2h, wash it repeatedly with deionized water and dry it to obtain a precursor powder;
[0045] 3) The precursor powder is placed in a tube furnace, kept at 300°C for 2 hours, then heated to 800°C, and kept at this temperature for another 2 hours. After naturally cooling to room temperature, the product is mixed with modified carbon nanotubes in a mass ratio of 1:2 and ball milled at a rotation speed of 120 r / min for 2 hours to obtain modified nanopowder.
[0046] The preparation method of the treatment solution is as follows:
[0047] 1) 4 g of multi-walled carbon nanotubes, 4 g of dispersant BYK-2155, 0.5 g of dispersant BYK-9076 and 400 mL of ethyl acetate were added to a ball kettle and ball-milled for 45 h, and then centrifuged at 8000 r / min for 5 min in a centrifuge to obtain a multi-walled carbon nanotube dispersion;
[0048] 2) Add 5 g of silicone resin into 5 mL of toluene, stir thoroughly to disperse evenly, then add 0.1 g of platinum catalyst and 2 mL of multi-walled carbon nanotube dispersion, stir thoroughly to disperse evenly.
[0049] Example 2
[0050] A method for preparing an antistatic polyester film specifically comprises the following steps:
[0051] S1, blending the polyester matrix and the modified nano powder in a mass ratio of 80:20, and granulating to obtain a polyester masterbatch;
[0052] S2, melt-blending the polyester masterbatch, casting the sheet with a die head, longitudinally stretching, transversely stretching, and winding to obtain a semi-finished polyester film;
[0053] S3. Immerse the semi-finished polyester film in the swelling liquid at 85°C for 35 minutes. After taking it out, spray the treatment liquid evenly on the surface, place it in an oven, dry it at 96°C, and control the total air volume in the oven to 28,000m 3 / h, dry for 110s;
[0054] The swelling liquid is composed of toluene, p-xylene, m-xylene and 1,1,2,2-tetrachloroethane in a mass ratio of 1:0.7:0.5:1.3.
[0055] The preparation method of the modified nanopowder is as follows:
[0056] 1) Add carbon nanotubes to a mixed solution of tin chloride and 2 mol / L hydrochloric acid solution at 95°C for sensitization for 55 min, the mass ratio of tin chloride to hydrochloric acid solution is 1:4, urea is used to adjust the pH value to 2.5, filtered and washed, and dried at 87°C to constant weight, and then placed in a 0.3 mol / L nickel sulfate solution, soaked at room temperature for 20 min, washed with water, reduced with potassium borohydride for 25 min, and then immersed in a chemical plating solution, treated with the plating solution at 86°C and pH 6.5 for 5 h, and dried to obtain modified carbon nanotubes;
[0057] The chemical plating solution is composed of 27 g / L nickel sulfate, 23 g / L sodium dihydrogen phosphate, 17 g / L sodium citrate and 7 g / L sodium acetate;
[0058] 2) Dissolve 15g zinc chloride and 0.2g aluminum nitrate in 120mL deionized water, then add 0.3g polyethylene glycol, stir at 400r / min for 40min to obtain a mixed solution, prepare a mixed alkali solution according to the molar ratio of sodium hydroxide to sodium carbonate of 2.3:1, and then add the mixed alkali solution dropwise to the mixed solution under magnetic stirring to ensure that the pH value is 8 during the reaction, react at 63°C for 3h, and after the reaction is completed, let the product stand for 3h, wash repeatedly with deionized water and dry to obtain a precursor powder;
[0059] 3) The precursor powder is placed in a tubular furnace, kept at 320°C for 3 hours, then heated to 850°C, and kept for 3 hours. After naturally cooling to room temperature, the product is mixed with modified carbon nanotubes in a mass ratio of 1:5 and ball milled at a rotation speed of 150 r / min for 3 hours to obtain modified nanopowder.
[0060] The preparation method of the treatment solution is as follows:
[0061] 1) 7 g of multi-walled carbon nanotubes, 7 g of dispersant BYK-2155, 0.7 g of dispersant BYK-9076 and 500 mL of ethyl acetate were added to a ball kettle and ball-milled for 46 h, and then centrifuged at 9000 r / min for 7 min in a centrifuge to obtain a multi-walled carbon nanotube dispersion;
[0062] 2) 8 g of silicone resin was added to 8 mL of toluene, and the mixture was stirred thoroughly to disperse the mixture evenly. Then, 0.2 g of platinum catalyst and 3 mL of multi-walled carbon nanotube dispersion were added, and the mixture was stirred thoroughly to disperse the mixture evenly.
[0063] Example 3
[0064] A method for preparing an antistatic polyester film specifically comprises the following steps:
[0065] S1. Blending the polyester matrix and the modified nano powder in a mass ratio of 85:15, and granulating to obtain a polyester masterbatch;
[0066] S2, melt-blending the polyester masterbatch, casting the sheet with a die head, longitudinally stretching, transversely stretching, and winding to obtain a semi-finished polyester film;
[0067] S3. Immerse the semi-finished polyester film in the swelling liquid at 90°C for 50 minutes. After taking it out, spray the treatment liquid evenly on the surface, place it in an oven, dry it at 98°C, and control the total air volume in the oven to 30,000m 3 / h, dry for 120s;
[0068] The swelling liquid is composed of toluene, p-xylene, m-xylene and 1,1,2,2-tetrachloroethane in a mass ratio of 1:1.2:0.7:1.8.
