Large-piece-weight disc round wire for TC4 fastener with coating on surface and production method of large-piece-weight disc round wire
By controlling the chemical composition of the ingot and adopting three-roller connecting, hot rolling, polishing and other processes, the problem of inconsistent performance and dimensional tolerances of large single-dish round wire materials for domestically produced TC4 surface coated fasteners is solved, and the performance and dimensional tolerances of large double-dish round wire materials for domestically produced TC4 surface coated fasteners is achieved. The stability of material performance and the improvement of production efficiency meet the continuous and batch production needs of aerospace fasteners.
Patent Information
- Application Number
- CN202411013278.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The large single-dish round wire material for domestically produced TC4 surface coated fasteners has differences in tensile strength, elongation, cross-section shrinkage and other indicators. The roundness and line diameter tolerance are inconsistent, and the quality of the surface lubricating coating is poor. Meet the continuous and batch production needs of aerospace fasteners.
By controlling the chemical composition of the ingot, using three smelting, two hot rolling, three rolling, hot pulling, polishing and high-precision spraying, the grain size is less than 3 μm, the single weight reaches 150kg, and the surface coating thickness is prepared. Large single-dish round wire material for TC4 surface coated fasteners of 0.07~0.015μm.
It achieves the stability of material performance, consistency of dimensional tolerances, uniformity of surface coatings and production efficiency, meets the requirements of continuous upsetting and mass production of fasteners, and improves the consistency of product quality.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of titanium alloy processing, and in particular to a large single-weight round wire for TC4 surface-coated fasteners and a production method thereof. Background Art
[0002] At present, the domestically produced TC4 surface coated fasteners with large single weight coiled wire have the following defects: (1) The wire performance is unstable. There are some gaps between the domestically produced high-strength fastener TC4 wire and imported products in terms of tensile strength, elongation, cross-sectional shrinkage and other indicators. Especially in terms of the consistency of performance indicators, the strength indicators of domestic materials fluctuate greatly between different batches, and the dispersion is even greater. Although the material performance meets the standard requirements, the index values vary greatly, which brings certain inconveniences to the fastener processing and ultimately affects the quality consistency of fastener products. (2) The roundness and wire diameter tolerance consistency of coiled wire are poor. The roundness and wire diameter tolerance of domestically produced titanium alloy coiled wire cannot fully meet the standard requirements, affecting the consistency of fastener dimensions and the continuous upsetting production of fasteners, and cannot meet the needs of mass production of fasteners. (3) The quality of the lubricating coating on the wire surface is not high. The lubricating coating effect of the domestically produced coiled wire surface is poor. During the upsetting process of the fastener, it is easy to damage the fastener rod and the mold, reducing the production efficiency of the fastener and even causing the mold to be scrapped.
[0003] Due to the above defects, the currently domestically produced TC4 surface coated fasteners with large single weight round wire cannot fully meet the requirements of continuous upsetting production of aerospace fastener manufacturers, nor can it meet the needs of mass production of aerospace fasteners. Summary of the invention
[0004] In view of this, the present invention provides a heavy single-weight coiled wire for TC4 surface-coated fasteners, wherein the ingot chemical composition of the coiled wire includes Al: 5.9%-6.3%; V: 3.9%-4.3%; Fe: 0.10%-0.20%; C: ≤0.05%; N: ≤0.03%; O: 0.13%-0.17%; H: ≤0.008%; and the balance is titanium.
[0005] Furthermore, the grain size of the coiled wire is not greater than 3 μm, the unit weight of the finished coiled wire can reach 150 kg, the tolerance is controlled within the range of 0 to -0.03 μm, and the surface coating thickness is 0.07 to 0.015 μm.
