Nanometer AlN particle reinforced magnesium-based composite material capable of achieving strength and toughness synergistic improvement and preparation method of nanometer AlN particle reinforced magnesium-based composite material

Through the combination of powder metallurgy technology and process, the problem of poor dispersion of nanoceramic particles in magnesium-based composite materials is solved, and the strength and strength of magnesium alloys are improved significantly, which significantly improves the mechanical properties of the materials.

CN118957346AActive Publication Date: 2024-11-15UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202411050025.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prepare magnesium-based composite materials with uniformly dispersed nanoceramic particles at low cost, resulting in less obvious improvement in strength and toughness of magnesium alloys or worsen performance.

Method used

NanoAlN-Al intermediate alloys are prepared through powder metallurgy technology, and combined with ball milling, cold compaction, hot sintering, solid solution treatment and hot extrusion processes, the uniform dispersion and tissue optimization of nanoAlN particles in the magnesium alloy matrix are achieved, and the composite is improved Mechanical properties of materials.

Benefits of technology

The preparation of low-cost and high-performance magnesium-based composite materials is realized, which significantly improves the strength and toughness of magnesium alloys, improves the dispersion quality of nanoparticles, closes the cast structure defects, and promotes dynamic recrystallization and grain refinement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957346A_ABST
    Figure CN118957346A_ABST
Patent Text Reader

Abstract

The invention provides a nanometer AlN particle reinforced magnesium-based composite material for achieving strength and toughness synergistic improvement and a preparation method of the nanometer AlN particle reinforced magnesium-based composite material, and belongs to the field of magnesium alloy preparation and processing. The AlN nano ceramic particles and the micron-sized Al powder are mixed and subjected to powder metallurgy to prepare the AlN-Al intermediate alloy, and then the AlN-Al intermediate alloy is used in the stirring casting preparation process of the magnesium-based composite material. And the obtained as-cast magnesium-based composite material is subjected to solution treatment to achieve structure homogenization and control of precipitated phase remelting, finally, hot extrusion is conducted to close microstructure defects, meanwhile, grain refinement is achieved through a dynamic recrystallization mechanism, and finally the strength and toughness synergistic mechanical property improvement of the magnesium-based composite material is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of magnesium alloy preparation and processing, and in particular relates to a nano-AlN particle reinforced magnesium-based composite material achieving synergistic improvement in strength and toughness and a preparation method thereof. Background Art

[0002] Magnesium alloys are considered to be one of the most promising structural materials due to their low density and good electromagnetic shielding properties. However, their poor strength and toughness limit their wide application in engineering. In order to achieve the synergistic improvement of the strength and toughness of magnesium alloys, the preparation of magnesium-based composites reinforced with ceramic particles has been conceptualized and studied, and some progress has been made. For Mg-Zn-Zr alloys, although their strength is slightly higher than that of magnesium alloys such as Mg-Al-Zn, their toughness is poor. Therefore, the preparation of Mg-Zn-Zr-based composites by adding ceramic particles is expected to further improve the comprehensive performance of Mg-Zn-Zr alloys in terms of strength and toughness matching.

[0003] Studies have shown that nano-ceramic particles can promote the particle hardening mechanism more effectively than micro-ceramic particles, thereby significantly improving the strength of composite materials. However, due to the stronger van der Waals force between nanoparticles, they are more likely to cluster, and then stress concentration occurs during the application of external loads, thereby inducing micro-damage. Therefore, the dispersion quality of nano-ceramic particles in the magnesium alloy matrix has a crucial influence on the performance of magnesium-based composites and is a huge challenge in the preparation of magnesium-based composites. In the process of casting to prepare magnesium-based composites, the use of methods such as mechanical stirring, ultrasonic vibration, and in-situ synthesis of particles has limited effects on the uniform dispersion of nanoparticles, resulting in no obvious performance improvement or even performance deterioration; although powder metallurgy technology has been used to prepare magnesium-based composites and has obtained relatively uniform nanoparticle dispersion quality and excellent mechanical properties, its product size is limited and the preparation cost is high. Therefore, it is very necessary to develop a low-cost technology for preparing magnesium-based composites with uniform dispersion of nano-ceramics and synergistic improvement of strength and toughness. Summary of the invention

[0004] In order to solve the above technical problems, the present invention proposes a nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness and a preparation method thereof.