[0069] The preparation method of the modified nanopowder is as follows:
[0070] 1) adding carbon nanotubes to a mixed solution of tin chloride and 3 mol / L hydrochloric acid solution at 98°C for sensitization for 60 min, wherein the mass ratio of tin chloride to hydrochloric acid solution is 1:5, adjusting the pH value to 2.5 with urea, filtering and washing, and drying at 90°C to constant weight, and then placing in a 0.5 mol / L nickel sulfate solution, soaking at room temperature for 30 min, washing with water, and reducing with potassium borohydride for 30 min, and then immersing in a chemical plating solution, plating at 89°C and pH 6.5 for 7 h, and drying to obtain modified carbon nanotubes;
[0071] The chemical plating solution is composed of 30 g / L nickel sulfate, 26 g / L sodium dihydrogen phosphate, 18 g / L sodium citrate and 8 g / L sodium acetate;
[0072] 2) Dissolve 16g zinc chloride and 0.2g aluminum nitrate in 130mL deionized water, then add 0.5g polyethylene glycol, stir at 500r / min for 50min to obtain a mixed solution, prepare a mixed alkali solution according to the molar ratio of sodium hydroxide to sodium carbonate of 2.6:1, and then add the mixed alkali solution dropwise to the mixed solution under magnetic stirring to ensure that the pH value is 8.5 during the reaction, react at 65°C for 5h, and after the reaction is completed, let the product stand for 5h, wash it repeatedly with deionized water and dry it to obtain a precursor powder;
[0073] 3) The precursor powder is placed in a tubular furnace, kept at 350°C for 4 hours, then heated to 860°C, and kept at this temperature for another 4 hours. After naturally cooling to room temperature, the product is mixed with modified carbon nanotubes in a mass ratio of 1:6 and ball milled at a rotation speed of 180 r / min for 5 hours to obtain modified nanopowder.
[0074] The preparation method of the treatment solution is as follows:
[0075] 1) 9 g of multi-walled carbon nanotubes, 9 g of dispersant BYK-2155, 0.8 g of dispersant BYK-9076 and 600 mL of ethyl acetate were added to a ball kettle and ball-milled for 50 h, and then centrifuged at 10000 r / min for 10 min in a centrifuge to obtain a multi-walled carbon nanotube dispersion;
[0076] 2) Add 10 g of silicone resin into 10 mL of toluene, stir thoroughly to disperse evenly, then add 0.3 g of platinum catalyst and 5 mL of multi-walled carbon nanotube dispersion, stir thoroughly to disperse evenly.
[0077] Comparative Example 1: This comparative example is basically the same as Example 1, except that it does not contain modified nanopowder.
[0078] Comparative Example 2: This comparative example is basically the same as Example 1, except that step 1) is omitted in the preparation of the modified nanopowder.
[0079] Comparative Example 3: This comparative example is basically the same as Example 1, except that step 2) is omitted in the preparation of the modified nanopowder.
[0080] Comparative Example 4: This comparative example is substantially the same as Example 1, except that it does not contain a treatment liquid.
[0081] Comparative Example 5: This comparative example is basically the same as Example 1, except that step 1) is omitted in the preparation of the treatment solution.
[0082] Test experiment:
[0083] The methods provided in Examples 1-3 and Comparative Examples 1-5 were used to obtain antistatic polyester film samples, and then the antistatic properties of the samples were tested. The specific results are shown in Table 1.
[0084] For the antistatic test, the antistatic polyester film sample was placed in an antistatic tester (Mitsubishi Corporation, MCP-T600) at a temperature of 23° C. and a humidity of 50% RH, and then its surface resistance was measured based on JIS K7194.
[0085] Table 1
[0086] Example 1 Example 2 Example 3 Comparative Example 1 Surface resistance Ω / sq <![CDATA[4.15×10 4 ]]> <![CDATA[4.06×10 4 ]]> <![CDATA[4.11×10 4 ]]> <![CDATA[3.68×10 8 ]]> Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 Surface resistance Ω / sq <![CDATA[5.23×10 6 ]]> <![CDATA[6.89×10 6 ]]> <![CDATA[8.57×10 5 ]]> <![CDATA[7.02×10 5 ]]>
[0087] It can be seen from Table 1 that the antistatic polyester film prepared in the present invention has the characteristic of low surface resistance and can show excellent antistatic performance.
[0088] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for preparing an antistatic polyester film, characterized in that: The specific steps include: S1, blending the polyester matrix with the modified nano powder, and granulating to obtain a polyester masterbatch; S2, melt-blending the polyester masterbatch, casting the sheet with a die head, longitudinally stretching, transversely stretching, and winding to obtain a semi-finished polyester film; S3. Immerse the semi-finished polyester film in the swelling liquid at 80-90℃ for 20-50min. After taking it out, spray the treatment liquid evenly on the surface, place it in an oven, dry it at 95-98℃, and control the total air volume in the oven to 25000-30000m 3 / h, dry for 90-120s.
