Thermosetting phenolic resin capable of improving stability and preparation method thereof

By introducing composite components of naphthalene boric acid and boron nitride into the phenolic resin to form a B-O bond and a three-dimensional network structure, the problem of the decrease in stability of the phenolic resin at high temperatures is solved, and its thermal stability and mechanical properties are significantly improved.

CN118956092APending Publication Date: 2024-11-15CHANGSHU SOUTHEAST PLASTIC CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411333601.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional phenolic resins are prone to thermal oxidation and degradation at high temperatures, resulting in a decrease in stability and affecting heat resistance.

Method used

Naphthalene boric acid is introduced to form B-O bonds, combining boron nitride composite components and carbon nanotubes, reducing thermal decomposition losses through the esterification reaction of phenolic hydroxyl groups, and forming a stable three-dimensional network structure to improve the mechanical and heat resistance of the resin.

Benefits of technology

It significantly improves the thermal stability and mechanical properties of phenolic resin, enhances its toughness and impact resistance, and improves the overall performance of the resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005057677840000081
    Figure BDA0005057677840000081
  • Figure BDA0005057677840000091
    Figure BDA0005057677840000091
Patent Text Reader

Abstract

The invention relates to thermosetting phenolic resin with improved stability and a preparation method thereof. The thermosetting phenolic resin comprises the following raw material components in parts by mass: 159-169 parts of a boronized phenolic resin precursor, 7-11 parts of a curing agent, 11-13 parts of a toughening agent and 2-4 parts of a dispersing agent, the boronized phenolic resin precursor comprises the following raw materials: phenol, naphthalene boric acid, formaldehyde and oxalic acid dihydrate. The method has the effect of improving the stability of the thermosetting phenolic resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of phenolic resins, and in particular to a thermosetting phenolic resin with improved stability and a preparation method thereof. Background Art

[0002] Phenolic resin is a polymer compound obtained by the condensation of phenolic formaldehyde or its derivatives. It is mainly used in the manufacture of various plastics, coatings, adhesives and synthetic fibers. Phenolic resin is divided into two categories: thermosetting resin and thermoplastic resin. After curing, it has excellent properties such as high mechanical strength, good rigidity, heat resistance, flame retardancy, ablation resistance, and good dielectric properties.

[0003] The traditional phenolic resin consists of two phenols with a methylene group sandwiched between them. The phenolic hydroxyl group and the methylene group in this structure are easily degraded by thermal oxidation at high temperatures, affecting the overall heat resistance of the system, thereby reducing the stability of the phenolic resin. Summary of the invention

[0004] In order to improve the stability of the prepared thermosetting phenolic resin, the present application provides a thermosetting phenolic resin with improved stability and a preparation method thereof.

[0005] The present application provides a thermosetting phenolic resin with improved stability and a preparation method thereof, which adopts the following technical solutions: In the first aspect, the present application provides a thermosetting phenolic resin, which adopts the following technical solutions: A thermosetting phenolic resin with improved stability comprises the following raw material components by weight: 159-169 parts of boronized phenolic resin precursor, 7-11 parts of curing agent, 11-13 parts of toughening agent, 2-4 parts of dispersant; The boronized phenolic resin precursor raw materials include phenol, naphthaleneboric acid, formaldehyde and oxalic acid dihydrate.

[0006] By adopting the above technical scheme, naphthaleneboric acid is introduced on the basis of preparing phenolic resin, thereby introducing B—O bond. The B—O bond has excellent flexibility and can reduce the internal stress of the rigid benzene ring, thereby improving the toughness of the resin system, improving the mechanical strength of the resin system, and improving the cross-linking degree of the resin material, so that the prepared phenolic resin precursor has a good three-dimensional network structure, further improving the mechanical properties of the resin precursor system, thereby improving the thermal stability of the prepared phenolic resin.