[0006] The present invention also provides a method for producing the large single-weight round wire for the TC4 surface-coated fastener, comprising the following steps: (1) Raw material selection and ingredients; (2) Ingot smelting: the raw materials prepared in step (1) are mixed and pressed into electrode blocks, and then the electrode blocks are smelted three times in a vacuum consumable arc furnace to obtain an ingot; (3) Billet forging: heating the ingot to 1150° C. in the β phase region, performing a single-shot forging, and deforming the ingot to obtain a square billet; (4) First hot rolling: After sawing and repairing the surface defects of the square billet, it is heated to 930-960℃ and hot rolled in a horizontal rolling mill to obtain a billet; (5) Skin peeling and wound repair; (6) Second hot rolling: The stripped and repaired billet is hot rolled at 900-940°C, and then hot rolled into coils by three-roll rolling. The maximum rolling weight can reach 220kg, and the total deformation is 99%; (7) Hot drawing: The coil is subjected to roller die hot drawing, the heating temperature is 750~850℃, and the single-pass deformation rate is controlled at 17%-25% to obtain coiled wire; (8) Annealing; (9) Polishing: Polish the annealed wire, and control the surface roughness Ra to 1.0 μm~1.6 μm; (10) Surface coating: The polished coiled wire is sprayed to obtain a large single weight coiled wire for TC4 surface coated fasteners.
[0007] Furthermore, the raw materials in step (1) include titanium sponge, aluminum vanadium alloy, aluminum beans and ferrotitanium.
[0008] Furthermore, the titanium sponge is selected from grade 0 or above titanium sponge that complies with the GB / T 2524-2019 standard.
[0009] Furthermore, the pressing density of the electrode block in step (2) is ≥3.7 g / cm 3 .
[0010] Furthermore, the peeling and repairing in step (5) includes surface polishing and pickling.
[0011] Furthermore, the annealing temperature in step (8) is 700-800° C., and the annealing time is 60-120 min.
[0012] Furthermore, the polishing in step (9) uses a high-precision peeling unit + polishing integrated equipment to improve product surface quality and production efficiency.
[0013] Furthermore, the composition of the spraying material in step (10) mainly includes 30-40% of modified potassium silicate resin, 20-35% of deionized water, 5-10% of graphite, and 20-25% of molybdenum disulfide, and an advanced spraying production line is used, and the spraying and drying are carried out through a spraying drying process.
[0014] Compared with the prior art, the present invention has the following beneficial effects: the present invention controls the chemical composition of the material, and adopts three-roll continuous rolling process, high-precision lathe polishing, surface coating and other processes to produce large single-weight round wire for TC4 surface coated fasteners, which can meet the requirements of continuous upsetting fasteners, and has the characteristics of stable material performance, good dimensional tolerance consistency, uniform surface lubrication coating, high production efficiency, good surface quality and the like. The advantage of the three-roll continuous rolling process adopted by the present invention over the traditional horizontal or vertical two-roll rolling is that the three-roll rolling has a smaller width, three-directional rolling force, uniform force on the rolled piece, good consistency of organization and performance, and can obtain better dimensional accuracy and surface quality. The three-roll hole type is conducive to the extension flow of metal rolling, and there will be no fish scale pattern on the surface of the rod and wire. The two hot rolling processes, the first hot rolling deformation is 65% to prepare the blank, and the second hot rolling deformation is 99%, which can fully crush and refine the grains to achieve consistency of organization and performance. DETAILED DESCRIPTION
[0015] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0016] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the raw materials and auxiliary agents are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified. Example
