High-temperature antioxidant bright quenching oil and preparation method thereof

By making homemade quenching base oil and combining with specific components, the problem of poor oxidation stability of quenching oil at high temperatures is solved, and a quenching oil with good oxidation resistance and brightness is achieved, and the cooling performance and surface brightness of the workpiece are optimized. .

CN118957217AInactive Publication Date: 2024-11-15AOURUM CHEM TECH CHANGZHOU CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411020606.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing quenching oil has poor oxidation stability under high temperature environments, resulting in unstable brightness performance on the surface of the workpiece. The hardenability of traditional vegetable oils is better than that of mineral oils, but the thermal stability is insufficient, making it difficult to meet the high-temperature anti-oxidation needs.

Method used

The homemade quenched base oil reacts tall oil fatty acids with neopentyl glycol through direct esterification to form a polyol with β-C only connected to methylene, eliminates the β-H structure, and combines alkylphenol polyoxyethylene ether. , sodium thiazolinyl dithiopropane sulfonate, fatty amine polyoxyethylene and sodium pentadecyl sulfonate, polyisobutyl succinimide, sodium petroleum sulfonate, alkyl dianiline and other components, through transesterification and Emulsification and synthesis technology, high-temperature antioxidant type bright quenching oil is prepared.

Benefits of technology

It improves the thermal stability and oxidation stability of the quenching oil, ensures the bright surface of the workpiece and excellent cooling performance, reduces the tissue stress during the martensite tissue transformation process, and enhances the corrosion resistance and oxidation resistance of the workpiece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004967120960000111
    Figure BDA0004967120960000111
  • Figure BDA0004967120960000121
    Figure BDA0004967120960000121
Patent Text Reader

Abstract

The invention relates to high-temperature antioxidant bright quenching oil and a preparation method thereof, and belongs to the technical field of quenching oil preparation. According to the quenching oil, the thermal oxidation stability of the quenching oil is fundamentally improved by self-preparing the quenching base oil, and then the brightness performance of the quenching oil is improved by directly compounding the alkylphenol polyoxyethylene ether, the thiazolinyl sodium dithiopropanesulfonate and the fatty amine polyoxyethylene with the quenching base oil; and finally, compounded sodium pentadecyl sulfonate, polyisobutylene succinimide, petroleum sodium sulfonate and alkyl diphenylamine are supplemented to improve the cooling performance and oxidation resistance of an oil product in high and low temperature sections, and the high-temperature anti-oxidation bright quenching oil with excellent performance is finally obtained and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to high-temperature anti-oxidation bright quenching oil and a preparation method thereof, belonging to the technical field of quenching oil preparation. Background Art

[0002] At present, quenching is a commonly used heat treatment process, which refers to the process of heating the workpiece to a certain temperature and keeping it warm for a period of time, and then cooling the workpiece with quenching oil to complete the transformation of martensite or bainite. Then, tempering at different temperatures is combined to greatly improve the strength, hardness, wear resistance, fatigue strength and toughness of the steel, so as to meet the different use requirements of various mechanical parts and tools.

[0003] The quenching oil used is a process oil used as a quenching medium. The quenching oil must have the following characteristics: good cooling performance, high flash point and ignition point, good thermal oxidation stability, low viscosity, and low moisture content. In addition to the above characteristics, the quenching oil should also be non-toxic, odorless, easy to handle, environmentally friendly, and make the surface of the workpiece bright after quenching. The quenching oil on the market often has the defect of unstable bright performance, and the vegetable oil used as the quenching base oil has higher hardenability than mineral oil. Although the quenching properties of vegetable oil are better than mineral oil and it is an excellent green and environmentally friendly quenching medium, the triglyceride structure of natural vegetable oil is easy to oxidize and decompose, and has poor thermal stability. This is because the chemical structure of triglyceride has a β-H structure, which is very easy to cause the self-decomposition of ester oil in a high temperature environment and decompose into fatty acids and olefins, which makes the thermal oxidation stability of the base quenching oil poor, which has prompted industry insiders to continuously try to improve this performance through formula adjustment.

[0004] In view of the above-mentioned defects, the designers have actively carried out research and innovation in order to create a high-temperature anti-oxidation bright quenching oil and its preparation method, so as to make it more valuable for industrial use. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a high temperature anti-oxidation bright quenching oil and a preparation method thereof.

[0006] The high-temperature anti-oxidation bright quenching oil of the present invention is characterized in that it comprises the following raw materials in parts by weight:

[0007] 83-89 parts of homemade quenching base oil;

[0008] 0.8-1.0 parts of sodium pentadecyl sulfate;

[0009] 1.0-1.2 parts of polyisobutylene succinimide;

[0010] 0.9-1.3 parts of sodium petroleum sulfonate;

[0011] 1.0-1.3 parts of alkyl diphenylamine;

[0012] The raw materials for preparing the self-made quenching base oil include tall oil fatty acid, neopentyl glycol and tin chloride.

