Method for recycling valuable metal in lithium ion battery positive electrode material
By employing a calcination process containing zinc sulfide and reducing agent, the problem of separating lithium from cobalt and nickel in lithium-ion battery cathode materials has been solved, achieving efficient recovery and low-cost lithium extraction, and providing high-quality nickel matte raw materials.
Patent Information
- Application Number
- CN202411027859.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing sulfidation method for lithium-ion battery cathode materials suffers from severe equipment corrosion, generates a large amount of waste gas, and introduces impurities that are difficult to separate, resulting in a complex and costly recycling process.
The positive electrode material of lithium-ion batteries is calcined by mixing zinc-containing sulfiding agents and reducing agents, and the oxygen volume fraction in the calcination atmosphere is controlled to be less than 5%. This forms lithium sulfate or oxide and cobalt and nickel sulfides. Zinc vapor volatilizes and is oxidized to zinc oxide, thus separating lithium from cobalt and nickel. The resulting sulfides are used as high-quality nickel matte raw materials and enter the nickel smelting system.
It achieves efficient separation of lithium and cobalt-nickel, with a lithium leaching rate of over 98% and a cobalt-nickel recovery rate of over 95%, reducing subsequent separation steps, lowering costs, and providing high-quality nickel matte feedstock.
Smart Images

Figure CN118957265A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recycling, and more specifically, relates to a method for recycling valuable metals in positive electrode materials of lithium-ion batteries. Background Art
[0002] Lithium-ion batteries are widely used in electric vehicles, communications, electronic equipment and other fields because of their long cycle life, large capacity and light weight. With the rapid increase in the use of lithium-ion batteries, it is expected that waste lithium-ion batteries will reach a peak of scrapping by 2025. Waste lithium-ion batteries contain toxic electrolytes and organic diaphragms, which will cause irreversible damage to soil and water quality. In addition, they contain a large amount of strategic key metals Li (2-3%), Co (5-30%), Ni (0.02-10%), and Cu (7-17%). If they are not recycled, it will cause a huge waste of resources. Therefore, the development of a green and efficient recovery process for valuable elements in waste lithium-ion batteries will not only help solve environmental pollution problems, but also ease the global energy metal resource tension. Pyrometallurgy has strong adaptability to raw materials, short process, high recovery rate of cobalt, nickel and copper, and large processing volume, but the lithium grade in slag phase is low and difficult to recover; hydrometallurgy has low investment, flexible production, good comprehensive metal recovery effect, high product purity, but long process, complex process, high cost of wastewater and waste residue treatment, and usually puts lithium recovery in the last step of the process, resulting in a large amount of lithium loss. The sulfidation method takes into account the advantages of both pyrometallurgy and hydrometallurgy. The existing sulfidation recovery methods are mainly divided into the following two categories: selective recovery of lithium by sulfate and selective recovery of lithium by sulfide.
[0003] After searching, the patent application document with Chinese patent application number 201710500482.0 and application publication date September 29, 2017 discloses a method for recovering lithium from waste lithium batteries. The method mixes the waste lithium battery positive electrode powder with a sulfiding agent and calcines it, and then separates the solid and liquid to obtain a lithium-containing aqueous solution. However, the sulfiding agent used in this process enters the solution, which will have an adverse effect on the subsequent separation and purification of lithium. On the other hand, the sulfide ore used as the sulfur source introduces new metal impurities, which is not conducive to the subsequent recovery of Co and purification of the product.
[0004] The patent application document with Chinese patent application number 202110552481.7 and application publication date of August 20, 2021 discloses a method for recovering lithium from waste lithium-ion battery positive electrode materials. The method mixes waste lithium-ion battery positive electrode materials with (NH4)2SO4 for sulfuric acid roasting, destroys the layered structure of the positive electrode material so that lithium ions can be smoothly released, and then the roasting product is leached in water to obtain a lithium-rich leachate and a transition metal oxide slag phase. After the leachate is purified by impurities removal, ammonium carbonate is added, and lithium is recovered in the form of Li2CO3 precipitation at a certain temperature. After lithium precipitation, the liquid is evaporated and crystallized to prepare (NH4)2SO4, thereby realizing the recovery of lithium in waste lithium-ion battery positive electrode materials and the recycling of (NH4)2SO4. At the same time, the lithium-containing residual liquid can be recycled in the water leaching stage. In order to avoid the decomposition of ammonium carbonate, the reaction temperature of this process is controlled at a relatively low level, the lithium precipitation time is long, and the lithium precipitation is incomplete. Although the remaining lithium will be brought into the ammonium sulfate and residual liquid return system for closed circulation, the lithium precipitation efficiency is low, which will lead to increased costs.