[0005] To achieve the above object, the present invention provides a method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness, comprising the following steps:

[0006] AlN ceramic particles (aluminum nitride ceramic particles) and Al powder are mixed, ball milled, compacted, and sintered to obtain AlN-Al master alloy;

[0007] The magnesium alloy billet is heated and melted, then cooled, and a preheated AlN-Al master alloy is added and stirred, and then the temperature is raised and allowed to stand, and the melt is cast into a mold and then cooled to obtain a cast AlN reinforced magnesium-based composite material;

[0008] The cast AlN reinforced magnesium-based composite material is subjected to a solid solution treatment to obtain a solid solution AlN reinforced magnesium-based composite material, and then subjected to a hot extrusion treatment to obtain the nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness.

[0009] The present invention firstly prepares an intermediate alloy containing nano-reinforced particles by powder metallurgy technology, and adds the intermediate alloy to a magnesium alloy melt to assist mechanical stirring, so as to form a cast magnesium-based composite material with uniformly dispersed reinforced particles; then, the structure is homogenized by solid solution treatment and the remelting of the precipitated phase is controlled; finally, hot extrusion is performed to close the defects of the cast structure, while considering the use of dynamic recrystallization mechanism to achieve grain refinement, and finally the strong and tough synergistic mechanical properties of the magnesium-based composite material are improved.

[0010] Furthermore, the nano-AlN particles account for 1 vol.% in the magnesium alloy billet.

[0011] Furthermore, the particle size of the AlN ceramic particles is ˜30 nm, and the particle size of the Al powder is ˜40 μm.

[0012] Furthermore, the mass ratio of the AlN ceramic particles to the Al powder is 1:2.

[0013] Furthermore, the AlN ceramic particles and Al powder need to be ultrasonically cleaned in alcohol and vacuum dried before mixed ball milling.

[0014] Furthermore, the ball-to-material ratio of the ball mill is 10:1, the rotation speed of the ball mill is 300 r / min, and the time is 180 min.

[0015] Furthermore, the balls used in the ball milling are ZrO2 ceramic balls.

[0016] Furthermore, the compaction is performed at room temperature with a pressure of 300 MPa maintained for 300 seconds.

[0017] Furthermore, the sintering is carried out under the protection of an inert atmosphere, the sintering temperature is 700° C., the sintering time is 120 min, and the sintering pressure is 0.8 MPa.

[0018] Furthermore, the sintering is performed under the protection of Ar gas atmosphere.

[0019] Furthermore, the cast magnesium alloy billet needs to be polished and cleaned with alcohol to remove oxide scale before melting.

[0020] Furthermore, the cast magnesium alloy billet is heated to 730° C. at a heating rate of 10° C. / min and kept at that temperature for 10 min, and then cooled to 720° C. During the heating and melting process, a mixed protective gas of CO2 and SF6 is continuously introduced into the resistance heating furnace to prevent the magnesium alloy from burning.

[0021] Furthermore, the temperature of the preheated AlN-Al master alloy is 100° C. The preheated AlN-Al master alloy is added and stirred at a speed of 320 r / min for 90 min to uniformly mix the AlN nanoparticles with the magnesium alloy melt.

[0022] Furthermore, the temperature rise rate of the solution treatment is 10°C / min, the temperature is 450°C, and the holding time is 480min.

[0023] Furthermore, the hot extrusion treatment process is to set the heating rate of the hot extrusion die and the blank to 10°C / min, the temperature to 350°C, and the holding time to 60min.

[0024] The present invention also proposes a nano-AlN particle reinforced magnesium-based composite material prepared by the preparation method and achieving synergistic improvement in strength and toughness.

[0025] Compared with the prior art, the present invention has the following advantages and technical effects:

[0026] 1) The present invention proposes a method for preparing a nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness. The method mainly includes three processes: preparation of an intermediate alloy containing nanoparticles, melt-casting of a magnesium-based composite material, and hot extrusion strengthening of the magnesium-based composite material, thereby achieving the preparation of a low-cost, high-performance magnesium-based composite material.