[0007] Preferably, the boronated phenolic resin precursor is prepared by the following method: Phenol and naphthaleneboric acid are mixed to obtain a mixture. The pH value is adjusted to acidic under oil bath conditions. After the reaction, the temperature is increased and the reaction is continued for 2 hours to obtain naphthaleneboric acid phenol ester. After the naphthaleneboric acid phenol ester is cooled, formaldehyde is added to the naphthaleneboric acid phenol ester, and then deionized water and dihydrated oxalic acid are added. The temperature is increased to react, and after washing, the mixture is distilled under reduced pressure and dehydrated to obtain a boronated phenolic resin precursor.

[0008] By adopting the above technical scheme, during the preparation, the esterification reaction of BO—H bonds and phenolic hydroxyl groups reduces the number of phenolic hydroxyl groups, further reducing the mass loss during the thermal decomposition process. At the same time, boron oxide is formed in the process, which can further reduce the overflow of small molecules of carbides during the thermal decomposition process. When the resin precursor system is formed, a B—O—C structure is obtained to form a stable three-dimensional network, which greatly improves the heat resistance of the resin, thereby improving the heat resistance and mechanical properties of the entire system.

[0009] Preferably, the mass ratio of phenol, naphthaleneboric acid and formaldehyde is 1:(0.14-0.18):2.45.

[0010] By adopting the above technical solution, preferably the mass ratio of phenol, naphthaleneboric acid and formaldehyde is within the above range, the stability of the prepared boronated phenolic resin precursor can be further improved.

[0011] Preferably, the toughening agent raw material includes a boron nitride composite component and carbon nanotubes.

[0012] By adopting the above technical scheme, a toughening agent is added to the phenolic resin system, so that the brittleness of the phenolic resin can be improved, thereby improving the toughness of the phenolic resin, further improving the stability of the prepared phenolic resin, and jointly modifying the phenolic resin system under the combination of boron nitride composite components and carbon nanotubes, so that the mechanical properties of the stabilizer of the phenolic resin are synergistically improved.

[0013] Preferably, the boron nitride composite component raw materials include nano boron nitride, polyethyleneimine and dopamine.

[0014] By adopting the above technical scheme, nano boron nitride has good temperature change resistance. By introducing polyethyleneimine into nano boron carbide through dopamine, on the one hand, it can promote the curing reaction of phenolic resin and reduce energy consumption. At the same time, it can improve the compatibility of boron nitride composite components, strengthen the interface of the resin system, and synergistically improve the overall heat resistance of the resin system and the overall stability of the resin material.

[0015] Preferably, the boron nitride composite component is prepared by the following method: The nano boron nitride is mixed with Tris buffer, and after ultrasonication, dopamine hydrochloride is added, and polyethyleneimine is added after stirring. After stirring, the impurities are removed by washing, and the washed material is dried to obtain a boron nitride composite component.

[0016] By adopting the above technical solution, dopamine is coated on nano-boron nitride and grafted with polyethyleneimine, so that the agglomeration effect between the nano-boron nitride sheets is weakened, and the dispersion uniformity of the nano-boron nitride in the system is improved.

[0017] Preferably, the mass ratio of polyethyleneimine, dopamine and nano-boron nitride is 0.3:(0.42-0.46):1.

[0018] By adopting the above technical solution, preferably the mass ratio between polyethyleneimine, dopamine and nano-boron nitride is within the above range, which can further improve the stability of the prepared boron nitride composite component.

[0019] Preferably, the toughening agent is prepared by the following method: The carbon nanotubes are mixed with ethanol to obtain a carbon nanotube dispersion, the boron nitride composite product is mixed with ethanol to obtain a boron nitride dispersion, the carbon nanotube dispersion and the boron nitride dispersion are mixed, refluxed and stirred, and the product is then centrifuged and washed, and dried to obtain a toughening agent.

[0020] By adopting the above technical scheme, the interface bonding between the boron nitride composite component and the resin is enhanced, and a stable three-dimensional network structure is formed between the boron nitride composite and the carbon nanotubes, so that the toughening agent has good thermal stability. At the same time, the interface bonding performance of the toughening agent in the system is enhanced, the toughness of the phenolic resin system is improved, and thus the overall stability of the resin system is improved.

