Low-cost secondary vulcanized black rubber sole and preparation method thereof

By adopting low-cost secondary vulcanized black rubber sole formula and specific processes, the problems of high cost and poor process performance of rubber soles of rubber shoes are solved, and the sole preparation with full patterns, clear appearance and durable appearance is achieved, reducing production costs and Improved competitiveness.

CN118956029APending Publication Date: 2024-11-15JIHUA 3537 SHOE MAKING
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411281341.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing rubber shoes have high cost, and while pursuing durability, it is difficult to achieve both excellent process performance and low cost, resulting in problems such as lack of rubber patterns, poor appearance, and unstable soles during the production process.

Method used

A low-cost secondary vulcanized black rubber sole formula is adopted, including 65 to 70 parts of natural rubber, 30 to 35 parts of butadiene rubber, 3.0 to 3.4 parts of sulfur, 12 to 14 parts of vulcanization accelerator, 4.5 to 5.5 parts of nano-oxidation Zinc and other components, and through specific refining and pressing processes, it can achieve automatic exhaust, full patterns and clear appearance sole preparation.

Benefits of technology

It reduces production costs, improves product quality, ensures the durability and appearance of the sole, reduces market competition pressure, and achieves the production advantages of simple process, low energy consumption and low labor and labor investment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005041717740000061
    Figure BDA0005041717740000061
  • Figure BDA0005041717740000071
    Figure BDA0005041717740000071
  • Figure BDA0005041717740000072
    Figure BDA0005041717740000072
Patent Text Reader

Abstract

The invention discloses a low-cost secondary vulcanized black rubber sole and a preparation method thereof. The wear-resistant rubber is prepared from the following raw materials in parts by weight: 65-70 parts of natural rubber, 30-35 parts of butadiene rubber, 3.0-3.4 parts of sulfur, 12-14 parts of a vulcanization accelerator, 4.5-5.5 parts of nano zinc oxide, 2-3 parts of stearic acid, 1.5-2.5 parts of a rubber internal release agent, 2-3 parts of a wear-resistant agent, 13-17 parts of white carbon black, 3.6-4.0 parts of an anti-aging agent, 14-16 parts of a rubber softener, 0.8-1.2 parts of a homogenizing tear-resistant agent, 490-510 parts of regenerated rubber and 46-50 parts of medium super wear-resistant carbon black. According to the product obtained through the method, the mold filling effect is directly achieved through the rubber sole and the rubber body, patterns are full and clear, and rubber exhaust attachments are thoroughly eliminated. The natural rubber does not need to be plastified, so that the method is simple in process, low in production energy consumption, low in labor input and small in occupied space. Due to the adoption of a large dose of high-strength reclaimed rubber, the production cost is reduced, and the market competition pressure is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a low-cost secondary vulcanized black rubber sole and a preparation method thereof, belonging to the technical field of shoemaking. Background Art

[0002] In the production process of rubber shoes, the rubber soles consume a lot of rubber, and the price accounts for more than 30% of the total cost. For enterprises pursuing maximum profits, reducing the cost of soles is an important way to ensure that the durability of rubber shoes meets the requirements of national industry standards.

[0003] Generally speaking, to achieve the effect of low cost and excellent process performance of rubber sole components of rubber shoes, there will be the following interference factors. First, due to the performance requirements of rubber shoes, the proportion of natural rubber used in the sole rubber is relatively high, and the cost of functional additives is still high. Second, the rubber material is limited by the roller sticking or roller-off performance in the rubber refining process, which increases the difficulty of making rubber materials.

[0004] Controlling the comprehensive performance of rubber is a necessary measure to achieve normal rubber making process and stable performance that meets standards. In the process of making the sole, the mold pattern is not fully vented, causing the sole to lack glue and have a poor appearance. In order to ensure that the pattern is not lacking glue and the pattern of the rubber nails is clear and full, it is forced to drill glue flow holes at the position where the pattern lacks glue. The soles made in this way have rubber nails, which are extra attachments and have a poor appearance. At the same time, due to the limited working pressure of the sole pressing machine, rubber with relatively high plasticity must be used to make the sole, which leads to the bad result that the sole is not stiff and there is a lot of glue flowing on the edge, which will not only affect the appearance quality, but also seriously affect the production process due to abnormal process.

[0005] At present, enterprises need a rubber sole with normal process, low cost, stable performance and optimized processing method to enhance the competitiveness of rubber shoe enterprises. Summary of the invention

[0006] The purpose of the present invention is to provide a low-cost secondary vulcanized black rubber sole and a preparation method thereof, so as to overcome the shortcomings of the prior art.