[0027] 2) The present invention uses powder metallurgy technology of ball milling, cold compaction and hot sintering to prepare the intermediate alloy, which helps to evenly disperse the nanoparticles in the magnesium alloy matrix melt, improves the serious clustering behavior of traditional nanoparticles, and helps to improve the performance of magnesium-based composite materials.

[0028] 3) The present invention helps to homogenize the structure and improve segregation in the cast magnesium-based composite material through solid solution treatment. The hot extrusion process can close the defects in the cast magnesium-based composite material and induce dynamic recrystallization behavior to refine the grains and achieve improved mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0030] Figure 1The microstructure diagram of the cast AlN / ZK60 magnesium-based composite material obtained in step (7) of Example 1;

[0031] Figure 2 The microstructure diagram of the AlN / ZK60 magnesium-based composite material obtained after extrusion in step (9) of Example 1;

[0032] Figure 3 The room temperature tensile test results of the AlN / ZK60 magnesium-based composite material obtained in Example 1 and the ZK60 magnesium-based material obtained in Comparative Example 1;

[0033] Figure 4 The room temperature tensile test results of the products obtained in Example 1 and Comparative Examples 1-7 are shown. DETAILED DESCRIPTION

[0034] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0035] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0036] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0037] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0038] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0039] The embodiment of the present invention provides a method for preparing a nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness, comprising the following steps:

[0040] AlN ceramic particles (aluminum nitride ceramic particles) and Al powder are mixed, ball milled, compacted, and sintered to obtain AlN-Al master alloy;

[0041] The magnesium alloy billet is heated and melted, then cooled, and a preheated AlN-Al master alloy is added and stirred, and then the temperature is raised and allowed to stand, and the melt is cast into a mold and then cooled to obtain a cast AlN reinforced magnesium-based composite material;

[0042] The cast AlN reinforced magnesium-based composite material is subjected to a solid solution treatment to obtain a solid solution AlN magnesium-based composite material, and then hot extrusion strengthening is performed to obtain the nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness.

[0043] In a preferred embodiment of the present invention, the nano-AlN particles account for 1 vol.% in the magnesium alloy billet.

[0044] In a preferred embodiment of the present invention, the particle size of the AlN ceramic particles is ˜30 nm, and the particle size of the Al powder is ˜40 μm.

[0045] In a preferred embodiment of the present invention, the mass ratio of the AlN ceramic particles to the Al powder is 1:2.

[0046] In a preferred embodiment of the present invention, the AlN ceramic particles and Al powder are ultrasonically cleaned in alcohol and vacuum dried before mixed ball milling.

[0047] In a preferred embodiment of the present invention, the ball-to-material ratio of the ball mill is 10:1, the rotation speed of the ball mill is 300 r / min, and the time is 180 min.

[0048] In a preferred embodiment of the present invention, the balls used in the ball milling are ZrO2 ceramic balls.

[0049] In a preferred embodiment of the present invention, the compaction is performed at room temperature with a pressure of 300 MPa maintained for 300 seconds.

[0050] In a preferred embodiment of the present invention, the sintering is carried out under the protection of an inert atmosphere, the sintering temperature is 700° C., the sintering time is 120 min, and the sintering pressure is 0.8 MPa.

[0051] In a preferred embodiment of the present invention, the sintering is performed under the protection of Ar gas atmosphere.

[0052] AlN-Al master alloy is prepared through ball milling, cold compaction and hot sintering. The prepared master alloy helps to evenly disperse the nanoparticles in the magnesium alloy matrix melt, improves the severe clustering behavior of traditional nanoparticles, and helps to improve the performance of magnesium-based composite materials.

[0053] Too low a sintering temperature and too short a sintering time are not enough to melt the Al powder to form an intermediate alloy, while too high a temperature and too long a sintering time can easily cause the intermediate alloy to overburn. The technical effect of cold compaction is to pre-combine the powder through high hydrostatic pressure, which is convenient for subsequent hot sintering process. Through the ball milling process, the nano-scale AlN reinforcement particles are welded to the micron-scale Al powder under the action of high-energy friction.

[0054] In a preferred embodiment of the present invention, the magnesium alloy blank is polished and cleaned with alcohol to remove oxide scale before melting.