[0013] Furthermore, the following raw materials are also included by weight:

[0014] 1-2 parts of alkylphenol polyoxyethylene ether;

[0015] 0.8-1.2 parts of sodium thiazoline dithiopropane sulfonate;

[0016] 1.0 to 1.5 parts of fatty amine polyoxyethylene.

[0017] A method for preparing high-temperature antioxidant bright quenching oil, the specific preparation steps are:

[0018] (1) A homemade quenching base oil was prepared using tall oil fatty acid, neopentyl glycol, and tin chloride;

[0019] (2) preparing a prefabricated quenching oil by using homemade quenching base oil, alkylphenol polyoxyethylene ether, sodium thiazoline disulfide propane sulfonate, and fatty amine polyoxyethylene;

[0020] (3) Prefabricated quenching oil is mixed with sodium pentadecyl sulfonate, polyisobutylene succinimide, sodium petroleum sulfonate and alkyl diphenylamine to obtain high-temperature antioxidant bright quenching oil.

[0021] Furthermore, the specific steps of preparing the homemade quenching base oil using tall oil fatty acid, neopentyl glycol and tin chloride in step (1) are:

[0022] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device, and the esterification reaction was carried out for 6 to 7 hours at a stirring rate of 300 rpm and a reaction temperature of 170 to 190° C. under nitrogen protection;

[0023] (2) After the esterification reaction is completed, the residual toluene and water in the reaction liquid are separated by pressure distillation, and the reaction liquid is washed 2 to 3 times with a saturated sodium carbonate solution to obtain a washed reaction liquid, and the washed reaction liquid is extracted with ethyl acetate, and the extract phase is placed in a vacuum distillation apparatus, and vacuum distilled at 90 to 95° C. for 30 to 40 minutes at a stirring rate of 450 to 500 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil. Without hydrogenation treatment and without adding antioxidants, oils with high oleic acid content have much higher oxidation stability than traditional oils. The present invention uses tall oil fatty acid with high oleic acid content as raw material, adopts direct esterification method, acid catalyzes fatty acid and neopentyl glycol to directly react, and finally obtains fatty acid polyol homemade quenching base oil. The homemade quenching base oil of the present invention uses chemical synthesis means of ester exchange and esterification synthesis to make the β-C of its polyol only connected to methylene in the end, so that it does not have β-H structure. β-H structure is very easy to cause self-decomposition of ester oil in high temperature environment to decompose into fatty acids and olefins. When the molecule does not contain β-H, the decomposition mechanism changes to free radical reaction, which requires higher energy to decompose, and it will only occur at a higher reaction temperature, so the thermal stability is improved, which is also the reason why the homemade quenching base oil of the present invention improves the thermal stability ability; at the same time, the homemade quenching base oil also has good quenching process performance. There is no steam film cooling period in the high temperature interval, and the cooling is more uniform. At the same time, the cooling rate in the low temperature interval is low, which can reduce the organizational stress generated by the martensitic structure transformation process. It has better cooling performance than vegetable oil and mineral oil. Through chemical synthesis methods such as transesterification and esterification synthesis, cheap natural fatty acids are chemically modified to eliminate the presence of functional groups such as β-H, optimize the chemical structure of the synthetic product, and improve the thermal stability and oxidation stability of synthetic ester oils.

[0024] Furthermore, in step (2), the specific steps of preparing the prefabricated quenching oil from the homemade quenching base oil, alkylphenol polyoxyethylene ether, sodium thiazoline disulfide propane sulfonate, and fatty amine polyoxyethylene are as follows:

[0025] By weight, 83 to 89 parts of homemade quenching base oil, 1 to 2 parts of alkylphenol polyoxyethylene ether, 0.8 to 1.2 parts of sodium thiazoline disulfide propane sulfonate and 1.0 to 1.5 parts of fatty amine polyoxyethylene are put into an emulsifying stirring kettle, and emulsified at a speed of 40 to 50 r / min for 20 to 30 minutes to obtain prefabricated quenching oil. The present invention uses nonionic surfactant alkylphenol polyoxyethylene ether as an emulsifying dispersant, and evenly disperses sodium thiazoline disulfide propane sulfonate and fatty amine polyoxyethylene in a self-made quenching base oil. During quenching, after the hot metal is quenched into the medium, a part of hydrocarbons is cracked to form free radicals, which undergo chemical reactions under the catalysis of the metal and a trace amount of water to generate aldehydes, ketones, acids, etc., and further condense into colloids, asphaltene and carbon deposits that are adsorbed on the surface of parts to pollute the parts. The addition of sodium thiazoline disulfide propane sulfonate and fatty amine polyoxyethylene as long-chain sulfonates and fatty amines can interact with the surface of the quenched parts through hydrogen bonds. Long-chain sulfonates and fatty amines will undergo a variety of chemical reactions during the high-temperature quenching process. The long-chain alkyl contained in the molecular structure of long-chain sulfonates promotes the acid-base neutralization reaction between the terminal sulfonate group and the amino group in the fatty amine to generate sulfonates and amine salts. Sulfonates make the surface of the quenched metal smoother and reduce the roughness of the surface of the quenched parts. Amine salts can improve the corrosion resistance of the quenched parts and the oxidation resistance of the quenched parts. Both of them can act as a buffer layer to prevent the oxidation products from forming large colloids that adhere to the metal surface and replace the insoluble matter that has already adhered to the metal surface to ensure the bright surface of the parts.