[0021] Preferably, the curing agent comprises hexamethylenetetramine.

[0022] By adopting the above technical solution, hexamethylenetetramine can be used as a curing agent to cure the phenolic resin. During the curing process, the secondary amine structure of hexamethylenetetramine reacts with the active hydrogen on the benzene ring, so that the phenolic resin structure has just the right flexibility to improve the overall toughness of the resin. At the same time, the carbon nanotubes in the toughening agent can compensate for the negative impact of hexamethylenetetramine on the thermal decomposition reaction of the phenolic resin, further improving the overall heat resistance and stability of the phenolic resin system.

[0023] In a second aspect, the present application provides a method for preparing a thermosetting phenolic resin with improved stability, using the following technical solution: A method for preparing a thermosetting phenolic resin with improved stability comprises the following steps: The boronized phenolic resin is ground and heated to be in a low-viscosity state, a curing agent is added, and magnetic stirring is performed to obtain a phenolic resin system, a toughening agent and a dispersant are added to ethanol, ultrasonically dispersed, and then added to the phenolic resin system, and magnetically stirred and cured to obtain a thermosetting phenolic resin.

[0024] In summary, the present application includes at least one of the following beneficial technical effects: 1. By introducing naphthaleneboric acid into the phenolic resin system, a B-O bond with good flexibility is introduced into the system, which can reduce the internal stress of the rigid benzene ring, improve the flexibility of the phenolic resin, and increase the cross-linking degree of the resin material. The prepared phenolic resin precursor has a good three-dimensional network structure and effectively improves the thermal stability of the phenolic resin precursor. After compounding with a toughening agent, the overall mechanical properties of the phenolic resin can be improved.

[0025] 2. The boron nitride composite component in the toughening agent can improve the brittleness of the phenolic resin and modify the phenolic resin precursor. Dopamine is coated on the surface of the boron nitride and polyethyleneimine is grafted to promote the curing reaction of the phenolic resin to reduce energy consumption. At the same time, the interface compatibility of the boron nitride composite component is improved. After compounding with carbon nanotubes, it can be evenly dispersed in the resin system, improving the mechanical properties of the resin material while synergistically improving the thermal stability of the resin system; 3. Hexamethylenetetramine is used as a curing agent, so that the prepared phenolic resin has good flexibility. At the same time, carbon nanotubes compensate for the negative impact of hexamethylenetetramine during the thermal decomposition reaction of the phenolic resin, thereby improving the stability of the phenolic resin system. DETAILED DESCRIPTION

[0026] The present application is further described in detail below with reference to the embodiments: Raw materials description: All raw materials in the examples can be obtained from commercial sources; among them, Example 1 Preparation of Boron Nitride Composite Components: Isopropanol and deionized water are mixed in a volume ratio of 4:6 to obtain an isopropanol solution, 50 g of hexagonal boron nitride powder is added to 800 g of the isopropanol solution, ultrasonicated for 8 hours, and then centrifuged at a speed of 5000 r / min for 30 minutes. The supernatant after centrifugation is removed and centrifuged at a speed of 10000 r / min for 30 minutes. The solid at the bottom of the centrifuge tube is dried in a vacuum drying oven at 60°C for 20 hours, and nano boron nitride is obtained after grinding; 34.88 g of nano boron nitride is mixed with 2000 g of Tris buffer, and after ultrasonication, 14.65 g of dopamine hydrochloride is added, stirred at a speed of 300 r / min for 18 hours, and then 10.47 g of polyethyleneimine is added and stirred for 3 hours. Finally, deionized water is used to repeatedly wash to remove impurities, and the washed material is dried in an oven at 60°C for 24 hours to obtain a boron nitride composite component.

[0027] Preparation of toughening agent: 12.5 g of carbon nanotubes were mixed with 600 g of ethanol to obtain a carbon nanotube dispersion, and 27.5 g of a boron nitride composite product was mixed with 800 g of ethanol to obtain a boron nitride dispersion. After the carbon nanotube dispersion and the boron nitride dispersion were mixed, they were refluxed at 60° C. and stirred at 600 r / min for 12 h. The product was then centrifuged, washed alternately with deionized water and ethanol for 3 times, and dried in an oven at 60° C. for 12 h to obtain a toughening agent.