[0055] In a preferred embodiment of the present invention, the magnesium alloy billet is heated to 730° C. at a heating rate of 10° C. / min and kept at that temperature for 10 minutes, and then cooled to 720° C. After heating and melting, a mixed protective gas of CO2 and SF6 is continuously introduced into the resistance heating furnace during the heating and melting process to prevent the magnesium alloy from burning.

[0056] In a preferred embodiment of the present invention, the temperature of the preheated AlN-Al master alloy is 100° C. The preheated AlN-Al master alloy is added and stirred at a speed of 320 r / min for 90 min to uniformly mix the AlN nanoparticles with the magnesium alloy melt.

[0057] In a preferred embodiment of the present invention, the temperature rise rate of the solution treatment is 10°C / min, the temperature is 450°C, and the holding time is 480min.

[0058] Solution treatment helps to homogenize the structure and improve segregation in cast magnesium-based composites. The heating rate is the maximum heating rate specified by the heat treatment furnace, which is generally 10°C / min. Too low solution temperature and too short time are not conducive to the remelting of certain precipitated phases, or cause incomplete remelting of precipitated phases, which is not conducive to strength and toughness. Too high solution temperature and too long time can easily lead to material melting (transformation into liquid phase) or severe oxidation (forming slag-like MgO), which is not conducive to the comprehensive performance of strength and toughness.

[0059] In a preferred embodiment of the present invention, the hot extrusion process is to increase the temperature of the hot extrusion die and the blank by 10°C / min, the temperature is 350°C, and the holding time is 60min.

[0060] The hot extrusion process can close the defects in the cast magnesium-based composite material and induce dynamic recrystallization behavior to refine the grains and improve the mechanical properties.

[0061] The heating rate refers to the heating rate of the hot extrusion die and the billet. Same as the solution treatment, the maximum heating rate specified by the heating furnace is 10℃ / min. Changing the extrusion temperature: lowering the extrusion temperature will increase the required extrusion force, and when the temperature is lower than the critical temperature of dynamic recrystallization, dynamic recrystallization will not be started to achieve fine grain strengthening. Although increasing the extrusion temperature is conducive to reducing the extrusion load, it will cause thermal cracks on the surface of the extruded material, which is not conducive to strength and toughness. Extrusion speed: (lowering the extrusion speed is conducive to improving the surface quality and mechanical properties of the extruded material, but too low an extrusion speed is generally difficult to achieve with a press, and too low an extrusion speed is not conducive to improving production efficiency. In fact, our work extrusion speed of 1mm / s is already very low.) Increasing the extrusion speed may increase the friction between the billet surface and the die, causing surface damage and defects. At the same time, too high an extrusion speed will cause a large temperature rise on the billet surface. When the temperature difference between the core and the surface is large, thermal cracks are likely to occur, resulting in performance deterioration.

[0062] The embodiment of the present invention also provides a nano-AlN particle reinforced magnesium-based composite material prepared by the preparation method and achieving synergistic improvement in strength and toughness.

[0063] In the embodiments of the present invention, the AlN ceramic particles and Al powder used are purchased from Beijing Dekedaojin Technology Co., Ltd., and the magnesium alloy billet used is a cast ZK60 magnesium alloy billet purchased from Shanxi Yinguang Huasheng Magnesium Co., Ltd.

[0064] The room temperature in the embodiments of the present invention refers to "25±3°C".

[0065] The symbol “~” in the embodiments of the present invention represents approximately, with a fluctuation of no more than 5%.

[0066] The technical solution of the present invention is further illustrated by the following embodiments.