[0007] The technical solution of the present invention is as follows: a low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 65-70 parts of natural rubber, 30-35 parts of butadiene rubber, 3.0-3.4 parts of sulfur, 12-14 parts of vulcanization accelerator, 4.5-5.5 parts of nano zinc oxide, 2-3 parts of stearic acid, 1.5-2.5 parts of rubber internal mold release agent, 2-3 parts of wear-resistant agent, 13-17 parts of white carbon black, 3.6-4.0 parts of antioxidant, 14-16 parts of rubber softener, 0.8-1.2 parts of homogenized tear-resistant agent, 490-510 parts of recycled rubber, and 46-50 parts of medium and super wear-resistant carbon black.

[0008] The aforementioned low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 part of homogenizing anti-tear agent, 500 parts of recycled rubber, and 48 parts of super wear-resistant carbon black.

[0009] In the aforementioned low-cost secondary vulcanized black rubber sole, the raw materials further include: 0.4-0.6 parts of scorch retarder and 0.1-0.2 parts of peptizer.

[0010] In the aforementioned low-cost secondary vulcanized black rubber sole, the vulcanization accelerator is composed of 2 parts of accelerator DM, 9 parts of accelerator CZ and 2 parts of accelerator DS per 13 parts of vulcanization accelerator.

[0011] In the aforementioned low-cost secondary vulcanized black rubber sole, the rubber softener is composed of 5 parts of solid coumarone and 10 parts of rubber softening oil per 15 parts of rubber softener.

[0012] A low-cost method for preparing secondary vulcanized black rubber soles comprises the following steps:

[0013] (1) Ingredients: natural rubber and cis-1,4-butadiene rubber are mixed to obtain product A; super wear-resistant carbon black is prepared to obtain product B; vulcanization accelerator and nano zinc oxide, rubber internal mold release agent, wear-resistant agent, white carbon black, antioxidant, homogenizing anti-tearing agent, recycled rubber, anti-scorch agent, peptizer, and stearic acid are mixed to obtain product C;

[0014] (2) Refining sulfur-free rubber mix: Put product A into a rubber mixer, and refine it for 0.5 to 1 minute at a temperature of 80 to 125°C and a pressure of 0.34 to 0.38 MPa. Then, add product B, product C and half of the rubber softener, and continue refining for 4 to 5 minutes. Then, add the other half of the rubber softener and continue refining until the material is uniform and free of powder to obtain a semi-finished mixed product. The semi-finished mixed product is discharged to an open rubber mixer for additional refining to make the material fully dispersed and uniform to obtain a rubber mix. The rubber mix is ​​made into a 7 to 8 mm film, and then the film is soaked in a release agent liquid, and then the moisture on the film is air-dried by a fan;

[0015] (3) Manufacturing secondary vulcanized black rubber sole glue: putting the air-dried rubber sheet into an open mill and refining it until it is smooth, adding sulfur, refining it evenly, and finally pressing it into sheets of the desired thickness to obtain secondary vulcanized black sole rubber blocks;

[0016] (4) After obtaining the secondary vulcanized black sole rubber block, place it in a sole mold without glue flow holes at 165-172° C. on a pressing machine with a working pressure of 200 tons for hot vulcanization for 2.5-3 minutes, take the sole out of the mold, trim off the flow glue, and obtain the secondary vulcanized black rubber sole.

[0017] Beneficial effects of the present invention: Compared with the prior art, the secondary vulcanized black rubber sole and its preparation method of the present invention have the following characteristics: (1) The rubber can be automatically vented to eliminate bubbles, saving the mold surface from sandblasting, and reducing production costs. (2) The sole pattern is full and clear in appearance, eliminating the vulcanized rubber nails generated by the mold glue flow holes and the lack of glue in the sole pattern caused by the colloid filling not being in place. (3) The production process is normal and the cost is at an advantageous level, which improves the product quality.

[0018] The shoe sole prepared by the formula and preparation method of the present invention has a Shore A degree of 58-63, a tensile strength of 9.0-10.5 MPa, an elongation at break of 380-150%, and an Akron abrasion of 0.65-0.85 cm 3 , ensuring the product's wear resistance. Since recycled rubber is the main component, the cost of rubber soles is at a relatively low level, which improves the competitiveness of producers. The product obtained by the present invention directly realizes the mold filling effect of the rubber sole and the rubber body, achieves a full and clear pattern, and completely eliminates rubber exhaust attachments. Since there is no need to plasticize natural rubber, this method has a simple process, low production energy consumption, low labor input, and less space occupied. The use of large doses of high-strength recycled rubber reduces production costs and reduces market competition pressure. DETAILED DESCRIPTION

[0019] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.