2. The method for preparing an antistatic polyester film according to claim 1, characterized in that: The mass ratio of the polyester matrix to the modified nano powder is (75-85): (15-25).
3. The method for preparing an antistatic polyester film according to claim 1, characterized in that: The preparation method of the modified nano powder is as follows: 1) adding carbon nanotubes to a mixed solution of tin chloride and hydrochloric acid solution at 93-98° C. for sensitization for 45-60 min, adjusting the pH value to 2.0-2.5 with urea, filtering and washing, and drying to constant weight at 85-90° C., then placing in a nickel sulfate solution, soaking at room temperature for 10-30 min, washing with water, and reducing with potassium borohydride for 15-30 min, then immersing in a chemical plating solution, plating at 85-89° C. and pH 6.0-6.5 for 3-7 h, and drying to obtain modified carbon nanotubes; 2) Dissolve zinc chloride and aluminum nitrate in deionized water, then add polyethylene glycol, stir at 300-500 r / min for 30-50 min to obtain a mixed solution, prepare a mixed alkali solution according to sodium hydroxide and sodium carbonate, and then add the mixed alkali solution dropwise to the mixed solution under magnetic stirring to ensure that the pH value is 7.5-8.5 during the reaction process, react at 60-65° C. for 2-5 h, after the reaction is completed, let the product stand for aging for 2-5 h, repeatedly wash with deionized water and dry to obtain a precursor powder; 3) The precursor powder is placed in a tube furnace, kept at 300-350°C for 2-4 hours, then heated to 800-860°C, and kept for 2-4 hours. After naturally cooling to room temperature, the product is mixed with modified carbon nanotubes in a mass ratio of 1: (2-6) and ball milled for 2-5 hours to obtain modified nanopowder.
4. The method for preparing an antistatic polyester film according to claim 3, characterized in that: In step 1), the mass ratio of the tin chloride to the hydrochloric acid solution is 1:(3-5); The concentration of the hydrochloric acid solution is 1-3 mol / L; The concentration of the nickel sulfate solution is 0.2-0.5 mol / L; The chemical plating solution consists of 25-30 g / L nickel sulfate, 20-26 g / L sodium dihydrogen phosphate, 15-18 g / L sodium citrate and 5-8 g / L sodium acetate.
5. The method for preparing an antistatic polyester film according to claim 3, characterized in that: In step 2), in the mixed solution, the ratio of zinc chloride, aluminum nitrate, deionized water, and polyethylene glycol is (10-16) g: (0.1-0.2) g: (80-130) mL: (0.2-0.5) g; In the mixed alkaline solution, the molar ratio of sodium hydroxide to sodium carbonate is (2.0-2.6):
1.
6. The method for preparing an antistatic polyester film according to claim 3, characterized in that: In step 3), the rotation speed of the ball mill is 120-180 r / min.
7. The method for preparing an antistatic polyester film according to claim 1, characterized in that: The swelling liquid is composed of toluene, p-xylene, m-xylene and 1,1,2,2-tetrachloroethane in a mass ratio of 1:(0.5-1.2):(0.2-0.7):(0.5-1.8).
8. The method for preparing an antistatic polyester film according to claim 1, characterized in that: The preparation method of the treatment solution is as follows: 1) adding multi-walled carbon nanotubes, a dispersant and ethyl acetate into a ball kettle and milling for 45-50 hours, then centrifuging in a centrifuge at a speed of 8000-10000 r / min for 5-10 minutes, taking the supernatant to obtain a multi-walled carbon nanotube dispersion; 2) Add the silicone resin to toluene, stir and disperse evenly, then add the platinum catalyst and the multi-walled carbon nanotube dispersion, stir and disperse evenly.
9. The method for preparing an antistatic polyester film according to claim 8, characterized in that: In step 1), the ratio of the multi-walled carbon nanotubes, the dispersant, and ethyl acetate is (4-9) g: (4.5-9.8) g: (400-600) mL; The dispersant is composed of dispersant BYK-2155 and dispersant BYK-9076 in a mass ratio of (4-9): (0.5-0.8); The centrifugal speed is 8000-10000r / min.
10. The method for preparing an antistatic polyester film according to claim 8, characterized in that: In step 2), the usage ratio of the silicone resin, toluene, platinum catalyst, and multi-walled carbon nanotube dispersion is (5-10) g: (5-10) mL: (0.1-0.3) g: (2-5) mL.
Citation Information
Patent Citations
Wide band electromagnetic wave-shielded polyethylene compound film containing nickel-plating carbon nanotube and preparation method thereof
CN101362389A
Antistatic polyester film and preparation method thereof
CN116426020A
Antistatic modified polyester film and preparation method thereof
CN116874861A
Flexible foam piezoresistive touch sensor, preparation method and pressure imaging system
CN117889996A
Polyester composition
JP2004263123A