[0005] The patent application document with Chinese patent application number 202310395906.7 and application publication date July 11, 2023 discloses a method for selectively recovering lithium from lithium batteries. The patent method is method 1: roasting a mixture of lithium battery pole powder, ammonium sulfate and carbon powder, and leaching the roasted product to obtain a lithium leachate; or, method 2: roasting a mixture of lithium battery pole powder and ammonium sulfate, adding alkaline solution to the roasted product after leaching to obtain a lithium leachate; or, method 3: roasting a mixture of lithium battery pole powder, ammonium sulfate and carbon powder, adding alkaline solution to the roasted product after leaching to obtain a lithium leachate. This process uses sulfur and ammonia as a vulcanizing agent, which will not only cause corrosion to electrical equipment, but also produce a large amount of ammonia-containing wastewater.
[0006] Therefore, it is an urgent problem to propose a new method for recovering valuable metals in lithium-ion battery positive electrode materials to improve the recycling process cycle and efficiently recover valuable metals. Summary of the invention
[0007] 1. Problem to be solved
[0008] In view of the problems faced by the existing sulfurization method of lithium-ion battery positive electrode materials, such as high degree of equipment corrosion, large amount of waste gas generation, and introduction of impurities that are difficult to separate, the present invention provides a method for valuable metals in lithium-ion battery positive electrode materials. By optimizing the recovery system formula, high-value metals such as cobalt and nickel in the battery can be simultaneously processed without introducing new impurities, reducing the burden of subsequent separation and impurity removal, thereby achieving the effect of lithium extraction through a short process. At the same time, the obtained sulfide can be used as a high-quality nickel matte raw material for nickel smelting enterprises to enter their smelting system for separation and recovery.
[0009] 2. Technical solution
[0010] In order to solve the above problems, the technical solution adopted by the present invention is as follows:
[0011] A method for recovering valuable metals in lithium-containing slag, comprising the steps of:
[0012] S1. Calcination process:
[0013] The positive electrode material of the lithium ion battery, the zinc-containing vulcanizing agent and the reducing agent are mixed and then roasted, and the volume fraction of oxygen in the roasting atmosphere is controlled to be less than 5% to obtain a roasting product and zinc oxide smoke.
[0014] Since the most valuable cobalt and nickel in the positive electrode material are sulfur-loving elements, they are very easy to form water-insoluble sulfides (Co3S4, CoS, NiS) with negative divalent sulfur, while the lithium in the positive electrode powder is more oxygen-loving and can form water-soluble sulfates during the sulfidation process, thereby achieving the separation of lithium from cobalt and nickel.
[0015] The reducing agent has two functions. One is to maintain the sulfur combined with cobalt and nickel as negative divalent sulfur. When the sulfiding agent is sulfate, it can also reduce the sulfate ion to negative divalent sulfur to combine with cobalt and nickel. The second is to reduce the metallic zinc in the sulfiding agent to convert it into zinc vapor and volatilize it into the flue gas without introducing new metal impurities.
[0016] The purpose of controlling the oxygen content is to maintain a relatively weak reducing atmosphere. On the one hand, it can promote the zinc vapor generated by reduction to be oxidized into zinc oxide in the flue gas for recovery. On the other hand, it can convert lithium and other substances into sulfate, which is beneficial for subsequent leaching and recovery. If the oxygen content is too low, it will easily cause an increase in the consumption of reducing agents. At the same time, it is difficult for zinc vapor to be converted into safe and stable zinc oxide smoke. If it is liquefied or even solidified in the flue gas system, it is very easy to corrode and clog the equipment.
[0017] S2, lithium extraction process:
[0018] The roasted product of step S1 is leached in water, and then solid-liquid separation is performed to obtain a leaching solution and a leaching residue, wherein the leaching solution is a lithium-containing solution, and the leaching residue contains cobalt and / or nickel sulfides.