[0067] Example 1

[0068] (1) 30 nm AlN ceramic particles and 40 μm Al powder were ultrasonically cleaned in alcohol and dried in vacuum, and the AlN ceramic particles and Al powder were mixed and ball-milled in a planetary ball mill at a mass ratio of 1:2. The ball milling speed was 300 r / min, the time was 180 min, the ball-to-material ratio was 10:1, and the ball used was a ZrO2 ceramic ball. After the ball milling, AlN-Al mixed powder was obtained;

[0069] (2) placing the obtained AlN-Al mixed powder in a special mold and placing it on a press at room temperature and maintaining a pressure of 300 MPa for 300 s to ensure compaction;

[0070] (3) placing the AlN-Al mixed powder compacted at room temperature in a tubular heating furnace, filling it with Ar gas until the quartz tube reaches 0.8 MPa to achieve Ar atmosphere protection, and sintering at 700° C. for 120 min to form an AlN-Al master alloy;

[0071] (4) Cutting the as-cast ZK60 magnesium alloy billet to fit the size of the melting crucible, and polishing and alcohol cleaning to remove the oxide scale;

[0072] (5) Spraying a boron nitride isolating agent on the melting crucible in the resistance heating furnace to inhibit element diffusion, and placing the ZK60 magnesium alloy billet processed in the previous step in the crucible, heating it to 730°C at a heating rate of 10°C / min, and keeping it warm for 10 minutes to ensure melting to obtain a ZK60 magnesium alloy melt. During this process, a mixed protective gas of CO2 and SF6 is continuously introduced into the resistance heating furnace to prevent the magnesium alloy from burning;

[0073] At the same time, the AlN-Al master alloy is placed in a box-type heating furnace and preheated to 100°C and kept warm continuously, and the steel mold used for casting is sprayed with a boron nitride isolation agent and placed in a box-type heating furnace and preheated to 200°C and kept warm continuously;

[0074] (6) cooling the ZK60 magnesium alloy melt to 720° C., adding the preheated AlN-Al master alloy (the amount of the AlN-Al master alloy added should satisfy the requirement that the proportion of the nano-AlN particles in the ZK60 magnesium alloy billet is 1 vol.%), and simultaneously starting a mechanical stirring device, using a propeller made of a high-temperature alloy to stir at a speed of 320 r / min for 90 min so that the AlN-Al master alloy and the ZK60 magnesium alloy melt are uniformly mixed to obtain a mixed melt;

[0075] (7) After the mechanical stirring is completed, the obtained mixed melt is heated to 750° C. and allowed to stand for 10 min, after which impurities on the surface of the melt are removed and the melt is cast into a preheated steel mold, and then naturally cooled to obtain a cast AlN / ZK60 reinforced magnesium-based composite material;

[0076] (8) The cooled cast AlN / ZK60 reinforced magnesium-based composite material was placed in a can made of a high-temperature alloy and filled with MgO sand (commercially purchased, 92 purity 200 mesh dead-burned magnesia sand), and placed in a box-type heating furnace, heated to 450°C at a heating rate of 10°C / min, maintained for 480min for solution treatment, and then water-cooled to preserve the structure;

[0077] (9) The solution-treated AlN / ZK60 magnesium-based composite material and an H13 steel mold with an extrusion ratio of 4:1 were placed in a box furnace, heated to 350°C at a heating rate of 10°C / min and kept warm for 60 min. After spraying MoS2 lubricant into the H13 steel mold cavity, the solution-treated AlN / ZK60 magnesium-based composite material was extruded through a press at an extrusion rate of 1 mm / s, and the extruded rod was quickly water-cooled to preserve the structure, thereby obtaining a nano-AlN particle reinforced magnesium-based composite material (AlN / ZK60 magnesium-based composite material).

[0078] The microstructure of the cast AlN / ZK60 reinforced magnesium-based composite material obtained in step (7) of Example 1 of the present invention is shown in Figure 1 The microstructure pointed by the white arrow in the figure is AlN particles.

[0079] The microstructure of the AlN / ZK60 magnesium-based composite material obtained after extrusion in step (9) of Example 1 of the present invention is shown in FIG. Figure 2 The microstructure pointed by the white arrow in the figure is AlN particles.

[0080] Combination Figure 1 and Figure 2 It can be seen that after hot extrusion, the microstructure presents a typical bimodal structure caused by incomplete dynamic recrystallization. The coarse deformed grains are parallel to the extrusion direction, and are surrounded by fine dynamic recrystallized grains.

