Polyvinyl chloride resin material and preparation method thereof
The synthesis of CuO-EDTA nanoparticles and heterojunction structures through co-precipitation method has solved the problem of limited use range and bacterial contamination of existing antibacterial PVC materials, significantly improved the antibacterial and flame retardant and smoke inhibitory properties of polyvinyl chloride resin, and ensured that The safety and environmental protection of the material.
Patent Information
- Application Number
- CN202411293131.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing antibacterial PVC materials can only be used for the synthesis of PVC films, which limits its scope of use, and additives may cause bacterial mold contamination during processing.
Nano-sized copper oxide (CuO) particles were synthesized by co-precipitation method, and combined with ethylenediaminetetraacetic acid (EDTA) to form CuO-EDTA nanoparticles, added to polyvinyl chloride resin, and passed the ratio of NaOH and copper sulfate pentahydrate. Control the particle structure and combine aluminum oxide (Al2O3) to form a heterojunction structure to enhance antibacterial and flame retardant and smoke inhibitory properties.
It significantly improves the antibacterial, flame-retardant and smoke-resisting properties of polyvinyl chloride resin, reduces bacterial pollution, expands the use range of materials, and is not toxic to the human body and the environment due to the absence of silver ions.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a polyvinyl chloride resin material and a preparation method thereof. Background Art
[0002] Polyvinyl chloride (PVC) is one of the most widely used plastics in the world. It is easy to process, low-priced, and has good chemical stability. It is in great demand in transportation, medical care, home furnishing, national defense, etc. However, PVC itself does not have bactericidal properties, and some additives added during the processing can provide sufficient nutrition for the growth of bacteria and molds, resulting in the contamination of the material by various bacteria and molds. Therefore, the research and preparation of high-performance antibacterial PVC products can reduce the spread and reproduction of bacteria, which is beneficial to human health and has great social and economic significance.
[0003] At present, all polyvinyl chloride products on the market are modified. Generally, various additives are added to the PVC resin to make PVC film to improve other properties. The Chinese invention patent application with publication number CN114479314A and publication date May 13, 2022 proposes an antibacterial PVC film, which discloses a PVC film with self-cleaning function, including the following raw materials in parts by weight: 80-120 parts of PVC resin powder, 20-25 parts of plasticizer, 20-25 parts of stabilizer, 15-25 parts of polyethersulfone and 1-5 parts of fluorinated polysiloxane.
[0004] The antibacterial principle is to use polysiloxane as a carrier to evenly disperse silver oxide and titanium oxide into the PVC film. Silver oxide and titanium oxide can degrade organic matter and have antibacterial and antifouling functions. Adding them to the PVC film makes the PVC film have antibacterial properties. Due to the addition of tannic acid, its structure has a large number of ortho-phenol structures that can form chelates with iron ions in microorganisms, depriving microorganisms of the elements necessary for growth, thereby achieving antibacterial and bactericidal effects.
[0005] Regarding the above technical solutions, although this type of material has antibacterial and bactericidal properties, it can only be used in the field of PVC film synthesis, rather than changing the properties of PVC itself, which greatly limits the scope of use of antibacterial PVC. Summary of the invention
[0006] In order to expand the application scope of antibacterial PVC, the present invention provides a polyvinyl chloride resin material and a preparation method thereof.
[0007] In the first aspect, the present invention provides a polyvinyl chloride resin material, which adopts the following technical solution: A polyvinyl chloride resin material comprises, by weight, 750-1250 parts of PVC resin, 70-350 parts of copper sulfate pentahydrate, 150-625 parts of sodium hydroxide (NaOH), and 5-15 parts of ethylenediaminetetraacetic acid (EDTA).