[0026] Furthermore, in step (3), the specific steps of mixing the prefabricated quenching oil with sodium pentadecyl sulfonate, polyisobutylene succinimide, sodium petroleum sulfonate, and alkyl diphenylamine to obtain the high-temperature antioxidant bright quenching oil are as follows:

[0027] According to the weight percentage, 0.8-1.0 parts of sodium pentadecyl sulfonate, 1.0-1.2 parts of polyisobutylene succinimide, 0.9-1.3 parts of sodium petroleum sulfonate and 1.0-1.3 parts of alkyl diphenylamine are added to the prefabricated quenching oil, and the mixture is stirred and mixed at a speed of 40-50 r / min for 1-2 hours to finally obtain a high-temperature anti-oxidation bright quenching oil. The present invention adds sodium pentadecyl sulfonate, polyisobutylene succinimide and sodium petroleum sulfonate to the quenching oil, and uses the compounding of the three to reduce the surface tension and contact angle of the quenching oil, improve the wettability of the oil product on the surface of the workpiece during the quenching process, thereby improving the cooling rate of the high and low temperature sections to a certain extent; at the same time, alkyl diphenylamine is used to improve the high-temperature anti-oxidation performance of the quenching oil.

[0028] By means of the above scheme, the present invention has at least the following advantages:

[0029] (1) Without hydrogenation treatment and without adding antioxidants, oils with high oleic acid content have much higher oxidation stability than traditional oils. The present invention uses tall oil fatty acid with high oleic acid content as raw material, adopts direct esterification method, acid catalyzes fatty acid and neopentyl glycol to directly react, and finally obtains fatty acid polyol self-made quenching base oil. The self-made quenching base oil of the present invention uses chemical synthesis means of ester exchange and esterification synthesis to make the β-C of its polyol only connected to methylene, so that it does not have β-H structure. The β-H structure is very easy to cause the ester oil to self-decompose into fatty acids and olefins under high temperature environment. When the molecule does not contain β-H, the decomposition mechanism changes to free radical reaction, which requires higher energy to decompose and will only occur at a higher reaction temperature, so the thermal stability is improved. This is also the reason why the self-made quenching base oil of the present invention improves the thermal stability ability; at the same time, the self-made quenching base oil also has good quenching process performance. There is no steam film cooling period in the high temperature range, and the cooling is more uniform. At the same time, the cooling rate in the low temperature range is low, which can reduce the tissue stress generated by the martensitic structure transformation process. It has better cooling performance than vegetable oil and mineral oil. Through chemical synthesis methods such as transesterification and esterification synthesis, cheap natural fatty acids are chemically modified to eliminate the presence of functional groups such as β-H, optimize the chemical structure of the synthetic product, and improve the thermal stability and oxidation stability of synthetic ester oils.

[0030] (2) The present invention uses nonionic surfactant alkylphenol polyoxyethylene ether as an emulsifying and dispersing agent to uniformly disperse sodium thiazolyl disulfide propane sulfonate and fatty amine polyoxyethylene in a homemade quenching base oil. This is because during quenching, after the hot metal is quenched into the medium, a portion of hydrocarbons are cracked to form free radicals, which undergo chemical reactions under the catalysis of the metal and trace amounts of water to generate aldehydes, ketones, acids, etc., and further condense into colloids, asphaltene and carbon deposits that are adsorbed on the surface of parts, polluting the parts. The addition of sodium thiazolyl disulfide propane sulfonate and fatty amine polyoxyethylene in the present invention, as long-chain sulfonates and fatty amines, can interact with the surface of the quenched parts through hydrogen bonds. Long-chain sulfonates and fatty amines will undergo a variety of chemical reactions during the high-temperature quenching process. The long-chain alkyl contained in the molecular structure of long-chain sulfonates promotes the acid-base neutralization reaction between the terminal sulfonate group and the amino group in the fatty amine to generate sulfonates and amine salts. Sulfonates make the surface of the quenched metal smoother and reduce the roughness of the surface of the quenched parts. Amine salts can improve the corrosion resistance of the quenched parts and the oxidation resistance of the quenched parts. Both of them can act as a buffer layer to prevent the oxidation products from forming large colloids that adhere to the metal surface and replace the insoluble matter that has already adhered to the metal surface to ensure the bright surface of the parts.