[0019] Furthermore, in step S1, the positive electrode material of the lithium-ion battery can be a positive electrode material of a waste lithium-ion battery, including but not limited to positive electrode powder obtained by disassembling at least one of lithium cobalt oxide batteries, lithium nickel oxide batteries, lithium manganese oxide batteries, nickel manganese lithium batteries, nickel cobalt lithium batteries, nickel cobalt manganese ternary lithium batteries, and nickel cobalt aluminum ternary lithium batteries, preferably at least one of lithium nickel oxide batteries, lithium cobalt oxide batteries, and nickel cobalt manganese ternary lithium batteries.
[0020] Furthermore, in step S1, the zinc-containing vulcanizing agent is at least one of ZnS, sphalerite, zinc sulfate, and basic zinc sulfate, preferably at least one of ZnS, sphalerite, and anhydrous zinc sulfate.
[0021] Furthermore, in step S1, the reducing agent is a reducing agent containing hydrogen or carbon, including but not limited to at least one of H2, graphite, carbon powder, coke, and coal powder.
[0022] Furthermore, in step S1, the mass ratio of the reducing agent to the zinc-containing vulcanizing agent added is (0.5-1.5):1.
[0023] Furthermore, in step S1, the mass ratio of the zinc-containing vulcanizing agent to the lithium-ion battery positive electrode material is (1-3):1, preferably (1.5-2.5):1.
[0024] Furthermore, in step S1, the roasting temperature is 600-1250°C, preferably 1000-1200°C; the roasting time is 0.5-3h, preferably 1.5-2h. The influence of roasting temperature: (1) affects the reaction rate, and thus affects the production efficiency. The higher the temperature, the faster the reaction rate and the better the production efficiency. However, too high a temperature will greatly increase energy consumption. (2) affects the existence state of zinc. Zinc is a low-melting-point volatile metal (melting point 420°C, boiling point 907°C). When the temperature exceeds 800°C, liquid zinc begins to evaporate violently into zinc vapor.
[0025] Furthermore, in step S1, the means for controlling the roasting environment to control the oxygen volume fraction in the roasting atmosphere to be lower than 5% is to adjust the flow rates of oxygen and (or) air and inert gas nitrogen in the ventilation device.
[0026] Furthermore, in step S2, the water immersion temperature is 10-80°C, the leaching time is 2 min-2 h, and the liquid-to-solid ratio is (3-50):1 mL / g, preferably 40-60°C, 10-30 min, (10-20):1 mL / g.
[0027] Furthermore, in step S2, the concentrations of impurities Co, Ni, Zn and Mn in the leaching solution are all less than 0.1 mg / L, and the leaching recovery rate of lithium is >98%.
[0028] Furthermore, in step S2, the main components of the leached slag are Co content of 15-55wt%, Ni content of 10-63wt%, S content of 20-35wt%, and the sulfidation recovery of cobalt and nickel are both >95%.
[0029] The above method for recovering valuable metals in lithium-containing slag can be applied to recover positive electrode materials of lithium-ion batteries. It can solve the problems faced by the existing sulfurization method of waste lithium-ion batteries, such as high degree of equipment corrosion, large amount of waste gas generation, and difficulty in separating impurities, and can simultaneously process high-value metals such as cobalt and nickel in the battery. Since the sulfides of lithium, cobalt and nickel have wider property difference bands than oxides, it is easier to achieve deep separation. In view of this, the present invention, based on the sulfide ore formation principle, proposes a new method for selective lithium extraction by sulfidation of waste lithium-ion battery positive electrode materials. Specifically, waste lithium battery positive electrode materials are used as raw materials, a zinc-containing sulfiding agent, waste lithium battery positive electrode materials, and a reducing agent are mixed and roasted in a certain proportion, and the roasted slag is then soaked in water to obtain a lithium-containing solution with a low impurity content. High-value metals such as nickel and cobalt form sulfides that are insoluble in water and can be sent to a nickel smelter as matte products, while zinc is reduced and the zinc vapor is further oxidized to zinc oxide and enters the smoke. Lithium can be separated from cobalt, nickel and zinc through a one-step reduction sulfidation roasting process, thereby achieving the effect of lithium extraction in a short process. At the same time, the obtained sulfides can be used as high-quality nickel matte raw materials of nickel smelting enterprises to enter their smelting system for separation and recovery.