[0008] By adopting the above technical scheme, copper sulfate pentahydrate and NaOH are used for the synthesis of nanoparticles (NPs) by coprecipitation. By carefully controlling the nucleation and growth process, the shape and size of the particles can be well controlled. Based on the specific surface area, the antibacterial activity of nanosized copper oxide (CuO) is greater than that of micron-sized CuO. The interaction between CuO NPs and the surrounding environment increases the antibacterial property, and the CuO NPs prepared by coprecipitation can form hydroxyl groups on their surface; EDTA is a suitable capping agent because it can form complexes with amino or carboxyl groups, play the role of preservative and stabilizer, and has antibacterial and antimicrobial effects. It can also produce steric hindrance between inorganic nanoparticles, thereby reducing their agglomeration and reducing the size of nanoparticles. At the same time, this amino polycarboxylic acid is also used for polymer modification, changing the surface of nanoparticles from hydrophilic to organic, and can be introduced or grafted onto the main chain of PVC resin polymer chain. Therefore, CuO NPs treated with EDTA have good compatibility and dispersibility in PVC resin, and higher performance can be obtained than the simple addition of CuO NPs. At the same time, the addition of CuO can increase the flame retardant and smoke suppression properties of PVC resin. After adding CuO, the system can reduce the temperature of HCl release during the thermal reaction, promote the early release of HCl, and remove a large amount of HCl in a shorter time. The released HCl is an effective gas phase flame retardant, which shortens the ignition time. The addition of CuO also promotes the cross-linking and carbonization of the molecular chain, which can promote the transformation of the main structure towards stabilization. The degree of cross-linking of the main chain increases, and the chain breaking decreases. Only in the cracking stage of the carbon skeleton can heat and smoke be released, thereby achieving the purpose of improving the flame retardant and smoke suppression properties. In addition, the porous and loose morphology finally formed makes it easier to transfer heat out of the system, thereby reducing the heat retention of the entire system and protecting the system from further damage.
[0009] Optionally, the ratio of NaOH to copper sulfate pentahydrate is 2-3:1.
[0010] By adopting the above technical solution, the ratio of NaOH to copper sulfate pentahydrate can affect the structure and morphology of the synthesized CuO particles. The ratio of NaOH to copper sulfate pentahydrate is 2-3:1, which makes it easier to synthesize nano-sized CuO particles.
[0011] Optionally, the EDTA is present in an amount of 6-9 parts by weight.
[0012] By adopting the above technical solution, the weight proportion of EDTA is 1.8-2.8, which can make EDTA better perform the functional effect of the capping agent and will not react too much with the Cu in copper sulfate pentahydrate. 2+ Chelation is performed, thereby reducing the production of the desired CuO.
[0013] Optionally, the polyvinyl chloride resin material composition also includes 45-80 parts of aluminum oxide (Al2O3).
[0014] By adopting the above technical scheme, the sintering activation process induced by NaOH electrolyte greatly enriches the CuO / Al2O3 interface, so that Al2O3 in PVC resin can act as a Lewis acid carrier, promoting the release of HCl from CuO NPs and the cross-linking and carbonization of molecular chains; At the same time, HCl also reacts with Al2O3 to generate AlCl3 and water, and will continue to form a strong electrophilic complex AlCl3·nHCl. When the complex continues to be heated, it will release nHCl, thereby accelerating the release of a large amount of HCl. HCl and water vapor quickly form a protective effect on the main material. In addition, Al2O3 has a large surface area and can adsorb cigarette cores and smoke particles. The combination of the two makes PVC begin to form a cross-linked structure while removing HCl, and the cross-linked structure promotes the entire cracking reaction, increases the gel content, and reduces the content of aromatic compounds, thereby producing a flame retardant and smoke suppression structure and performance. The combination of the two makes Al2O3 have a more suitable band gap range, and can also produce active oxygen species under visible light, thereby improving the bactericidal performance. In addition, since aluminum oxide and copper oxide do not contain harmful substances such as silver ions, they are non-toxic and non-irritating to the human body and do not pollute the environment.
[0015] In a second aspect, the present invention provides a method for preparing a polyvinyl chloride resin material, which adopts the following technical solution: A method for preparing a polyvinyl chloride resin material comprises the following steps: The copper sulfate pentahydrate described in the first aspect is dissolved in distilled water, and then a NaOH solution is added dropwise every 15 minutes to obtain a desired pH value, wherein the desired pH value is pH=12-14, and the whole mixture is stirred at room temperature for 1 hour using a magnetic stirrer at a speed of 100 rpm to obtain a liquid solution; Adding EDTA as a capping agent to the liquid solution of step (1) and stirring for 3 hours to obtain a precursor; The precursor was rinsed with distilled water and ethanol three times to remove the residue and filtered using filter paper, and the resulting paste was dried at 80 °C for 12 h and then ground using an agate mortar to form mixture A; The PVC resin was dissolved in tetrahydrofuran (THF) and subjected to ultrasonic treatment at room temperature for 15 min to form a homogeneous polymer solution; Adding mixture A to the homogeneous polymer solution of step (4), and ultrasonically treating for 1 hour to obtain PVC / mixture A; The obtained PVC / mixture A was placed in a petri dish and dried at room temperature for 24 hours, and then the remaining solvent was removed by vacuum, and finally the PVC / mixture A film was isolated.