[0031] (3) The present invention adds sodium pentadecyl sulfonate, polyisobutylene succinimide and sodium petroleum sulfonate to the quenching oil, and uses the combination of the three to reduce the surface tension and contact angle of the quenching oil, thereby improving the wettability of the oil on the workpiece surface during the quenching process, thereby improving the cooling rate in the high and low temperature sections to a certain extent; at the same time, alkyl diphenylamine is used to improve the high-temperature antioxidant performance of the quenching oil.

[0032] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION

[0033] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.

[0034] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device, and the esterification reaction was carried out for 6 to 7 hours at a stirring rate of 300 rpm and a reaction temperature of 170 to 190° C. under nitrogen protection;

[0035] (2) After the esterification reaction is completed, the residual toluene and water in the reaction liquid are separated by pressure distillation, and the reaction liquid is washed 2 to 3 times with a saturated sodium carbonate solution to obtain a washed reaction liquid, and the washed reaction liquid is extracted with ethyl acetate, and the extracted phase is placed in a vacuum distillation apparatus, and vacuum distilled at 90 to 95° C. for 30 to 40 minutes at a stirring rate of 450 to 500 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil;

[0036] Without hydrogenation treatment and without adding antioxidants, oils with high oleic acid content have much higher oxidation stability than traditional oils. The present invention uses tall oil fatty acid with high oleic acid content as raw material, adopts direct esterification method, acid catalyzes fatty acid and neopentyl glycol to directly react, and finally obtains fatty acid polyol homemade quenching base oil. The homemade quenching base oil of the present invention uses chemical synthesis means of ester exchange and esterification synthesis to make the β-C of its polyol only connected to methylene in the end, so that it does not have β-H structure. β-H structure is very easy to cause self-decomposition of ester oil in high temperature environment to decompose into fatty acids and olefins. When the molecule does not contain β-H, the decomposition mechanism changes to free radical reaction, which requires higher energy to decompose, and it will only occur at a higher reaction temperature, so the thermal stability is improved, which is also the reason why the homemade quenching base oil of the present invention improves the thermal stability ability; at the same time, the homemade quenching base oil also has good quenching process performance. There is no steam film cooling period in the high temperature interval, and the cooling is more uniform. At the same time, the cooling rate in the low temperature interval is low, which can reduce the organizational stress generated by the martensitic structure transformation process. It has better cooling performance than vegetable oil and mineral oil. Through chemical synthesis methods such as transesterification and esterification synthesis, cheap natural fatty acids are chemically modified to eliminate the presence of functional groups such as β-H, optimize the chemical structure of the synthetic product, and improve the thermal stability and oxidation stability of synthetic ester oils.

[0037] (3) by weight, 83 to 89 parts of homemade quenching base oil, 1 to 2 parts of alkylphenol polyoxyethylene ether, 0.8 to 1.2 parts of sodium thiazoline disulfide propane sulfonate and 1.0 to 1.5 parts of fatty amine polyoxyethylene are placed in an emulsifying stirring kettle, and emulsified at a speed of 40 to 50 r / min for 20 to 30 minutes to obtain a prefabricated quenching oil;

[0038] The present invention uses nonionic surfactant alkylphenol polyoxyethylene ether as an emulsifying dispersant, and evenly disperses sodium thiazoline disulfide propane sulfonate and fatty amine polyoxyethylene in a self-made quenching base oil. During quenching, after the hot metal is quenched into the medium, a part of hydrocarbons is cracked to form free radicals, which undergo chemical reactions under the catalysis of the metal and a trace amount of water to generate aldehydes, ketones, acids, etc., and further condense into colloids, asphaltene and carbon deposits that are adsorbed on the surface of parts to pollute the parts. The addition of sodium thiazoline disulfide propane sulfonate and fatty amine polyoxyethylene as long-chain sulfonates and fatty amines can interact with the surface of the quenched parts through hydrogen bonds. Long-chain sulfonates and fatty amines will undergo a variety of chemical reactions during the high-temperature quenching process. The long-chain alkyl contained in the molecular structure of long-chain sulfonates promotes the acid-base neutralization reaction between the terminal sulfonate group and the amino group in the fatty amine to generate sulfonates and amine salts. Sulfonates make the surface of the quenched metal smoother and reduce the roughness of the surface of the quenched parts. Amine salts can improve the corrosion resistance of the quenched parts and the oxidation resistance of the quenched parts. Both of them can act as a buffer layer to prevent the oxidation products from forming large colloids that adhere to the metal surface and replace the insoluble matter that has already adhered to the metal surface to ensure the bright surface of the parts.