[0020] Embodiment 1 of the present invention: A low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 part of homogenizing tear-resistant agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black, 0.5 parts of anti-scorch agent, and 0.15 parts of plasticizer.

[0021] Embodiment 2 of the present invention: A low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 65 parts of natural rubber, 30 parts of butadiene rubber, 3.0 parts of sulfur, 12 parts of vulcanization accelerator, 4.5 parts of nano zinc oxide, 2 parts of stearic acid, 1.5 parts of rubber internal mold release agent, 2 parts of wear-resistant agent, 13 parts of white carbon black, 3.6 parts of antioxidant, 14 parts of rubber softener, 0.8 parts of homogenizing tear-resistant agent, 490 parts of recycled rubber, 46 parts of medium and super wear-resistant carbon black, 0.4 parts of anti-scorch agent, and 0.10 parts of plasticizer.

[0022] Embodiment 3 of the present invention: A low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 70 parts of natural rubber, 35 parts of butadiene rubber, 3.4 parts of sulfur, 14 parts of vulcanization accelerator, 5.5 parts of nano zinc oxide, 3 parts of stearic acid, 2.5 parts of rubber internal mold release agent, 3 parts of wear-resistant agent, 17 parts of white carbon black, 4.0 parts of antioxidant, 16 parts of rubber softener, 1.2 parts of homogenized tear-resistant agent, 510 parts of recycled rubber, 50 parts of medium and super wear-resistant carbon black, 0.6 parts of anti-scorch agent, and 0.20 parts of plasticizer.

[0023] Embodiment 4 of the present invention: A low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 66 parts of natural rubber, 32 parts of butadiene rubber, 3.1 parts of sulfur, 13 parts of vulcanization accelerator, 4.8 parts of nano zinc oxide, 2.5 parts of stearic acid, 1.8 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 14 parts of white carbon black, 3.7 parts of antioxidant, 15 parts of rubber softener, 0.9 parts of homogenized tear-resistant agent, 495 parts of recycled rubber, 47 parts of medium and super wear-resistant carbon black, 0.5 parts of anti-scorch agent, and 0.18 parts of plasticizer.

[0024] Embodiment 5 of the present invention: A low-cost secondary vulcanized black rubber sole is made of the following raw materials in parts by weight: 69 parts of natural rubber, 34 parts of butadiene rubber, 3.3 parts of sulfur, 14 parts of vulcanization accelerator, 5.2 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.2 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 16 parts of white carbon black, 3.9 parts of antioxidant, 15 parts of rubber softener, 1.1 parts of homogenized tear-resistant agent, 505 parts of recycled rubber, 49 parts of medium and super wear-resistant carbon black, 0.6 parts of anti-scorch agent, and 0.20 parts of plasticizer.

[0025] In the above embodiment, the vulcanization accelerator is composed of 2 parts of accelerator DM, 9 parts of accelerator CZ and 2 parts of accelerator DS per 13 parts of vulcanization accelerator; the rubber softener is composed of 5 parts of solid coumarone and 10 parts of rubber softening oil per 15 parts of rubber softener.

[0026] The low-cost preparation method of the secondary vulcanized black rubber sole of the above embodiment comprises the following steps:

[0027] (1) Ingredients: natural rubber and cis-1,4-butadiene rubber are mixed to obtain product A; super wear-resistant carbon black is prepared to obtain product B; vulcanization accelerator and nano zinc oxide, rubber internal mold release agent, wear-resistant agent, white carbon black, antioxidant, homogenizing anti-tearing agent, recycled rubber, anti-scorch agent, peptizer, and stearic acid are mixed to obtain product C;

[0028] (2) Refining sulfur-free rubber mix: Put product A into a rubber mixer, and refine it for 0.5 to 1 minute at a temperature of 80 to 125°C and a pressure of 0.34 to 0.38 MPa. Then, add product B, product C and half of the rubber softener, and continue refining for 4 to 5 minutes. Then, add the other half of the rubber softener and continue refining until the material is uniform and free of powder to obtain a semi-finished mixed product. The semi-finished mixed product is discharged to an open rubber mixer for additional refining to make the material fully dispersed and uniform to obtain a rubber mix. The rubber mix is ​​made into a 7 to 8 mm film, and then the film is soaked in a release agent liquid, and then the moisture on the film is air-dried by a fan;

[0029] (3) Manufacturing secondary vulcanized black rubber sole glue: putting the air-dried rubber sheet into an open mill and refining it until it is smooth, adding sulfur, refining it evenly, and finally pressing it into sheets of the desired thickness to obtain secondary vulcanized black sole rubber blocks;

[0030] (4) After obtaining the secondary vulcanized black sole rubber block, place it in a sole mold without glue flow holes at 165-172° C. on a pressing machine with a working pressure of 200 tons for hot vulcanization for 2.5-3 minutes, take the sole out of the mold, trim off the flow glue, and obtain the secondary vulcanized black rubber sole.