[0016] By adopting the above technical scheme, in step (1), the NaOH solution is gradually added dropwise to obtain a suitable pH value so that the reaction between NaOH and copper sulfate pentahydrate can be more complete and sufficient, and the shape and size of the particles can be controlled to generate CuO nanoparticles; in step (2), EDTA is used as a capping agent for polymer modification to make CuO have better compatibility and dispersibility in PVC resin; in step (3), the desired mixture A, i.e., CuO-EDTA, is obtained by filtering and drying; in step (4), the PVC resin is dispersed more evenly by ultrasonic action; in steps (5) and (6), the desired PVC / CuO-EDTA is obtained by combining CuO-EDTA and PVC resin, and the film is dried to facilitate subsequent reaction testing.
[0017] Optionally, the weight percentage of PVC resin added to the mixture A in step (5) is 10-13%.
[0018] By adopting the above technical solution, mixture A can be better dispersed in the resin, reducing the agglomeration effect in the resin, so that the material can exert better bactericidal, flame retardant and smoke suppression properties.
[0019] Optionally, in step (1), copper sulfate pentahydrate and Al2O3 are added to distilled water simultaneously; In step (3), the precursor was dried at 80°C for 12 hours, placed in a crucible, calcined at 400°C for 2 hours, and then ground into mixture A using an agate mortar.
[0020] By adopting the above technical scheme, in the NaOH electrolyte-induced sintering activation process, Al2O3 and NaOH can generate sodium tetrahydroxyaluminate, and Al2O3 is dispersed on the surface of the synthesized CuO NPs, which greatly enriches the CuO / Al2O3 interface. Through sintering, the two are not just a simple mechanical composite, but a heterojunction structure is formed. The synthetic mixture A, namely CuO@Al2O3-EDTA, makes Al2O3 effectively act as a Lewis acid carrier, promotes the release of HCl from CuO NPs and the cross-linking and carbonization of the molecular chains. At the same time, it makes Al2O3 have a more suitable band gap range, and can also produce active oxygen species under visible light, thereby improving the bactericidal performance.
[0021] In summary, the present invention includes at least one of the following beneficial technical effects: The co-precipitation method was applied to the synthesis of CuO NPs, and the shape and size of the particles could be well controlled by carefully controlling the nucleation and growth processes.
[0022] The addition of EDTA can produce steric hindrance between inorganic nanoparticles, thereby reducing their agglomeration and reducing the size of nanoparticles. At the same time, this amino polycarboxylic acid is also used for polymer modification, changing the surface of the nanoparticles from hydrophilic to organophilic, and can be introduced or grafted onto the main chain of the PVC resin polymer chain.
[0023] The addition of CuO can increase the flame retardant and smoke suppression properties of PVC resin. After adding CuO, the system can reduce the temperature of HCl release during the thermal reaction and promote the early release of HCl. The addition of CuO also promotes the cross-linking and carbonization of the molecular chain, which can promote the transformation of the main structure towards stabilization.
[0024] The sintering activation process induced by NaOH electrolyte greatly enriches the CuO / Al2O3 interface, allowing Al2O3 in PVC resin to act as a Lewis acid carrier, promoting the release of HCl from CuO NPs and the cross-linking and carbonization of molecular chains. The combination of the two gives Al2O3 a more suitable band gap range, and it can also produce active oxygen species under visible light, thereby improving the bactericidal performance. In addition, since aluminum oxide and copper oxide do not contain harmful substances such as silver ions, they are non-toxic and non-irritating to the human body and do not pollute the environment. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below with reference to the embodiments.
[0026] Example 1: This example discloses a polyvinyl chloride resin material, which comprises the following components by weight: 1000 parts of PVC resin, 180 parts of copper sulfate pentahydrate, 445 parts of NaOH, and 7.2 parts of EDTA.
[0027] The preparation method is as follows, The copper sulfate pentahydrate was dissolved in distilled water, and then a NaOH solution was added dropwise every 15 minutes to obtain a desired pH value, wherein the desired pH value is pH=12-14, and the whole mixture was stirred at room temperature for 1 hour using a magnetic stirrer at a speed of 100 rpm to obtain a liquid solution; Adding EDTA as a capping agent to the liquid solution of step (1) and stirring for 3 hours to obtain a precursor; The precursor was rinsed with distilled water and ethanol three times to remove the residue and filtered using filter paper, and the resulting paste was dried at 80 °C for 12 h and then ground into CuO-EDTA using an agate mortar; The PVC resin was dissolved in tetrahydrofuran (THF) and subjected to ultrasonic treatment at room temperature for 15 min to form a homogeneous polymer solution; Adding mixture A to the homogeneous polymer solution described in step (4), and ultrasonically treating for 1 hour to obtain PVC / CuO-EDTA; The obtained PVC / CuO-EDTA was placed in a petri dish and dried at room temperature for 24 hours, and then the remaining solvent was removed by vacuum, and finally the PVC / CuO-EDTA membrane was separated.