[0039] (4) Add 0.8-1.0 parts of sodium pentadecyl sulfonate, 1.0-1.2 parts of polyisobutylene succinimide, 0.9-1.3 parts of sodium petroleum sulfonate and 1.0-1.3 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, continue to stir and mix at a speed of 40-50 r / min for 1-2 hours, and finally prepare a high-temperature antioxidant bright quenching oil. The present invention adds sodium pentadecyl sulfonate, polyisobutylene succinimide and sodium petroleum sulfonate to the quenching oil, and uses the combination of the three to reduce the surface tension and contact angle of the quenching oil, improve the wettability of the oil on the surface of the workpiece during the quenching process, thereby improving the cooling rate of the high and low temperature sections to a certain extent; at the same time, alkyl diphenylamine is used to improve the high-temperature antioxidant performance of the quenching oil.

[0040] Example 1

[0041] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device. Under nitrogen protection, the stirring rate was 300 rpm, the reaction temperature was 170° C., and the esterification reaction was carried out for 6 hours;

[0042] (2) After the esterification reaction is completed, the residual toluene and water in the reaction solution are separated by pressure distillation, and the reaction solution is washed twice with a saturated sodium carbonate solution to obtain a washed reaction solution, and the washed reaction solution is extracted with ethyl acetate, and the extracted phase is placed in a vacuum distillation apparatus, and vacuum distilled at 90° C. for 30 minutes at a stirring rate of 450 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil;

[0043] (3) by weight, 83 parts of homemade quenching base oil, 1 part of alkylphenol polyoxyethylene ether, 0.8 parts of sodium thiazoline disulfide propane sulfonate and 1.0 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 40 r / min for 20 minutes to obtain a prefabricated quenching oil;

[0044] (4) Add 0.8 parts of sodium pentadecyl sulfonate, 1.0 parts of polyisobutylene succinimide, 0.9 parts of sodium petroleum sulfonate and 1.0 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, continue to stir and mix at a speed of 40 r / min for 1 hour, and finally obtain a high-temperature antioxidant bright quenching oil.

[0045] Example 2

[0046] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device. Under nitrogen protection, the stirring rate was 300 rpm, the reaction temperature was 175° C., and the esterification reaction was carried out for 6 hours;

[0047] (2) After the esterification reaction is completed, the residual toluene and water in the reaction liquid are separated by pressure distillation, and the reaction liquid is washed twice with a saturated sodium carbonate solution to obtain a washed reaction liquid, and the washed reaction liquid is extracted with ethyl acetate, and the extract phase is placed in a vacuum distillation apparatus, and vacuum distilled at 92° C. for 30 to 40 minutes at a stirring rate of 460 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil;

[0048] (3) by weight, 84 parts of homemade quenching base oil, 1 part of alkylphenol polyoxyethylene ether, 0.9 parts of sodium thiazoline disulfide propane sulfonate and 1.1 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 40 to 50 r / min for 22 minutes to obtain a prefabricated quenching oil;

[0049] (4) Add 0.8 parts of sodium pentadecyl sulfonate, 1.0 parts of polyisobutylene succinimide, 1.0 parts of sodium petroleum sulfonate and 1.1 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, and continue to stir and mix at a speed of 43 r / min for 1 hour to finally obtain a high-temperature antioxidant bright quenching oil.

[0050] Example 3

[0051] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device. Under nitrogen protection, the stirring rate was 300 rpm, the reaction temperature was 180° C., and the esterification reaction was carried out for 7 hours;

[0052] (2) After the esterification reaction is completed, the residual toluene and water in the reaction solution are separated by pressure distillation, and the reaction solution is washed three times with a saturated sodium carbonate solution to obtain a washed reaction solution, and the washed reaction solution is extracted with ethyl acetate, and the extract phase is placed in a vacuum distillation apparatus, and vacuum distilled at 93° C. for 35 minutes at a stirring rate of 480 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil;

[0053] (3) by weight, 86 parts of homemade quenching base oil, 2 parts of alkylphenol polyoxyethylene ether, 1.0 part of sodium thiazoline disulfide propane sulfonate and 1.3 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 45 r / min for 25 minutes to obtain a prefabricated quenching oil;

[0054] (4) Add 0.9 parts of sodium pentadecyl sulfonate, 1.1 parts of polyisobutylene succinimide, 1.2 parts of sodium petroleum sulfonate and 1.2 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, continue stirring and mixing at a speed of 45 r / min for 2 hours, and finally obtain a high-temperature antioxidant bright quenching oil.