[0028] Preparation of boronated phenolic resin precursor: 83.57 g of phenol and 11.7 g of naphthaleneboric acid are mixed to obtain a mixture, hydrogen chloride is added under oil bath conditions at 90° C. to adjust the pH value of the mixture to 2.5, the mixture is reacted for 1 h, the temperature is raised to 120° C. and the reaction is continued for 2 h to obtain naphthaleneboric acid phenol ester, the naphthaleneboric acid phenol ester is cooled to 65° C., 204.73 g of formaldehyde is added to the naphthaleneboric acid phenol ester, and then 100 g of deionized water and 1 g of oxalic acid dihydrate are added, the temperature is raised to 95° C., the mixture is reacted for 1.5 h, the mixture is washed with distilled water, and then distilled under reduced pressure to dehydrate the mixture to obtain a boronated phenolic resin precursor.

[0029] Preparation of thermosetting phenolic resin: 169 g of boronated phenolic resin was ground and heated to 60°C to make it in a low-viscosity state. 7 g of curing agent was added and magnetically stirred to mix the two evenly to obtain a phenolic resin system. 22 g of toughening agent and 2 g of dispersant were added to ethanol, ultrasonically dispersed for 60 minutes, and then added to the phenolic resin system. The mixture was magnetically stirred until the system was uniform, and then transferred to a vacuum oven, heated to 180°C, and cured for 2 hours to obtain a thermosetting phenolic resin.

[0030] Example 2 Preparation of Boron Nitride Composite Components: Isopropanol and deionized water are mixed in a volume ratio of 4:6 to obtain an isopropanol solution, 50 g of hexagonal boron nitride powder is added to 800 g of the isopropanol solution, ultrasonicated for 8 hours, and then centrifuged at a speed of 5000 r / min for 30 minutes. The supernatant after centrifugation is removed and centrifuged at a speed of 10000 r / min for 30 minutes. The solid at the bottom of the centrifuge tube is dried in a vacuum drying oven at 60°C for 20 hours, and nano boron nitride is obtained after grinding; 34.09 g of nano boron nitride is mixed with 2000 g of Tris buffer, ultrasonicated, 15.68 g of dopamine hydrochloride is added, stirred at a speed of 300 r / min for 18 hours, and then 10.23 g of polyethyleneimine is added and stirred for 3 hours. Finally, deionized water is used to repeatedly wash to remove impurities, and the washed material is dried in an oven at 60°C for 24 hours to obtain a boron nitride composite component.

[0031] Preparation of toughening agent: 11.76 g of carbon nanotubes were mixed with 600 g of ethanol to obtain a carbon nanotube dispersion, and 28.24 g of a boron nitride composite product was mixed with 800 g of ethanol to obtain a boron nitride dispersion. After the carbon nanotube dispersion and the boron nitride dispersion were mixed, they were refluxed at 60° C. and stirred at 600 r / min for 12 h. The product was then centrifuged, washed alternately with deionized water and ethanol for 3 times, and dried in an oven at 60° C. for 12 h to obtain a toughening agent.

[0032] Preparation of boronated phenolic resin precursor: 82.64 g of phenol and 14.88 g of naphthaleneboric acid were mixed to obtain a mixture, hydrogen chloride was added under oil bath conditions at 90° C. to adjust the pH value of the mixture to 2.5, the mixture was reacted for 1 h, the temperature was raised to 120° C. and the reaction was continued for 2 h to obtain naphthaleneboric acid phenol ester, the naphthaleneboric acid phenol ester was cooled to 65° C., 202.48 g of formaldehyde was added to the naphthaleneboric acid phenol ester, and then 100 g of deionized water and 1 g of oxalic acid dihydrate were added, the temperature was raised to 95° C., the mixture was reacted for 1.5 h, the mixture was washed with distilled water, and then distilled under reduced pressure to obtain a boronated phenolic resin precursor.