[0081] Comparative Example 1

[0082] (1) The as-cast ZK60 magnesium alloy billet was cut to fit the size of the melting crucible, and polished and cleaned with alcohol to remove the oxide scale;

[0083] (2) Spraying a boron nitride isolating agent on the melting crucible in the resistance heating furnace to inhibit element diffusion, and placing the ZK60 magnesium alloy billet processed in the previous step in the crucible, heating it to 730°C at a heating rate of 10°C / min, and keeping it warm for 10 minutes to ensure that the ZK60 magnesium alloy melt is melted. During this process, a mixed protective gas of CO2 and SF6 is continuously introduced into the resistance heating furnace to prevent the magnesium alloy from burning;

[0084] At the same time, the steel mold used for casting is sprayed with boron nitride isolation agent and placed in a box-type heating furnace to be preheated to 200°C and kept warm continuously;

[0085] (3) heating the obtained ZK60 magnesium alloy melt to 750° C. and standing for 10 min, then removing impurities from the surface of the melt, casting it into a preheated steel mold, and then naturally cooling it to obtain a cast ZK60 magnesium-based material;

[0086] (4) The cooled cast ZK60 magnesium alloy was placed in a can made of a high-temperature alloy and filled with MgO sand (commercially available, 92% purity 200-mesh dead-burned magnesia), and placed in a box-type heating furnace, heated to 450°C at a heating rate of 10°C / min, maintained for 480min for solution treatment, and then water-cooled to preserve the structure;

[0087] (5) The solution-treated ZK60 magnesium alloy and an H13 steel mold with an extrusion ratio of 4:1 were placed in a box furnace, heated to 350°C at a heating rate of 10°C / min and kept warm for 60 min. After spraying MoS2 lubricant into the cavity of the H13 steel mold, the solution-treated ZK60 magnesium alloy was extruded through a press at an extrusion rate of 1 mm / s, and the extruded rod was quickly water-cooled to preserve the structure, thereby obtaining an extruded magnesium alloy (ZK60 magnesium alloy).

[0088] The AlN / ZK60 magnesium-based composite material obtained in Example 1 and the ZK60 magnesium alloy obtained in Comparative Example 1 were subjected to room temperature tensile tests according to the national standard GB / T228.1-2021B method. The test results are shown in Figure 3 It can be seen that the tensile strength and elongation after fracture of AlN / ZK60 magnesium-based composite materials are improved compared with ZK60 magnesium alloy, achieving a synergistic improvement in strength and toughness.

[0089] Comparative Example 2

[0090] The same as Example 1, except that the AlN-Al master alloy is replaced with AlN ceramic particles of equal volume fraction, and the AlN ceramic particles are directly added to the ZK60 magnesium alloy melt. The specific steps are as follows:

[0091] (1) The as-cast ZK60 magnesium alloy billet was cut to fit the size of the melting crucible, and polished and cleaned with alcohol to remove the oxide scale;

[0092] (2) Spraying a boron nitride isolating agent on the melting crucible in the resistance heating furnace to inhibit element diffusion, and placing the ZK60 magnesium alloy billet processed in the previous step in the crucible, heating it to 730°C at a heating rate of 10°C / min, and keeping it warm for 10 minutes to ensure that the ZK60 magnesium alloy melt is melted. During this process, a mixed protective gas of CO2 and SF6 is continuously introduced into the resistance heating furnace to prevent the magnesium alloy from burning;

[0093] At the same time, the AlN ceramic particles are placed in a box-type heating furnace and preheated to 100°C and kept warm continuously, and the steel mold used for casting is sprayed with a boron nitride isolation agent and placed in a box-type heating furnace and preheated to 200°C and kept warm continuously;

[0094] (3) cooling the ZK60 magnesium alloy melt to 720° C., adding preheated AlN ceramic particles (the amount of AlN ceramic particles added should satisfy the requirement that the proportion of nano AlN particles in the ZK60 magnesium alloy billet is 1 vol.%), and simultaneously starting a mechanical stirring device, using a propeller made of a high-temperature alloy to stir at a speed of 320 r / min for 90 min to uniformly mix the AlN-Al master alloy and the ZK60 magnesium alloy melt to obtain a mixed melt;

[0095] (7) After the mechanical stirring is completed, the obtained mixed melt is heated to 750° C. and allowed to stand for 10 min, after which impurities on the surface of the melt are removed and the melt is cast into a preheated steel mold, and then naturally cooled to obtain a cast AlN / ZK60 reinforced magnesium-based composite material;

