Gold and silver surface anti-oxidation and anti-discoloration protective agent and preparation method thereof
By combining multiple components in a gold and silver surface protectant, the problem of single-function technology in existing technologies has been solved, achieving a multi-functional protective effect. It is particularly suitable for jewelry and medical devices, improving the durability and hygiene of gold and silver surfaces.
Patent Information
- Application Number
- CN202411141941.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing gold and silver surface protectants have limited functions in terms of anti-oxidation, anti-discoloration, UV protection, antibacterial properties, and anti-corrosion, and cannot fully meet the protection needs of different environments.
A multifunctional protective agent is formed by combining water, silane coupling agent, polyvinyl alcohol, silicone oil, nano zinc oxide, polyacrylate and other components. It has anti-oxidation, anti-discoloration, anti-ultraviolet, antibacterial and anti-corrosion properties. By precisely controlling the temperature, stirring speed and pH value, the uniform distribution and stability of the components are ensured.
It provides comprehensive protection, enhancing the adhesion, weather resistance, chemical resistance, UV resistance, and antibacterial properties of gold and silver surfaces. It is suitable for high-hygiene applications such as jewelry and medical devices, extending service life and improving durability.
Smart Images

Figure CN118956260A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of gold and silver plating, and in particular to a gold and silver surface anti-oxidation and anti-discoloration protective agent and a preparation method thereof. Background Art
[0002] As a precious metal, gold and silver are widely used in jewelry, accessories, electronic products and other fields. However, gold and silver easily react with sulfides, oxygen and other substances in the air, resulting in surface oxidation and discoloration, which affects their beauty and value. Traditional anti-oxidation methods include the use of chemical coatings, electroplating, etc., but these methods often have problems such as poor durability and environmental pollution. Therefore, the market is in urgent need of an efficient and environmentally friendly anti-oxidation and anti-discoloration protective agent for the surface of gold and silver.
[0003] In the prior art, although there are some anti-oxidation protective agents, they can only provide a single protective function and cannot fully meet the protection needs of gold and silver surfaces in different environments. For example, although some protective agents can prevent oxidation, they lack anti-ultraviolet and antibacterial properties; while other protective agents have good wear resistance, they perform poorly in terms of corrosion resistance and anti-oxidation. Therefore, the development of a multifunctional and efficient anti-oxidation and anti-discoloration protective agent for gold and silver surfaces has important practical application value. Summary of the invention
[0004] The purpose of the present invention is to provide a gold and silver surface anti-oxidation and anti-discoloration protective agent and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A protective agent for preventing oxidation and discoloration of gold and silver surfaces, comprising the following ingredients:
[0007] Water ~98.0%, silane coupling agent ~0.02%, polyvinyl alcohol ~0.2%, silicone oil ~0.5%, nano zinc oxide ~0.05%, polyacrylate ~0.1%, antioxidant ~0.002%, chelating agent ~0.002%, pH regulator ~0.0002%, anti-corrosion agent ~0.002%, ultraviolet absorber ~0.005% and antibacterial agent ~0.005%.
[0008] In the present invention, the silane coupling agent is γ-aminopropyltriethoxysilane, the polyvinyl alcohol is polyvinyl alcohol with a degree of polymerization of 1700, and the organic silicone oil is dimethyl silicone oil.
[0009] In the present invention, the particle size of the nano zinc oxide is 20 to 50 nanometers, and the polyacrylate is a high molecular weight polyacrylate.
[0010] In the present invention, the antioxidant is butylated hydroxyanisole, the chelating agent is ethylenediaminetetraacetic acid, and the pH regulator is disodium hydrogen phosphate.
[0011] In the present invention, the anticorrosive agent is benzotriazole, the ultraviolet absorber is a benzotriazole ultraviolet absorber, and the antibacterial agent is a silver ion antibacterial agent.