[0033] Preparation of thermosetting phenolic resin: 159 g of boronated phenolic resin was ground and heated to 60°C to make it in a low-viscosity state. 11 g of curing agent was added and magnetically stirred to mix the two evenly to obtain a phenolic resin system. 26 g of toughening agent and 4 g of dispersant were added to ethanol, ultrasonically dispersed for 60 minutes, and then added to the phenolic resin system. The mixture was magnetically stirred until the system was uniform, and then transferred to a vacuum oven, heated to 180°C, and cured for 2 hours to obtain a thermosetting phenolic resin.

[0034] Example 3 Preparation of Boron Nitride Composite Components: Isopropanol and deionized water are mixed in a volume ratio of 4:6 to obtain an isopropanol solution, 50 g of hexagonal boron nitride powder is added to 800 g of the isopropanol solution, ultrasonicated for 8 hours, and then centrifuged at a speed of 5000 r / min for 30 minutes. The supernatant after centrifugation is removed and centrifuged at a speed of 10000 r / min for 30 minutes. The solid at the bottom of the centrifuge tube is dried in a vacuum drying oven at 60°C for 20 hours, and nano boron nitride is obtained after grinding; 34.48 g of nano boron nitride is mixed with 2000 g of Tris buffer, and after ultrasonication, 15.18 g of dopamine hydrochloride is added, stirred at a speed of 300 r / min for 18 hours, and then 10.34 g of polyethyleneimine is added and stirred for 3 hours. Finally, deionized water is used to repeatedly wash to remove impurities, and the washed material is dried in an oven at 60°C for 24 hours to obtain a boron nitride composite component.

[0035] Preparation of toughening agent: 12.12 g of carbon nanotubes were mixed with 600 g of ethanol to obtain a carbon nanotube dispersion, and 27.88 g of a boron nitride composite product was mixed with 800 g of ethanol to obtain a boron nitride dispersion. After the carbon nanotube dispersion and the boron nitride dispersion were mixed, they were refluxed at 60° C. and stirred at 600 r / min for 12 h. The product was then centrifuged, washed alternately with deionized water and ethanol for 3 times, and dried in an oven at 60° C. for 12 h to obtain a toughening agent.

[0036] Preparation of boronated phenolic resin precursor: 83.1 g of phenol and 13.3 g of naphthaleneboric acid are mixed to obtain a mixture, hydrogen chloride is added to adjust the pH value of the mixture to 2.5 under oil bath conditions at 90° C., the mixture is reacted for 1 h, the temperature is raised to 120° C. and the reaction is continued for 2 h to obtain naphthaleneboric acid phenol ester, the naphthaleneboric acid phenol ester is cooled to 65° C., 203.6 g of formaldehyde is added to the naphthaleneboric acid phenol ester, and then 100 g of deionized water and 1 g of oxalic acid dihydrate are added, the temperature is raised to 95° C., the mixture is reacted for 1.5 h, the mixture is washed with distilled water, and then distilled under reduced pressure to dehydrate the mixture to obtain a boronated phenolic resin precursor.

[0037] Preparation of thermosetting phenolic resin: 164 g of boronated phenolic resin was ground and heated to 60°C to make it in a low-viscosity state. 9 g of curing agent was added and magnetically stirred to mix the two evenly to obtain a phenolic resin system. 24 g of toughening agent and 3 g of dispersant were added to ethanol, ultrasonically dispersed for 60 minutes, and then added to the phenolic resin system. The mixture was magnetically stirred until the system was uniform, and then transferred to a vacuum oven, heated to 180°C, and cured for 2 hours to obtain a thermosetting phenolic resin.

[0038] Example 4 Example 4 is based on Example 3. The difference between Example 4 and Example 3 is that when preparing the boron nitride composite component, Example 4 uses 35.71 g of nano boron nitride, 10.71 g of polyethyleneimine, and 13.58 g of dopamine.