[0028] Example 2: This example discloses a polyvinyl chloride resin material, which comprises, by weight, 1000 parts of PVC resin, 180 parts of copper sulfate pentahydrate, 445 parts of NaOH, 7.2 parts of EDTA, and 56 parts of Al2O3.
[0029] The preparation method is as follows, The copper sulfate pentahydrate and Al2O3 were dissolved in distilled water, and then NaOH solution was added dropwise every 15 minutes to obtain a desired pH value, wherein the desired pH value is pH=12-14, and the whole mixture was stirred at room temperature for 1 hour using a magnetic stirrer at a speed of 100 rpm to obtain a liquid solution; Adding EDTA as a capping agent to the liquid solution of step (1) and stirring for 3 hours to obtain a precursor; The precursor was rinsed with distilled water and ethanol for 3 times to remove the residue, and filtered with filter paper. The obtained paste was dried at 80 °C for 12 hours. After drying, it was placed in a crucible and calcined at 400 °C for 2 hours, and then ground into CuO@Al2O3-EDTA using an agate mortar. The PVC resin was dissolved in tetrahydrofuran (THF) and subjected to ultrasonic treatment at room temperature for 15 min to form a homogeneous polymer solution; Adding mixture A to the homogeneous polymer solution described in step (4), and ultrasonically treating for 1 hour to obtain PVC / CuO@Al2O3-EDTA; The obtained PVC / CuO@Al2O3-EDTA was placed in a Petri dish and dried at room temperature for 24 h, and then the remaining solvent was removed by vacuum, and finally the PVC / CuO@Al2O3-EDTA membrane was separated.
[0030] Example 3: This example discloses a polyvinyl chloride resin material, which comprises, by weight, 1000 parts of PVC resin, 180 parts of copper sulfate pentahydrate, 300 parts of NaOH, and 7.2 parts of EDTA.
[0031] The preparation method thereof is completely the same as that of Example 1 except that the ratio of the polyvinyl chloride resin material is different from that of Example 1.
[0032] Example 4: This example discloses a polyvinyl chloride resin material, which comprises the following components by weight: 1000 parts of PVC resin, 180 parts of copper sulfate pentahydrate, 445 parts of NaOH, and 15 parts of EDTA.
[0033] The preparation method thereof is completely the same as that of Example 1 except that the ratio of the polyvinyl chloride resin material is different from that of Example 1.
[0034] Example 5: This example discloses a polyvinyl chloride resin material, which comprises the following components by weight: 750 parts of PVC resin, 275 parts of copper sulfate pentahydrate, 610 parts of NaOH, and 7.2 parts of EDTA.
[0035] The preparation method thereof is completely the same as that of Example 1 except that the ratio of the polyvinyl chloride resin material is different from that of Example 1.
[0036] Comparative Example 1: This comparative example discloses a polyvinyl chloride resin material, The preparation method is as follows, The PVC resin was dissolved in tetrahydrofuran and subjected to ultrasonic treatment at room temperature for 15 min to form a homogeneous polymer solution; The obtained PVC polymer solution was placed in a Petri dish and dried at room temperature for 24 hours, and then the remaining solvent was removed by vacuum, and finally the PVC film was isolated.
[0037] Comparative Example 2: This comparative example discloses a polyvinyl chloride resin material, The preparation method is as follows, (1) dissolving the copper sulfate pentahydrate and NaOH in distilled water, stirring the entire mixture at room temperature for 1 hour using a magnetic stirrer at a speed of 100 rpm to obtain a liquid solution; The weight parts of the composition and the preparation method are exactly the same as those of Example 1, except that step (1) is different from that of Example 1.
[0038] The high ductility thin layer repair concrete prepared in Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 were tested and experimented.
[0039]
[0040] By comparing Example 1 with Comparative Example 1, and comparing the performance of the PVC / CuO-EDTA film synthesized in Example 1 with that of the pure PVC film synthesized in Comparative Example 1, it can be seen that the addition of CuO-EDTA significantly improves the bactericidal and flame retardant and smoke suppression properties of the material, and the bactericidal and antibacterial rates of Escherichia coli and Staphylococcus aureus can reach more than 98%, and the total smoke production and heat release rate are significantly reduced. The lower the heat release rate, the less heat is fed back to the surface of the material, so that the thermal decomposition rate of the material and the amount of volatile combustibles generated are reduced. At the same time, the increase in the amount of charring reflects that the addition of CuO-EDTA promotes the cross-linking of the carbon chain and the amount of charring in the early stage, stabilizes the carbon skeleton, reduces the thermal cracking of the carbon skeleton, can promote the transformation of the main structure in the direction of stabilization, and reduces the further oxidation of residual carbon, showing a good flame retardant and smoke suppression effect.