[0012] A method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent comprises the following steps:
[0013] Step S1, adding silane coupling agent, polyvinyl alcohol, silicone oil, nano zinc oxide and polyacrylate into a reaction kettle, starting a stirring device, heating to 75° C., stirring and mixing until completely dissolved, and the reaction time is 60 minutes;
[0014] Step S2, gradually adding antioxidant, chelating agent, pH regulator, anticorrosive agent, ultraviolet absorber and antibacterial agent to the mixed solution, maintaining the reaction temperature at 75° C., continuously stirring and mixing, and the reaction time is 90 minutes;
[0015] Step S3, adjusting the pH value of the solution to 8.2;
[0016] Step S4, filtering the solution to remove insoluble matter to obtain a gold and silver surface anti-oxidation and anti-discoloration protective agent.
[0017] In the present invention, in step S1, the rotation speed of the stirring device is 150 rpm.
[0018] In the present invention, in step S1, the reaction temperature is controlled within the range of 73°C to 77°C.
[0019] In the present invention, in step S1, the heating and stirring time of the mixed solution is 60 minutes, and the stirring and mixing time is continued for 90 minutes.
[0020] In the present invention, in step S2, the speed of gradual addition is 20 ml per minute.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention provides comprehensive protection functions including anti-oxidation, anti-discoloration, anti-ultraviolet, anti-bacterial and anti-corrosion by combining multiple high-efficiency ingredients, including silane coupling agent, nano zinc oxide, polyacrylate, etc.
[0023] 2. The addition of polyvinyl alcohol and silicone oil in the present invention enhances the adhesion and film-forming property of the protective agent on the gold and silver surfaces, ensuring that the protective layer is uniform and durable. The silane film formed by the silane coupling agent and silicone oil improves the weather resistance and chemical resistance of the gold and silver surfaces, effectively preventing oxidation and discoloration.
[0024] 3. The combination of nano zinc oxide and ultraviolet absorber in the present invention provides strong anti-ultraviolet ability, and the addition of antibacterial agent prevents the growth of microorganisms. It is particularly suitable for occasions with high hygiene requirements such as jewelry and medical equipment. The introduction of polyacrylate increases the wear resistance and scratch resistance of the protective agent, making the gold and silver surface more durable. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The present invention is a schematic flow chart of a method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent. DETAILED DESCRIPTION
[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The present invention provides a technical solution:
[0028] A protective agent for preventing oxidation and discoloration of gold and silver surfaces, comprising the following ingredients:
[0029] Water ~98.0%, silane coupling agent ~0.02%, polyvinyl alcohol ~0.2%, silicone oil ~0.5%, nano zinc oxide ~0.05%, polyacrylate ~0.1%, antioxidant ~0.002%, chelating agent ~0.002%, pH regulator ~0.0002%, anti-corrosion agent ~0.002%, ultraviolet absorber ~0.005% and antibacterial agent ~0.005%.
[0030] Preferably, the silane coupling agent is γ-aminopropyltriethoxysilane;
[0031] In this embodiment, the silane coupling agent (γ-aminopropyltriethoxysilane) can form a stable silane film on the surface of gold and silver, improve the weather resistance and chemical resistance of the surface, and reduce oxidation and discoloration.
[0032] Preferably, the polyvinyl alcohol is polyvinyl alcohol having a degree of polymerization of 1700;
[0033] In this embodiment, polyvinyl alcohol enhances the adhesion and film-forming properties of the protective agent, so that the protective agent can be more evenly distributed on the surface of gold and silver, thereby improving the durability of the protective layer.
[0034] Preferably, the silicone oil is dimethyl silicone oil;
[0035] In this embodiment, the organic silicone oil (dimethyl silicone oil) provides lubrication and waterproof properties, enhances the wear resistance and scratch resistance of the protective layer, and improves the glossiness of the surface.
[0036] Preferably, the particle size of nano zinc oxide is 20 to 50 nanometers;
[0037] In this embodiment, nano zinc oxide provides anti-ultraviolet and antibacterial properties, preventing discoloration and microbial growth caused by ultraviolet rays, and is particularly suitable for outdoor and high humidity environments.
[0038] Preferably, the polyacrylate is a high molecular weight polyacrylate;
[0039] In this embodiment, polyacrylate increases the wear resistance and scratch resistance of the protective agent, making the gold and silver surface more durable while providing a certain degree of flexibility and elasticity.