[0039] Example 5 Example 5 is based on Example 3. The difference between Example 5 and Example 3 is that when preparing the boron nitride composite component in Example 5, 33.33 g of nano boron carbide, 10 g of polyethyleneimine and 16.67 g of dopamine are used.

[0040] Example 6 Example 6 is based on Example 3. The difference between Example 6 and Example 3 is that when preparing the toughening agent in Example 6, 26.67 g of the boron nitride composite component and 13.33 g of the carbon nanotubes are used.

[0041] Example 7 Example 7 is based on Example 3. The difference between Example 7 and Example 3 is that when preparing the toughening agent in Example 7, 28.89 g of boron nitride component and 11.11 g of carbon nanotubes are used.

[0042] Example 8 Example 8 is based on Example 3. The difference between Example 8 and Example 3 is that when preparing the phenolic resin precursor in Example 8, 84.27 g of phenol, 9.27 g of naphthalene boronic acid and 206.46 g of formaldehyde are used.

[0043] Example 9 Example 9 is based on Example 3. The difference between Example 9 and Example 3 is that when preparing the phenolic resin precursor in Example 9, 81.97 g of phenol, 17.21 g of naphthalene boronic acid and 200.82 g of formaldehyde are used.

[0044] Example 10 Example 10 is based on Example 3. The difference between Example 10 and Example 3 is that in Example 10, dopamine is not added when preparing the boron nitride composite component.

[0045] Embodiment 11 Example 11 is based on Example 3. The difference between Example 11 and Example 3 is that when preparing the boron nitride composite component in Example 11, polyethyleneimine is not added.

[0046] Example 12 Example 12 is based on Example 3. The difference between Example 12 and Example 3 is that when preparing the toughening agent in Example 12, the boron nitride composite component is replaced with an equal amount of nano boron nitride.

[0047] Embodiment 13 Example 13 is based on Example 3. The difference between Example 13 and Example 3 is that in Example 13, when preparing the thermosetting phenolic resin, 174 g of boronized phenolic resin precursor and 14 g of toughening agent are used.

[0048] Embodiment 14 Example 14 is based on Example 3. The difference between Example 14 and Example 3 is that in Example 14, when preparing the thermosetting phenolic resin, 154 g of the boronized phenolic resin precursor and 34 g of the toughening agent are used.

[0049] Embodiment 15 Example 15 is based on Example 3. The difference between Example 15 and Example 3 is that in Example 15, when preparing the thermosetting phenolic resin, 169 g of boronized phenolic resin precursor and 4 g of curing agent are used.

[0050] Example 16 Example 16 is based on Example 3. The difference between Example 16 and Example 3 is that in Example 16, when preparing the thermosetting phenolic resin, 159 g of boronized phenolic resin precursor and 14 g of curing agent are used.

[0051] Comparative Example 1 Comparative Example 1 is based on Example 3, and the toughening agent in Comparative Example 1 is only a boron nitride composite component.

[0052] Comparative Example 2 Comparative Example 2 is based on Example 3, and the toughening agent in Comparative Example 2 is only carbon nanotubes.

[0053] Comparative Example 3 Comparative Example 3 is based on Example 3, and the toughening agent in Comparative Example 3 is only nano boron nitride.

[0054] Comparative Example 4 Comparative Example 4 is based on Example 3, and in Comparative Example 4, naphthaleneboric acid is not added to the boronated phenolic resin precursor.

[0055] Performance testing The samples of Examples 1-16 and Comparative Examples 1-5 were sampled and subjected to the following performance tests: (1) Based on GB / T7124-2008 as the test standard, the tensile shear strength test was carried out on the samples. Each sample was tested three times, and the average value was taken. The test results were filled in Table 1.

[0056] (2) Based on GB / T2570-1995 as the testing standard, the bending performance of the samples was tested three times for each sample, and the average value was taken. The test results were filled in Table 1.

[0057] (3) Using GB / T3803-2002 as the testing standard, the impact performance test was carried out on the samples. Three samples were tested for each sample, and the average value was taken. The test results were filled in Table 1.