[0030] 3. Beneficial effects
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) Good selectivity
[0033] The invention is based on the significant difference in sulfur affinity between lithium, cobalt and nickel. In the reduction sulfurization roasting process, the affinity of cobalt and nickel to sulfur is stronger, forming water-insoluble sulfides, and the sulfurization recovery rates of cobalt and nickel are greater than 95%. Lithium is more oxygen-affinity and is finally converted into soluble lithium sulfate or lithium oxide. The concentrations of impurities cobalt, nickel and manganese in the lithium-containing leachate obtained after water leaching are all less than 0.1 mg / L, and the leaching rate of lithium exceeds 98%. For zinc, in the reduction sulfurization roasting process, the zinc-containing compound first volatilizes into the flue gas as zinc vapor under a reducing atmosphere, but will continue to be oxidized by the flue gas containing carbon dioxide to stably exist in the flue dust, and will not enter the cobalt and nickel sulfide products and the lithium-containing leachate, so as not to affect the purity of the product.
[0034] (2) Zinc compounds are cheap and easy to obtain
[0035] The present invention can use sphalerite widely existing in nature or zinc sulfate as a vulcanizing agent. The raw material is cheap and easy to obtain. The raw material is the positive electrode material obtained by disassembling waste lithium-ion batteries. In addition, sulfide is a zinc-containing compound, and its source is wide. In addition to chemical products, zinc sulfide concentrate widely existing in nature can also be used.
[0036] (3) The products obtained are widely used in the future
[0037] The cobalt-nickel sulfide product obtained by this method is a high-quality "nickel matte", which can be used as a high-quality intermediate material for nickel smelting enterprises and enter the blowing process of "nickel matte", thereby minimizing the cost of developing independent recovery and separation of cobalt and nickel wet separation technology routes, and realizing the coordinated disposal of lithium-containing waste batteries and existing typical heavy metals. For lithium, the concentration of impurity ions in the Li-containing solution obtained after simple sulfurization roasting-water leaching treatment is low, and the concentrations of Ni, Co, Al, Si, and Mn are all lower than 0.1ppm. There is no need for subsequent complicated separation processes. It can be used as a high-quality lithium-containing raw material, which can be simply removed and concentrated and crystallized, and high-purity Li2CO3 can be produced by passing CO2 or adding potassium or sodium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a process flow chart of the recovery method of the present invention;
[0039] Figure 2 is the XRD pattern of the leached residue in Example 15;
[0040] Figure 3 This is the SEM image of the leached residue in Example 15. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with specific embodiments.
[0042] Examples 1-26
[0043] like Figure 1 As shown, the method for recovering valuable metals in lithium-containing slag comprises the following steps:
[0044] S1. Calcination process:
[0045] Waste battery positive electrode materials from different sources are mixed evenly with different vulcanizing agents and different reducing agents according to the addition amounts in Table 1 and then calcined, maintaining the oxygen content in the atmosphere and the rest being N2. The calcination temperature and calcination time are as shown in Table 2 to obtain calcined products and zinc oxide smoke.
[0046] S2, lithium extraction process:
[0047] The roasted product of step S1 is water-leached at a water-leaching temperature of 60°C, a leaching time of 2h, and a liquid-solid ratio of slag to water of 20:1mL / g; solid-liquid separation is then performed to obtain a leachate, leached slag, and zinc oxide smoke, wherein the leachate is a lithium-containing solution, and the contents of cobalt, nickel, zinc, and manganese in the lithium-containing solution are all less than 0.1ppm, and the leached slag contains cobalt and / or nickel sulfides. The recovery rates of lithium, nickel, and cobalt are shown in Table 2. Figure 2 and Figure 3 Shown are the XRD and SEM images of the leached residue in Example 15, respectively.
[0048] It should be noted that during the sulfidation roasting of lithium nickel cobalt manganese oxide, there will be no manganese in the solution. The main reason is that: although manganese is also oxygen-philic, manganese oxides or sulfides are insoluble in water. Even if manganese sulfate is generated during the sulfidation roasting process, manganese will be hydrolyzed into manganese hydroxide during water leaching and precipitated into the leaching residue, thereby separating it from lithium.