[0040] Preferably, the antioxidant is butylated hydroxyanisole;
[0041] In this embodiment, the antioxidant (butylated hydroxyanisole) is used to inhibit the oxidation reaction on the metal surface, extend the service life, and prevent discoloration caused by oxidation.
[0042] Preferably, the chelating agent is ethylenediaminetetraacetic acid;
[0043] In this embodiment, the chelating agent (ethylenediaminetetraacetic acid) is used to form a stable chelate with the metal ions to prevent discoloration and corrosion caused by the metal ions.
[0044] Preferably, the pH adjuster is disodium hydrogen phosphate;
[0045] In this embodiment, the pH adjuster (disodium hydrogen phosphate) is used to adjust the pH value of the protective agent to ensure its optimal performance on the gold and silver surfaces and to prevent corrosion or other adverse reactions caused by improper pH value.
[0046] Preferably, the anticorrosion agent is benzotriazole,
[0047] In this embodiment, an anti-corrosion agent (benzotriazole) is used to provide additional anti-corrosion protection, especially in humid and corrosive environments, to prevent corrosion of gold and silver surfaces.
[0048] Preferably, the ultraviolet absorber is a benzotriazole ultraviolet absorber;
[0049] In this embodiment, the ultraviolet absorber (benzotriazole ultraviolet absorber) can further enhance the protective agent's ability to protect against ultraviolet rays, thereby preventing the coating from aging and discoloration.
[0050] Preferably, the antibacterial agent is a silver ion antibacterial agent;
[0051] In this embodiment, the antibacterial agent (silver ion antibacterial agent) is used to provide sanitary protection and prevent the growth of microorganisms, and is suitable for application scenarios requiring antibacterial properties.
[0052] Specifically, by combining a variety of high-efficiency ingredients, including silane coupling agent, nano zinc oxide, polyacrylate, etc., it provides comprehensive protection functions, including anti-oxidation, anti-discoloration, anti-ultraviolet, anti-bacterial and anti-corrosion;
[0053] Furthermore, the addition of polyvinyl alcohol and silicone oil enhances the adhesion and film-forming properties of the protective agent on the gold and silver surfaces, ensuring that the protective layer is uniform and durable. The silane film formed by the silane coupling agent and silicone oil improves the weather resistance and chemical resistance of the gold and silver surfaces, effectively preventing oxidation and discoloration.
[0054] Furthermore, the combination of nano zinc oxide and UV absorbers provides strong UV resistance, while the addition of antimicrobial agents prevents the growth of microorganisms, making it particularly suitable for applications with high hygiene requirements such as jewelry and medical equipment. The introduction of polyacrylates increases the wear and scratch resistance of the protective agent, making the gold and silver surfaces more durable.
[0055] like Figure 1 As shown, a method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent comprises the following steps:
[0056] Step S1, adding silane coupling agent, polyvinyl alcohol, silicone oil, nano zinc oxide and polyacrylate into a reaction kettle, starting a stirring device, heating to 75° C., stirring and mixing until completely dissolved, and the reaction time is 60 minutes;
[0057] In this step, the speed of the stirring device is 150 rpm; the reaction temperature is controlled within the range of 73°C to 77°C; the heating and stirring time of the mixed solution is 60 minutes, and the stirring and mixing time is continued for 90 minutes;
[0058] Step S2, gradually adding antioxidant, chelating agent, pH regulator, anticorrosive agent, ultraviolet absorber and antibacterial agent to the mixed solution, maintaining the reaction temperature at 75° C., continuously stirring and mixing, and the reaction time is 90 minutes;
[0059] In this step, the rate of gradual addition was 20 ml per minute;
[0060] Step S3, adjusting the pH value of the solution to 8.2;
[0061] Step S4, filtering the solution to remove insoluble matter to obtain a gold and silver surface anti-oxidation and anti-discoloration protective agent.
[0062] It can be understood that the precise control of temperature, stirring speed and addition speed in the above preparation method ensures sufficient mixing and reaction of the components, thereby improving the performance and stability of the protective agent; by gradually adding the components and continuously stirring, the uniform distribution of the components in the protective agent is ensured, avoiding the problem of local concentration being too high or too low; the precise adjustment of the pH value to 8.2 helps the protective agent to perform optimally on the surface of gold and silver, while preventing corrosion or other adverse reactions caused by improper pH value; the filtration step removes insoluble matter, ensures the purity and transparency of the protective agent, and improves its appearance and use effect.