[0058] (4) Thermal stability test: Test the heat deformation temperature of the sample. Test each sample three times, take the average value, and fill in the test results in Table 1.

[0059] Table 1 Performance test results of samples of Examples 1-16 and Comparative Examples 1-4 Data analysis Combined with Table 1, it can be seen that the heat deformation temperature of Examples 1-3 is 226°C or above, indicating that the thermosetting phenolic resin prepared in the present application has good thermal stability; the tensile shear strength of Examples 1-3 is 13.4 MPa or above, and the flexural strength is 58.4 MPa or above, indicating that the thermosetting phenolic resin prepared in the present application has good toughness; the impact strength of Examples 1-3 is 3.34 / kJ·m -2 The above indicates that the thermosetting phenolic resin prepared in the present application has good impact resistance.

[0060] In Example 4 and Example 5, when preparing the boron nitride composite component, the mass ratios of nano-boron nitride, polyethyleneimine and dopamine are not within the range specified in the present application. When the content of dopamine is too little, the coating performance of the surface of nano-boron nitride is reduced. On the one hand, it affects the distribution uniformity of dopamine on the surface of nano-boron nitride, and on the other hand, it affects the grafting rate of polyethyleneimine, which affects the dispersibility and compatibility of nano-boron nitride. When the content of dopamine is too much, the distribution uniformity of dopamine on the surface of nano-boron nitride is reduced, which also affects the uniformity of polyethyleneimine grafting. Therefore, the performance of Examples 4 and 5 is reduced.

[0061] When there are too many or too few carbon nanotubes in the toughening agent, the overall stability of the toughening agent system is affected, but the impact is small. Therefore, the performance of Example 6 and Example 7 is reduced, but the degree of reduction is small.

[0062] In Examples 8 and 9, when preparing the phenolic resin precursor, the mass ratios of phenol, naphthalene boronic acid and formaldehyde are not within the range specified in the present application. When the content of naphthalene boronic acid is too much, the viscosity of the phenolic resin system will increase dramatically, affecting the subsequent reaction and the stability of the system. In addition, part of the formaldehyde does not participate in the reaction, and the subsequent formaldehyde overflow causes pores to remain on the resin surface, affecting the performance of the system. When the content of naphthalene boronic acid is too little, the crosslinking degree of the resin is difficult to improve, and it is difficult to form a stable three-dimensional network structure. Therefore, the various performances of Examples 8 and 9 are reduced.

[0063] In both Example 10 and Example 11, only a single modification was performed on boron nitride. Dopamine was not used, which reduced the grafting effect between polyethyleneimine and boron nitride. Polyethyleneimine was not used, which reduced the compatibility between boron nitride and the system. The improvement effect on boron nitride was reduced.

[0064] In Example 12, the nano-boron nitride is not modified, the compatibility of the boron nitride decreases, and it is difficult to further improve the strength of the system.

[0065] In Example 13 and Example 14, when preparing thermosetting phenolic resin, the content of the toughening agent is not within the range specified in the present application. Excessive toughening agent reduces the dispersion effect in the system, affecting the stability of the system; too little toughening agent makes it difficult to further enhance the improvement effect on the system, because the performance of Example 13 and Example 14 are both reduced.

[0066] In Example 15 and Example 16, when preparing thermosetting phenolic resin, the content of the curing agent used is not within the range specified in the present application. When the content of the curing agent is too little, the curing and toughening effect on the resin system is reduced; too much hexamethylenetetramine agglomerates in the system, causing the stability of the prepared phenolic resin to decrease.

[0067] The toughening agent of Comparative Example 1 is only a boron nitride composite component, which reduces the overall toughening effect of the system, and without carbon nanotubes, it is difficult to compensate for the negative effects of hexamethylenetetramine, resulting in reduced system performance.

[0068] In Comparative Example 2, the toughening agent is only carbon nanotubes, and the interface bonding performance between the toughening agent and the resin system is reduced, and the effect of improving the overall toughness of the system is also reduced.