[0096] (8) The cooled cast AlN / ZK60 reinforced magnesium-based composite material was placed in a can made of a high-temperature alloy and filled with MgO sand (commercially purchased, 92 purity 200 mesh dead-burned magnesia sand), and placed in a box-type heating furnace, heated to 450°C at a heating rate of 10°C / min, maintained for 480min for solution treatment, and then water-cooled to preserve the structure;

[0097] (9) The solution-treated AlN / ZK60 magnesium-based composite material and an H13 steel mold with an extrusion ratio of 4:1 were placed in a box furnace, heated to 350°C at a heating rate of 10°C / min and kept warm for 60 min. After MoS2 lubricant was sprayed into the H13 steel mold cavity, the solution-treated AlN / ZK60 magnesium-based composite material was extruded through a press at an extrusion rate of 1 mm / s, and the extruded rod was quickly water-cooled to preserve the structure, thereby obtaining an AlN ceramic particle reinforced magnesium-based composite material.

[0098] Comparative Example 3

[0099] The same as Example 1, except that in step (1), the AlN ceramic particles and Al powder are mixed and ball-milled on a planetary ball mill at a rotation speed of 150 r / min.

[0100] Comparative Example 4

[0101] The same as Example 1, except that in step (6), the ZK60 magnesium alloy melt is cooled to 630° C. and then the preheated AlN—Al master alloy is added.

[0102] Comparative Example 5

[0103] The same as Example 1, except that in step (6), the preheated AlN-Al master alloy is added and the mechanical stirring device is started at the same time, and a propeller made of a high-temperature alloy is used to stir at a speed of 320 r / min for 30 minutes.

[0104] Comparative Example 6

[0105] The same as Example 1, except that in step (8), the temperature is heated to 300° C. at a heating rate of 10° C. / min and maintained for 480 min for solution treatment.

[0106] Comparative Example 7

[0107] The same as Example 1, except that the hot extrusion process temperature in step (9) is set to 400°C, that is, the temperature is heated to 400°C at a heating rate of 10°C / min and kept at this temperature for 60 minutes.

[0108] The products obtained in Example 1 and Comparative Examples 1-7 were subjected to room temperature tensile test according to the national standard GB / T228.1-2021B method. The test results are shown in Figure 4 ,Depend on Figure 4 It can be seen that the performance of Comparative Examples 1-7 is reduced compared with Example 1, because:

[0109] In Comparative Example 1, since AlN ceramic particles are not added to the ZK60 magnesium alloy, the degree of dynamic recrystallization during hot extrusion is low, resulting in a weakened grain refinement effect. Therefore, the strength-toughness synergy is poorer than that of Example 1;

[0110] In Comparative Example 2, when AlN particles are directly added to the ZK60 magnesium alloy melt, the heat flow caused by the large temperature difference between the inside and outside of the melt causes the AlN particles to escape outward, so the particles actually added to the melt are less than the theoretical volume fraction. Furthermore, due to the lack of a layer-by-layer dispersion process of the melting of the intermediate alloy, the AlN particles added to the melt are severely clustered in the melt due to strong van der Waals forces, resulting in deterioration of mechanical properties;

[0111] In Comparative Example 3, during the preparation of the AlN-Al master alloy, the ball milling speed was reduced by half compared with Example 1, resulting in uneven mixing of the AlN nanoparticles and the Al powder. The uneven powder was further prepared into a master alloy and added to the ZK60 magnesium alloy, resulting in uneven distribution of AlN particles inside the AlN / ZK60 composite material, which in turn caused uncoordinated deformation during the stretching process, resulting in poorer synergistic performance of strength and toughness than Example 1;

[0112] In Comparative Example 4, since the ZK60 magnesium alloy melt temperature is a semi-solid state of 630° C. when the AlN-Al master alloy is added, the melt fluidity of the AlN-Al master alloy decreases during the stirring process after the AlN-Al master alloy is melted, which is not conducive to the uniform dispersion of AlN particles and causes local clusters. The result is similar to that of Comparative Example 3, resulting in poorer strength-toughness synergy than that of Example 1;

[0113] In Comparative Example 5, the time for mechanically stirring the AlN / ZK60 composite melt was reduced by 60 min compared with Example 1. Too short a stirring time resulted in insufficient melting of the AlN-Al master alloy and uneven dispersion of the AlN particles after melting. The above reasons together caused the AlN / ZK60 composite to deform uncoordinatedly during the tensile test, resulting in poorer synergistic performance of strength and toughness than that of Example 1.