[0063] The specific use steps of the gold and silver surface anti-oxidation and anti-discoloration protective agent based on the above formula and preparation method are as follows:
[0064] Step 1: Before using the protective agent, make sure the surface of gold and silver is clean, free of oil and impurities. You can use detergent to clean it and wipe it dry with a dry cloth or paper towel.
[0065] Step 2: Evenly apply the prepared gold and silver surface anti-oxidation and anti-discoloration protective agent on the gold and silver surface. You can use a sprayer, brush or cotton cloth to apply it, ensuring that all areas that need protection are covered.
[0066] Step 3: After coating, allow the protective agent to dry and solidify naturally at room temperature. Depending on the ambient temperature and humidity, it usually takes 1 to 2 hours. During the drying process, avoid touching or rubbing the coated area.
[0067] Step 4: After drying and curing, check the surface of the gold and silver to ensure that the protective agent is evenly applied and not missed. If necessary, you can make repairs or additional coatings.
[0068] Step 5. In order to maintain the best protective effect, it is recommended to reapply the protective agent regularly (such as every 3 to 6 months), especially for gold and silver products that are frequently used or exposed to harsh environments.
[0069] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A protective agent for preventing oxidation and discoloration of gold and silver surfaces, characterized in that: Includes the following ingredients: Water ~98.0%, silane coupling agent ~0.02%, polyvinyl alcohol ~0.2%, silicone oil ~0.5%, nano zinc oxide ~0.05%, polyacrylate ~0.1%, antioxidant ~0.002%, chelating agent ~0.002%, pH regulator ~0.0002%, anti-corrosion agent ~0.002%, ultraviolet absorber ~0.005% and antibacterial agent ~0.005%.
2. The gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: The silane coupling agent is γ-aminopropyltriethoxysilane, the polyvinyl alcohol is polyvinyl alcohol with a polymerization degree of 1700, and the organic silicone oil is dimethyl silicone oil.
3. The gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: The particle size of the nano zinc oxide is 20 to 50 nanometers, and the polyacrylate is a high molecular weight polyacrylate.
4. The gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: The antioxidant is butylated hydroxyanisole, the chelating agent is ethylenediaminetetraacetic acid, and the pH regulator is disodium hydrogen phosphate.
5. The gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: The anti-corrosion agent is benzotriazole, the ultraviolet absorber is a benzotriazole ultraviolet absorber, and the antibacterial agent is a silver ion antibacterial agent.
6. A method for preparing a protective agent for preventing oxidation and discoloration of gold and silver surfaces, characterized in that: The following steps are involved: Step S1, adding silane coupling agent, polyvinyl alcohol, silicone oil, nano zinc oxide and polyacrylate into a reaction kettle, starting a stirring device, heating to 75° C., stirring and mixing until completely dissolved, and the reaction time is 60 minutes; Step S2, gradually adding antioxidant, chelating agent, pH regulator, anticorrosive agent, ultraviolet absorber and antibacterial agent to the mixed solution, maintaining the reaction temperature at 75° C., continuously stirring and mixing, and the reaction time is 90 minutes; Step S3, adjusting the pH value of the solution to 8.2; Step S4, filtering the solution to remove insoluble matter to obtain a gold and silver surface anti-oxidation and anti-discoloration protective agent.
7. The method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: In the step S1, the rotation speed of the stirring device is 150 rpm.
8. The method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: In step S1, the reaction temperature is controlled within the range of 73°C to 77°C.
9. The method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: In the step S1, the heating and stirring time of the mixed solution is 60 minutes, and the stirring and mixing time is continued for 90 minutes.
10. The method for preparing a gold and silver surface anti-oxidation and anti-discoloration protective agent according to claim 1, characterized in that: In step S2, the speed of gradual addition is 20 ml per minute.
Citation Information
Patent Citations
Environment-friendly gold plating protection liquid and preparation method thereof
CN115304945A