[0069] In Comparative Example 3, the toughening agent is only nano boron nitride, which is difficult to significantly improve the resin system, and the interface bonding performance is reduced.

[0070] In Comparative Example 4, no toughening agent was added, and the comprehensive properties of the phenolic resin were difficult to be further improved.

[0071] In Comparative Example 4, naphthaleneboric acid was not used to modify the resin, and it was difficult to improve the mechanical properties and thermal stability.

[0072] This specific embodiment is only an explanation of the present application, and it is not a limitation of the present application. Through the above description, relevant staff can make various changes and modifications without deviating from the technical idea of ​​the present application. The technical scope of the present application is not limited to the content in the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A thermosetting phenolic resin with improved stability, characterized in that: The raw material components include the following mass fractions: 159-169 parts of boronized phenolic resin precursor, 7-11 parts of curing agent, 11-13 parts of toughening agent, 2-4 parts of dispersant; The boronized phenolic resin precursor raw materials include phenol, naphthaleneboric acid, formaldehyde and oxalic acid dihydrate.

2. A thermosetting phenolic resin with improved stability according to claim 1, characterized in that: The boronated phenolic resin precursor is prepared by the following method: Phenol and naphthaleneboric acid are mixed to obtain a mixture. The pH value is adjusted to acidic under oil bath conditions. After the reaction, the temperature is increased and the reaction is continued for 2 hours to obtain naphthaleneboric acid phenol ester. After the naphthaleneboric acid phenol ester is cooled, formaldehyde is added to the naphthaleneboric acid phenol ester, and then deionized water and dihydrated oxalic acid are added. The temperature is increased to react, and after washing, the mixture is distilled under reduced pressure and dehydrated to obtain a boronated phenolic resin precursor.

3. A thermosetting phenolic resin with improved stability according to claim 2, characterized in that: The mass ratio of the phenol, naphthaleneboric acid and formaldehyde is 1:(0.14-0.18):2.

45.

4. The thermosetting phenolic resin with improved stability according to claim 1, characterized in that: The toughening agent raw material comprises a boron nitride composite component and carbon nanotubes.

5. A thermosetting phenolic resin with improved stability according to claim 4, characterized in that: The boron nitride composite component raw materials include nano boron nitride, polyethyleneimine and dopamine.

6. A thermosetting phenolic resin with improved stability according to claim 4, characterized in that: The boron nitride composite component is prepared by the following method: The nano boron nitride is mixed with Tris buffer, and after ultrasonication, dopamine hydrochloride is added, and polyethyleneimine is added after stirring. After stirring, the impurities are removed by washing, and the washed material is dried to obtain a boron nitride composite component.

7. A thermosetting phenolic resin with improved stability according to claim 6, characterized in that: The mass ratio of the polyethyleneimine, dopamine and nano-boron nitride is 0.3:(0.42-0.46):

1.

8. The thermosetting phenolic resin with improved stability according to claim 4, characterized in that: The toughening agent is prepared by the following method: The carbon nanotubes are mixed with ethanol to obtain a carbon nanotube dispersion, the boron nitride composite product is mixed with ethanol to obtain a boron nitride dispersion, the carbon nanotube dispersion and the boron nitride dispersion are mixed, refluxed and stirred, and the product is then centrifuged and washed, and dried to obtain a toughening agent.

9. The thermosetting phenolic resin with improved stability according to claim 1, characterized in that: The curing agent includes hexamethylenetetramine.

10. A method for preparing the thermosetting phenolic resin with improved stability as claimed in claim 1, characterized in that: The steps include: The boronized phenolic resin is ground and heated to be in a low-viscosity state, a curing agent is added, and magnetic stirring is performed to obtain a phenolic resin system, a toughening agent and a dispersant are added to ethanol, ultrasonically dispersed, and then added to the phenolic resin system, and magnetically stirred and cured to obtain a thermosetting phenolic resin.

Citation Information

Cited By

  • Carbon nanotube modified phenolic resin and application thereof in porous carbon and silicon carbon

    CN121045734A