[0055] Example 4

[0056] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device. Under nitrogen protection, the stirring rate was 300 rpm, the reaction temperature was 185° C., and the esterification reaction was carried out for 7 hours;

[0057] (2) After the esterification reaction is completed, the residual toluene and water in the reaction solution are separated by pressure distillation, and the reaction solution is washed three times with a saturated sodium carbonate solution to obtain a washed reaction solution, and the washed reaction solution is extracted with ethyl acetate, and the extract phase is placed in a vacuum distillation apparatus, and vacuum distilled at 94° C. for 38 minutes at a stirring rate of 480 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil;

[0058] (3) by weight, 88 parts of homemade quenching base oil, 2 parts of alkylphenol polyoxyethylene ether, 1.1 parts of sodium thiazoline dithiopropane sulfonate and 1.4 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 48 r / min for 28 minutes to obtain a prefabricated quenching oil;

[0059] (4) Add 0.9 parts of sodium pentadecyl sulfonate, 1.2 parts of polyisobutylene succinimide, 1.2 parts of sodium petroleum sulfonate and 1.2 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, continue stirring and mixing at a speed of 48 r / min for 2 hours, and finally obtain a high-temperature antioxidant bright quenching oil.

[0060] Example 5

[0061] (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device. Under nitrogen protection, the stirring rate was 300 rpm, the reaction temperature was 190° C., and the esterification reaction was carried out for 7 hours;

[0062] (2) After the esterification reaction is completed, the residual toluene and water in the reaction solution are separated by pressure distillation, and the reaction solution is washed three times with a saturated sodium carbonate solution to obtain a washed reaction solution, and the washed reaction solution is extracted with ethyl acetate, and the extracted phase is placed in a vacuum distillation apparatus, and vacuum distilled at 95° C. for 40 minutes at a stirring rate of 500 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil;

[0063] (3) 89 parts of homemade quenching base oil, 2 parts of alkylphenol polyoxyethylene ether, 1.2 parts of sodium thiazoline disulfide propane sulfonate and 1.5 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 50 r / min for 30 minutes to obtain a prefabricated quenching oil;

[0064] (4) Add 1.0 part of sodium pentadecyl sulfonate, 1.2 parts of polyisobutylene succinimide, 1.3 parts of sodium petroleum sulfonate and 1.3 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, continue to stir and mix at a speed of 50 r / min for 2 hours, and finally obtain a high-temperature antioxidant bright quenching oil.

[0065] Comparative Example 1

[0066] (1) by weight, 83 parts of paraffin-based white oil, 1 part of alkylphenol polyoxyethylene ether, 0.8 parts of sodium thiazoline disulfide propane sulfonate and 1.0 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 40 r / min for 20 minutes to obtain a prefabricated quenching oil;

[0067] (2) Add 0.8 parts of sodium pentadecyl sulfonate, 1.0 parts of polyisobutylene succinimide, 0.9 parts of sodium petroleum sulfonate and 1.0 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, and continue to stir and mix at a speed of 40 r / min for 1 hour to finally obtain a high-temperature antioxidant bright quenching oil.

[0068] Comparative Example 2

[0069] (1) by weight, 83 parts of high oleic soybean oil, 1 part of alkylphenol polyoxyethylene ether, 0.8 parts of sodium thiazoline disulfide propane sulfonate and 1.0 parts of fatty amine polyoxyethylene were placed in an emulsifying stirring kettle, and stirred and emulsified at a speed of 40 r / min for 20 minutes to obtain a prefabricated quenching oil;

[0070] (2) Add 0.8 parts of sodium pentadecyl sulfonate, 1.0 parts of polyisobutylene succinimide, 0.9 parts of sodium petroleum sulfonate and 1.0 parts of alkyl diphenylamine to the prefabricated quenching oil by weight, and continue to stir and mix at a speed of 40 r / min for 1 hour to finally obtain a high-temperature antioxidant bright quenching oil.

[0071] Comparative Example 3

[0072] The preparation methods of Control Example 3 and Example 1 of the present invention are basically the same, except that the alkylphenol polyoxyethylene ether, sodium thiazoline disulfide propane sulfonate and fatty amine polyoxyethylene of the present invention are not added, and other preparation raw materials and methods are the same, and quenching oil is also prepared;

[0073] Comparative Example 4

[0074] The preparation methods of Control Example 4 and Example 1 of the present invention are basically the same, except that the sodium pentadecyl sulfonate, polyisobutylene succinimide and sodium petroleum sulfonate of the present invention are not added, and the other raw materials and methods are the same, and quenching oil is also prepared;

[0075] Comparative Example 5

[0076] The preparation methods of Comparative Example 5 and Example 1 of the present invention are basically the same, except that the alkyl diphenylamine of the present invention is not added, and quenching oil is also prepared;

[0077] The performance of Examples 1-5 and Comparative Examples 1-5 of the present invention were tested respectively, and the test results are shown in Table 1:

[0078] Testing items and methods:

[0079] Kinematic viscosity test: Test according to the method of GB / T 265;

[0080] Flash point test: Tested according to the method of GB / T 3536;

[0081] Brightness test: Tested in accordance with the method in Appendix A of SH / T 0564-1993; Corrosion test: Tested in accordance with GB / T5096;

[0082] Oxidation stability test: Tested according to the method of SH / T 0219;

[0083] Cooling performance test: Tested according to the method of SH / T 0220;

[0084] Table 1 Performance test results

[0085]

[0086]

[0087] It can be seen from the test data in the above table that the quenching oils prepared in Examples 1-5 of the present invention have excellent high temperature oxidation resistance and good brightness, and can quickly cool the workpiece after quenching, with excellent performance;

[0088] Then, the performance of Control Examples 1 and 2 is compared with Example 1 of the present invention. Since Control Examples 1 and 2 use mineral oil and vegetable oil instead of the homemade base oil of the present invention, respectively, the high-temperature oxidation stability of the final quenching oil is significantly reduced. It can be confirmed that the present invention adopts a direct esterification method, and acid-catalyzed fatty acids and neopentyl glycol directly react to finally obtain a homemade quenching base oil of fatty acid polyesters. The homemade quenching base oil of the present invention is synthesized by chemical synthesis means of ester exchange and esterification synthesis so that the β-C of the polyol is only connected to the methylene group, so that it does not have a β-H structure. The β-H structure is very easy to cause the self-decomposition of ester oils in a high temperature environment to decompose into fatty acids and olefins. When the molecule does not contain β-H, the decomposition mechanism is changed to a free radical reaction, which requires higher energy to decompose and will only occur at a higher reaction temperature. Therefore, the thermal stability is improved, which is also the reason why the homemade quenching base oil of the present invention improves the thermal stability capability; at the same time, the homemade quenching base oil also has good quenching process performance. There is no steam film cooling period in the high temperature range, and the cooling is more uniform. At the same time, the cooling rate in the low temperature range is low, which can reduce the tissue stress generated by the martensitic transformation process. It shows better cooling performance than vegetable oil and mineral oil. Through chemical synthesis methods such as ester exchange and esterification synthesis, cheap natural fatty acids are chemically modified to eliminate the presence of functional groups such as β-H, optimize the chemical structure of the synthetic product, and improve the thermal stability and oxidation stability of synthetic ester oils.

[0089] The performance of the control example 3 and the embodiment 1 of the present invention are compared. Since the alkylphenol polyoxyethylene ether, sodium thiazolinyl dithiopropane sulfonate and fatty amine polyoxyethylene of the present invention are not added in the control example 3, the brightness of the final quenching oil is significantly reduced. It can be confirmed that the present invention uses the non-ionic surfactant alkylphenol polyoxyethylene ether as an emulsifying dispersant, and the sodium thiazolinyl dithiopropane sulfonate and fatty amine polyoxyethylene are uniformly dispersed in the homemade quenching base oil. Because during quenching, after the hot metal is quenched into the medium, a part of the hydrocarbons are cracked to form free radicals, which react chemically under the catalysis of the metal and a trace amount of water to generate aldehydes, ketones, acids, etc., and further condense into colloids, asphaltene and carbon deposits adsorbed on the surface of parts, polluting the parts. The addition of sodium thiazolinyl dithiopropane sulfonate and fatty amine polyoxyethylene of the present invention, as long-chain sulfonates and fatty amines, can interact with the surface of the quenched parts through hydrogen bonds. Long-chain sulfonates and fatty amines will undergo a variety of chemical reactions during the high-temperature quenching process. The long-chain alkyl contained in the molecular structure of long-chain sulfonates promotes the acid-base neutralization reaction between the terminal sulfonate group and the amino group in the fatty amine to generate sulfonates and amine salts. Sulfonates make the surface of the quenched metal smoother and reduce the roughness of the surface of the quenched parts. Amine salts can improve the corrosion resistance of the quenched parts and the oxidation resistance of the quenched parts. Both of them can act as a buffer layer to prevent the oxidation products from forming large colloids that adhere to the metal surface and replace the insoluble matter that has already adhered to the metal surface to ensure the bright surface of the parts.