[0049] Table 1 Types and addition amounts of positive electrode materials, zinc-containing vulcanizing agents and reducing agents for lithium-ion batteries
[0050]
[0051]
[0052] Table 2 Roasting parameters and valuable metal recovery
[0053]
[0054]
[0055] It is worth noting that the reaction conditions in the above embodiments are all the optimal reaction conditions for the reaction, and the reaction conditions within the scope of the claims can synthesize the complex of the present invention. In order to avoid redundancy, no examples are given here; in addition, those skilled in the art can reproduce the present invention based on the general formula of the complex of the present invention and the listed related solvents, catalysts and other reagents. Since there are too many examples, several representative examples are selected here, which are sufficient to prove that the complex of the present invention has excellent luminescence efficiency and low oxygen quenching rate, so the examples are not repeated here.
Claims
1. A method for recovering valuable metals in positive electrode materials of lithium-ion batteries, characterized in that: The positive electrode material of a lithium-ion battery, a zinc-containing vulcanizing agent and a reducing agent are mixed and then roasted, the oxygen volume fraction in the roasting atmosphere is controlled to be less than 5%, the roasted product is then leached in water, and finally solid-liquid separation is performed to obtain a leachate and a leach residue, wherein the leachate is a lithium-containing solution, and the leach residue contains cobalt and / or nickel sulfides.
2. The method for recovering valuable metals in positive electrode materials of lithium ion batteries according to claim 1, characterized in that: The positive electrode material of lithium-ion batteries is the positive electrode material of waste lithium-ion batteries, including positive electrode powder obtained by disassembling at least one of lithium cobalt oxide batteries, lithium nickel oxide batteries, lithium manganese oxide batteries, nickel manganese lithium batteries, nickel cobalt lithium batteries, nickel cobalt manganese ternary lithium batteries, and nickel cobalt aluminum ternary lithium batteries.
3. The method for recovering valuable metals in positive electrode materials of lithium ion batteries according to claim 1, characterized in that: The zinc-containing vulcanizing agent is at least one of ZnS, sphalerite, zinc sulfate, and basic zinc sulfate.
4. The method for recovering valuable metals in positive electrode materials of lithium ion batteries according to claim 1, characterized in that: The reducing agent is a reducing agent containing hydrogen or carbon.
5. The method for recovering valuable metals in positive electrode materials of lithium ion batteries according to claim 1, characterized in that: The mass ratio of reducing agent to zinc-containing vulcanizing agent added is (0.5-1.5):
1.
6. The method for recovering valuable metals in positive electrode materials of lithium-ion batteries according to claim 1, characterized in that: The mass ratio of the zinc-containing vulcanizing agent to the lithium-ion battery positive electrode material is (1-3):1, preferably (1.5-2.5):
1.
7. The method for recovering valuable metals in positive electrode materials of lithium ion batteries according to claim 1, characterized in that: The calcination temperature is 600-1250° C., preferably 1000-1200° C.; the calcination time is 0.5-3 h, preferably 1.5-2 h.
8. The method for recovering valuable metals in positive electrode materials of lithium-ion batteries according to claim 1, characterized in that: The calcining atmosphere also contains inert gas.
9. The method for recovering valuable metals in positive electrode materials of lithium-ion batteries according to claim 1, characterized in that: The immersion temperature is 10-80°C, the leaching time is 2min-2h, and the liquid-to-solid ratio is (3-50):1mL / g; preferably, the immersion temperature is 40-60°C, the leaching time is 10-30min, and the liquid-to-solid ratio is (10-20):1mL / g.
10. The method for recovering valuable metals in positive electrode materials of lithium-ion batteries according to any one of claims 1 to 9, characterized in that: The concentrations of impurities Co, Ni, Zn and Mn in the leaching solution are all less than 0.1 mg / L, and the leaching recovery rate of lithium is >98%; the main components of the leaching residue are Co content 15-55wt%, Ni content 10-63wt%, S content 20-35wt%, and the sulfide recovery of cobalt and nickel is >95%.
Citation Information
Patent Citations
Method for recycling valuable metals in waste lithium ion batteries
CN111733328A
Synergistic resource recycling method for industrial sulfate solid waste and waste nickel-cobalt-manganese-lithium series batteries
CN115367732A
Valuable metal recovery method
CN116804243A
Valuable metal recovery method
CN116926331A
Method for extracting lithium from positive electrode material of waste lithium ion battery
CN117144143A