[0031] During the process of the present invention, the performance of the product was tested and the following formula screening test was performed to verify the technical solution of the present invention:

[0032] Formula test data:

[0033] Formula: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal release agent, 2.5 parts of wear-resistant agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 part of homogenizing anti-tear agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black, 0.5 parts of anti-scorch agent, and 0.15 parts of plasticizer.

[0034] Experimental data screening process:

[0035] (1) Research on the amount of reinforcing filler

[0036] A basic formula: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal mold release agent, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 parts of homogenizing tearing agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black, 0.5 parts of anti-scorch agent, 0.15 parts of plasticizer. Medium and super wear-resistant carbon black, rubber softener, wear agent, and white carbon black are variables.

[0037] B test plan:

[0038] Table 1

[0039]

[0040] From Table 1, the best ratio of the test materials is: 48 parts of super wear-resistant carbon black, 15 parts of rubber softener, 15 parts of white carbon black, and 2.5 parts of wear-resistant agent. This ratio achieves appropriate hardness and stiffness, achieves a full pattern filling effect, has the best physical properties, and normal process performance.

[0041] (2) Comparative test of vulcanization system

[0042] A basic formula: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 part of homogenizing tear-resistant agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black. Vulcanization accelerator is a variable.

[0043] B test comparison table

[0044] Table 2

[0045]

[0046] The results in Table 2 show that the optimal dosage of the vulcanization system and the active system is: 13 parts of vulcanization accelerator consists of 2 parts of accelerator DM, 9 parts of accelerator CZ and 2 parts of accelerator DS.

[0047] (3) Raw rubber and rubber combination test

[0048] A basic formula: 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 parts of homogenizing tear-resistant agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black. Natural rubber and synthetic rubber are variables.

[0049] B test comparison

[0050] Table 3

[0051]

[0052] The results in Table 3 show that the combination of natural rubber and butadiene rubber = 68:32 achieves the best effect and can take into account the performance requirements of various projects.

[0053] (4) Research on application of auxiliary materials

[0054] Table 4

[0055]

[0056] Table 4 shows that among the attached materials, the optimal amount of anti-scorch agent is 0.5 parts, the optimal amount of release agent LTM-A is 2.0 parts, the optimal amount of antioxidant is 3.5 parts, and the optimal amount of plasticizer is 0.15 parts.

[0057] (5) Comparative test of natural rubber plasticity

[0058] Table 5

[0059]

[0060] Table 5 shows that natural rubber is not plasticized, which can take into account both process performance and clear appearance and pattern requirements, consumes less energy, requires less labor, and does not occupy space, which is the best condition.

[0061] (6) Application research of vulcanizing agents and activators

[0062] A basic formula: 68 parts of natural rubber, 32 parts of butadiene rubber, 13 parts of vulcanization accelerator, 2.0 parts of rubber internal mold release agent, 2.5 parts of wear-resistant agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 parts of homogenizing anti-tear agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black, 0.5 parts

[0063] Anti-scorch agent, 0.15 parts of peptizer. Sulfur, nano zinc oxide, stearic acid variable.

[0064] Table 6

[0065]

[0066] Table 6 shows that among the attached materials, the optimal amount of sulfur is 3.2 parts, the optimal amount of nano zinc oxide is 5.0 parts, and the optimal amount of stearic acid is 2.0 parts.

[0067] (7) Research on the application of recycled rubber

[0068] Table 7

[0069]

[0070]

[0071] The test results in Table 7 show that the combined performance shows that the optimal amount of reclaimed rubber is 500 parts of high-strength reclaimed rubber.

[0072] (8) Study on sole vulcanization conditions

[0073] Vulcanization temperature and vulcanization time

[0074] Table 8

[0075]

[0076] The results in Table 8 show that the optimal conditions for sole vulcanization are: temperature 170°C, net vulcanization time 2.5 minutes, and working pressure 200 MPa.

[0077] Test conclusion:

[0078] Through the above experiments, the best formula and process conditions are as follows:

[0079] The best formula: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal release agent, 2.5 parts of wear agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 part of homogenizing anti-tear agent, 500 parts of recycled rubber, 48 parts of medium and super wear-resistant carbon black, 0.5 parts of anti-scorch agent, and 0.15 parts of plasticizer.