[0090] Finally, the performance of the control examples 4-5 of the present invention and the embodiment 1 of the present invention is compared. Since the control example 4 does not add the sodium pentadecyl sulfonate, polyisobutylene succinimide and sodium petroleum sulfonate of the present invention, and the control example 5 does not add the alkyl diphenylamine of the present invention, the cooling rate and the antioxidant performance of the final quenching oil are significantly reduced. It can be confirmed that the present invention adds sodium pentadecyl sulfonate, polyisobutylene succinimide and sodium petroleum sulfonate to the quenching oil, and uses the compound of the three to reduce the surface tension and contact angle of the quenching oil, improve the wettability of the oil on the workpiece surface during the quenching process, thereby improving the cooling rate of the high and low temperature sections to a certain extent; at the same time, the high temperature antioxidant performance of the quenching oil is improved by using alkyl diphenylamine.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the technical principles of the present invention, and these improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A high temperature anti-oxidation bright quenching oil, characterized by: The following raw materials are included by weight: 83-89 parts of homemade quenching base oil; 0.8-1.0 parts of sodium pentadecyl sulfate; 1.0-1.2 parts of polyisobutylene succinimide; 0.9-1.3 parts of sodium petroleum sulfonate; 1.0-1.3 parts of alkyl diphenylamine; The raw materials for preparing the self-made quenching base oil include tall oil fatty acid, neopentyl glycol and tin chloride.

2. The high temperature anti-oxidation bright quenching oil according to claim 1, characterized in that: The following raw materials are also included by weight: 1-2 parts of alkylphenol polyoxyethylene ether; 0.8-1.2 parts of sodium thiazolyl dithiopropane sulfonate; 1.0 to 1.5 parts of fatty amine polyoxyethylene.

3. The method for preparing a high temperature anti-oxidation bright quenching oil as claimed in claim 2, characterized in that The specific preparation steps are: (1) A homemade quenching base oil was prepared using tall oil fatty acid, neopentyl glycol, and tin chloride; (2) preparing a prefabricated quenching oil by using a homemade quenching base oil, alkylphenol polyoxyethylene ether, sodium thiazoline disulfide propane sulfonate, and fatty amine polyoxyethylene; (3) Prefabricated quenching oil is mixed with sodium pentadecyl sulfonate, polyisobutylene succinimide, sodium petroleum sulfonate and alkyl diphenylamine to obtain high-temperature antioxidant bright quenching oil.

4. The method for preparing a high temperature anti-oxidation bright quenching oil according to claim 3, characterized in that: The specific steps of preparing the homemade quenching base oil using tall oil fatty acid, neopentyl glycol and tin chloride in step (1) are: (1) tall oil fatty acid and neopentyl glycol were mixed in an alcohol-acid molar ratio of 1:3 and added to an esterification reaction device, and then 1% by weight of tin chloride was added to the esterification reaction device, and the esterification reaction was carried out for 6 to 7 hours at a stirring rate of 300 rpm and a reaction temperature of 170 to 190° C. under nitrogen protection; (2) After the esterification reaction is completed, the residual toluene and water in the reaction liquid are separated by pressure distillation, and the reaction liquid is washed 2 to 3 times with a saturated sodium carbonate solution to obtain a washed reaction liquid, and the washed reaction liquid is extracted with ethyl acetate, and the extract phase is placed in a vacuum distillation apparatus, and vacuum distilled at 90 to 95° C. for 30 to 40 minutes at a stirring rate of 450 to 500 rpm and a vacuum degree of 0.3 kPa to separate and remove ethyl acetate to obtain a homemade quenching base oil.

5. The method for preparing a high temperature anti-oxidation bright quenching oil according to claim 3, characterized in that: In the step (2), the specific steps of preparing the prefabricated quenching oil by using the homemade quenching base oil, alkylphenol polyoxyethylene ether, sodium thiazoline disulfide propane sulfonate, and fatty amine polyoxyethylene are as follows: By weight, 83 to 89 parts of homemade quenching base oil, 1 to 2 parts of alkylphenol polyoxyethylene ether, 0.8 to 1.2 parts of sodium thiazoline disulfide propane sulfonate and 1.0 to 1.5 parts of fatty amine polyoxyethylene are put into an emulsifying stirring kettle, and emulsified at a speed of 40 to 50 r / min for 20 to 30 minutes to obtain prefabricated quenching oil.

6. The method for preparing a high temperature anti-oxidation bright quenching oil according to claim 3, characterized in that: The specific steps of preparing the high-temperature antioxidant bright quenching oil by mixing the prefabricated quenching oil with sodium pentadecyl sulfonate, polyisobutylene succinimide, sodium petroleum sulfonate and alkyl diphenylamine in step (3) are as follows: According to weight proportions, 0.8-1.0 parts of sodium pentadecyl sulfonate, 1.0-1.2 parts of polyisobutylene succinimide, 0.9-1.3 parts of sodium petroleum sulfonate and 1.0-1.3 parts of alkyl diphenylamine are added to the prefabricated quenching oil, and the mixture is stirred at a speed of 40-50 r / min for 1-2 hours to finally obtain a high-temperature antioxidant bright quenching oil.

Citation Information

Cited By

  • Quenching agent for heat treatment and alkaline high-molecular polymer thereof

    CN122444906A