[0114] In Comparative Example 6, the temperature of the solution treatment of the cast AlN / ZK60 composite material is reduced by 50°C compared with Example 1. The solution treatment temperature of 300°C is lower than the precipitation temperature of MgZn, Mg7Zn3 and Mg5Zn2Al2 phases in the AlN / ZK60 composite material, and it is difficult to effectively control the melting back of the precipitated phases. In the subsequent hot extrusion, the presence of large-sized precipitated phases will lead to damage such as thermal cracks, which makes the strength-toughness synergy performance worse than that of Example 1;

[0115] In Comparative Example 7, the temperature of the hot extruded AlN / ZK60 composite material is 50°C higher than that of Example 1, which exceeds the temperature range for safe processing of the AlN / ZK60 composite material. High-temperature extrusion leads to a large difference in flow velocity between the surface and the core of the billet, which is manifested as thermal cracks on the surface of the extruded rod, making the strength-toughness synergy worse than that of Example 1.

[0116] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness, characterized in that: The following steps are involved: AlN ceramic particles and Al powder are mixed, ball milled, compacted and sintered to obtain AlN-Al master alloy; The magnesium alloy blank is heated and melted, then cooled, and a preheated AlN-Al master alloy is added and stirred, and then the temperature is raised and allowed to stand, and after casting, the cast AlN reinforced magnesium-based composite material is obtained by cooling. The cast AlN reinforced magnesium-based composite material is subjected to a solid solution treatment to obtain a solid solution AlN magnesium-based composite material, and then subjected to a hot extrusion treatment to obtain the nano-AlN particle reinforced magnesium-based composite material that achieves synergistic improvement in strength and toughness.

2. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The nano-AlN particles account for 1 vol.% in the magnesium alloy billet.

3. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The particle size of the AlN ceramic particles is ∼30 nm, and the particle size of the Al powder is ∼40 μm.

4. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The ball-to-material ratio of the ball mill is 10:1, the rotation speed of the ball mill is 300 r / min, and the time is 180 min.

5. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The sintering is carried out under the protection of an inert atmosphere, the sintering temperature is 700° C., the sintering time is 120 min, and the sintering pressure is 0.8 MPa.

6. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The magnesium alloy billet is heated to 730°C at a heating rate of 10°C / min and kept at that temperature for 10 minutes. After heating and melting, the temperature is lowered to 720°C.

7. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The temperature of the preheated AlN-Al master alloy is 100° C. The preheated AlN-Al master alloy is added and stirred at a speed of 320 r / min for 90 minutes.

8. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The temperature rise rate of the solution treatment is 10°C / min, the temperature is 450°C, and the holding time is 480min.

9. The method for preparing a nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness according to claim 1, characterized in that: The heating rate of the hot extrusion treatment is 10°C / min, the temperature is 350°C, and the holding time is 60min.

10. A nano-AlN particle reinforced magnesium-based composite material with synergistically improved strength and toughness, prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of fine-grain Mg-based composite material comprising AlN (aluminum nitride) particles

    CN104928510A

  • Magnesium-based composite material with improved heat resistance and preparation method thereof

    CN114277297A

  • Mixed reinforced phase magnesium-based composite material and preparation method thereof

    CN115058707A

  • AlN / AE44 composite material with excellent high-temperature mechanical property and preparation method thereof

    CN115976384A

  • Method for improving agglomeration of micron-sized AlN particles in magnesium-rare earth-based composite material

    CN117230341A

Cited By

  • High-fatigue-resistance low-content nanoparticle reinforced magnesium alloy and preparation method

    CN120041730A

  • Modular semi-solid forming method and system for particle-reinforced magnesium-based composite material

    CN121373351A

  • Modular semi-solid forming method and system for particulate reinforced magnesium matrix composites

    CN121373351B