[0080] Process control conditions: The starting point of vulcanization is 2'40"~3'00", and natural rubber does not need to be plasticized. The best vulcanization conditions for the sole are: use a flat vulcanizer with a working pressure of 200 tons and vulcanize at 170℃ (range 168-172℃) for 2.5 minutes.

[0081] Since the physical properties of the obtained soles are at the optimal level, the wearing life of the rubber shoes reaches more than 6 months, achieving the purpose of durability.

Claims

1. A low-cost secondary vulcanized black rubber sole, characterized in that: The invention is made of the following raw materials in parts by weight: 65-70 parts of natural rubber, 30-35 parts of butadiene rubber, 3.0-3.4 parts of sulfur, 12-14 parts of vulcanization accelerator, 4.5-5.5 parts of nano zinc oxide, 2-3 parts of stearic acid, 1.5-2.5 parts of rubber internal mold release agent, 2-3 parts of wear-resistant agent, 13-17 parts of white carbon black, 3.6-4.0 parts of antioxidant, 14-16 parts of rubber softener, 0.8-1.2 parts of homogenizing tear-resistant agent, 490-510 parts of recycled rubber and 46-50 parts of medium and super wear-resistant carbon black.

2. A low-cost secondary vulcanized black rubber sole according to claim 1, characterized in that: It is made of the following raw materials in parts by weight: 68 parts of natural rubber, 32 parts of butadiene rubber, 3.2 parts of sulfur, 13 parts of vulcanization accelerator, 5.0 parts of nano zinc oxide, 2.5 parts of stearic acid, 2.0 parts of rubber internal mold release agent, 2.5 parts of wear agent, 15 parts of white carbon black, 3.8 parts of antioxidant, 15 parts of rubber softener, 1.0 part of homogenizing anti-tear agent, 500 parts of recycled rubber, and 48 parts of super wear-resistant carbon black.

3. A low-cost secondary vulcanized black rubber sole according to claim 1 or 2, characterized in that: The raw materials also contain: 0.4-0.6 parts of anti-scorching agent and 0.1-0.2 parts of peptizer.

4. A low-cost secondary vulcanized black rubber sole according to claim 1 or 2, characterized in that: The vulcanization accelerator is composed of 2 parts of accelerator DM, 9 parts of accelerator CZ and 2 parts of accelerator DS per 13 parts of vulcanization accelerator.

5. A low-cost secondary vulcanized black rubber sole according to claim 1 or 2, characterized in that: The rubber softener is composed of 5 parts of solid coumarone and 10 parts of rubber softening oil per 15 parts of the rubber softener.

6. A method for preparing a low-cost secondary vulcanized black rubber sole as claimed in any one of claims 1 to 5, characterized in that: The following steps are included: (1) Ingredients: natural rubber and cis-1,4-butadiene rubber are mixed to obtain product A; super wear-resistant carbon black is prepared to obtain product B; vulcanization accelerator and nano zinc oxide, rubber internal mold release agent, wear-resistant agent, white carbon black, antioxidant, homogenizing anti-tearing agent, recycled rubber, anti-scorch agent, peptizer, and stearic acid are mixed to obtain product C; (2) Refining sulfur-free rubber mix: Put product A into a rubber mixer, and refine it for 0.5 to 1 minute at a temperature of 80 to 125°C and a pressure of 0.34 to 0.38 MPa. Then, add product B, product C and half of the rubber softener, and continue refining for 4 to 5 minutes. Then, add the other half of the rubber softener and continue refining until the material is uniform and free of powder to obtain a semi-finished mixed product. The semi-finished mixed product is discharged to an open rubber mixer for additional refining to make the material fully dispersed and uniform to obtain a rubber mix. The rubber mix is ​​made into a 7 to 8 mm film, and then the film is soaked in a release agent liquid, and then the moisture on the film is air-dried by a fan; (3) Manufacturing secondary vulcanized black rubber sole glue: putting the air-dried rubber sheet into an open mill and refining it until it is smooth, adding sulfur, refining it evenly, and finally pressing it into sheets of the desired thickness to obtain secondary vulcanized black sole rubber blocks; (4) After obtaining the secondary vulcanized black sole rubber block, place it in a sole mold without glue flow holes at 165-172° C. on a pressing machine with a working pressure of 200 tons for hot vulcanization for 2.5-3 minutes, take the sole out of the mold, trim off the flow glue, and obtain the secondary vulcanized black rubber sole.

Citation Information

Cited By

  • Method for improving exhaust performance of sharp pattern rubber bottom basin and application of method

    CN122500865A