[0041] By comparing Example 2 with Example 1, it can be seen that by adding Al2O3, Al2O3 and CuO form a heterojunction structure, and Al2O3 can serve as a Lewis acid carrier to promote the release of HCl from CuO NPs and the cross-linking and carbonization of the molecular chains, showing good flame retardant and smoke suppression effects. At the same time, the combination of the two makes Al2O3 have a more suitable band gap range, and can also produce active oxygen species under visible light, thereby improving the bactericidal performance.
[0042] By comparing Example 3 with Example 1, it can be seen that by changing the ratio of sodium hydroxide to copper sulfate pentahydrate, the ratio of sodium hydroxide to copper sulfate pentahydrate is reduced, and copper sulfate pentahydrate cannot fully react with sodium hydroxide to generate CuONPs, so that the performance of the material in all aspects is reduced, but within an acceptable range.
[0043] By comparing Example 4 with Example 1, it can be seen that by increasing the content of EDTA, EDTA will replace part of the OH - With Cu 2+ Chelation reduces the production of CuO NPs, causing all aspects of the material performance to decline. At the same time, the EDTA content increases, and the combustion of its organic skeleton will release more smoke and heat, which affects the flame retardant and smoke suppression properties of the product, but is within an acceptable range.
[0044] By comparing Example 5 with Example 1, it can be seen that increasing the content of CuO-EDTA reduces the dispersibility of CuO-EDTA and produces agglomeration, which reduces various performances of the material, but is within an acceptable range.
[0045] By comparing Example 2 with Example 1, it can be seen that by changing the way of adding NaOH, the direct addition of NaOH reduces the amount of CuO NPs generated, produces more micron-sized CuO, reduces the specific surface area, reduces the interaction with the surrounding environment, and reduces various aspects of the material performance.
[0046] The above are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A polyvinyl chloride resin material, It is characterized in that The composition comprises, by weight: 750-1250 parts of polyvinyl chloride resin, 70-350 parts of copper sulfate pentahydrate, 150-625 parts of sodium hydroxide and 5-15 parts of ethylenediaminetetraacetic acid.
2. A polyvinyl chloride resin material according to claim 1, Features: The ratio of the sodium hydroxide to copper sulfate pentahydrate is 2-3:
1.
3. A polyvinyl chloride resin material according to claim 1, Features: The weight proportion of the ethylenediaminetetraacetic acid is 6-9 parts.
4. A polyvinyl chloride resin material according to claim 1, Features: The polyvinyl chloride resin material also includes 45-80 parts of aluminum oxide.
5. A method for preparing a polyvinyl chloride resin material, It is characterized by the following step: Dissolve the copper sulfate pentahydrate according to any one of claims 1 to 4 in distilled water, then add a sodium hydroxide solution dropwise every 15 minutes to obtain a desired pH value, wherein the desired pH value is pH=12-14, and stir the entire mixture at room temperature for 1 hour using a magnetic stirrer at a speed of 100 rpm to obtain a liquid solution; Adding ethylenediaminetetraacetic acid as a capping agent into the liquid solution of step (1) and stirring for 3 hours to obtain a precursor; The precursor was rinsed with distilled water and ethanol three times to remove the residue and filtered using filter paper, and the resulting paste was dried at 80 °C for 12 h and then ground using an agate mortar to form mixture A; The polyvinyl chloride resin was dissolved in tetrahydrofuran and subjected to ultrasonic treatment at room temperature for 15 minutes to form a homogeneous polymer solution; Adding mixture A to the homogeneous polymer solution of step (4), and ultrasonically treating for 1 hour to obtain polyvinyl chloride / mixture A; The obtained polyvinyl chloride / mixture A was placed in a petri dish and dried at room temperature for 24 hours, and then the remaining solvent was removed by vacuum, and finally the polyvinyl chloride / mixture A film was separated.
6. A method for preparing a polyvinyl chloride resin material according to claim 5, Features: The weight percentage of polyvinyl chloride resin added to the mixture A in step (5) is 10-13%.
7. A method for preparing a high-ductility thin-layer repair concrete according to claim 5, Features: In step (1), copper sulfate pentahydrate and aluminum oxide are added to distilled water simultaneously; In step (3), the precursor was dried at 80°C for 12 hours, placed in a crucible, calcined at 300°C for 2 hours, and then ground into mixture A using an agate mortar.