[0017] A method for producing a large single-weight round wire for TC4 surface-coated fasteners, the specific steps are as follows: (1) Raw material selection and batching: Use "grade 0" titanium sponge as raw material, ALV55%, aluminum bean and titanium iron as added alloying elements, and batch according to the alloy composition requirements in Table 1; (2) Ingot smelting: The raw materials prepared in step (1) are mixed and pressed into electrode blocks using a 4000-ton hydraulic press. The pressed density of the electrode blocks is greater than 3.7 g / cm 3 , a vacuum welding box welding process is adopted to protect the welding point from atmospheric oxidation and reduce the introduction of gas impurities, and then a vacuum consumable arc furnace is used for three smelting to obtain a Φ630×L ingot. The chemical composition analysis of the ingot is shown in Table 1. The ingot composition meets the GB / T3620.1-2016 standard and has a uniform composition; (3) Billet forging: After ultrasonic testing, the ingot is sawn to forge the bottom and mouth of the cap; the ingot is heated to 1150°C in the β phase region in an electric furnace, and is forged once in a 1600-ton press to deform the ingot with an outer diameter of 630 mm into a square billet with a side length of 150 mm; (4) First hot rolling: After sawing and repairing the surface defects of the square billet, it is heated to 940°C in a resistance furnace and hot rolled into a Φ100×L mm billet in a horizontal rolling mill; (5) Peeling and repairing: surface polishing, pickling and repairing to ensure that surface defects are repaired cleanly and thoroughly; (6) Second hot rolling: the bar billet after peeling and repairing is heated to 930℃ in a resistance furnace for hot rolling: the Φ100×L mm bar billet is hot rolled to Φ10.0 mm coil using a three-roller continuous binding line, with a total deformation of 99%; (7) Hot drawing: The coil is subjected to multi-die roller hot drawing, and the Φ10.0 mm coil is drawn to Φ6.9 mm. The coil is heated in a resistance furnace at 750-850°C, and the deformation rate of a single pass is controlled at 17%-25% to obtain a coiled wire; (8) Annealing: Annealing is carried out at an atmospheric furnace temperature of 750°C for 120 minutes to obtain stable structure and properties; (9) Polishing: The annealed Φ6.9 mm wire is polished to Φ6.35 (-0.02, -0.04) mm, and the surface roughness Ra is controlled at 1.0 μm~1.6 μm, which is conducive to the subsequent coating spraying; (10) Surface coating: The surface of the polished coiled wire is sprayed with a lubricant with MoS2 as the main component. The thickness of the surface coating is controlled at 0.07~0.015μm to ensure the finished product tolerance Φ6.35(0,-0.03)mm, and a large single weight coiled wire for TC4 surface coated fasteners is obtained.
[0018] The results of mechanical property test and grain size test on the finished product are shown in Table 2. The test results show that after heat treatment, the material meets the requirements of GJB2219A-2015 standard, and the surface coating can meet the requirements of continuous upsetting.
[0019] Table 1 Chemical composition of ingot
[0020] Table 2 Mechanical properties of TC4 Φ6.35mm finished products
[0021] Comparative Example 1 The difference from Example 1 is that the square billet with a side length of 150 mm is rolled to Φ55 mm using an ordinary horizontal rolling mill for hot rolling, and Φ54 mm is polished and ground before being rolled into Φ10 mm coils using an ordinary horizontal rolling mill with a maximum single weight of 30 kg. The skinning is done using an ordinary skinning machine + polishing, and other conditions remain unchanged.
[0022] The mechanical properties of the finished rod of Example 1 were tested, and the results are shown in Table 3.
[0023] Table 3 Mechanical properties of TC4 Φ6.35mm finished bars
[0024] As shown in Table 3, the mechanical properties of the finished wire coils and batches of coils produced by the traditional horizontal rolling process have large deviations, as well as large deviations in grain size. The traditional stripping + polishing equipment has poor dimensional control stability, and the head, middle, and tail dimensional deviations are large.
[0025] By comparison, it is found that the three-roll continuous rolling method used in the present invention can fully crush the grains, and the grain refinement is very obvious. The unit weight of the finished product is 150kg, and the unit weight of the rolled billet can reach 220kg, which can effectively solve the problem of performance consistency between batches.
[0026] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A large single-weight round wire for TC4 surface coated fasteners, characterized in that: The ingot chemical composition of the coiled wire includes Al: 5.9%-6.3%; V: 3.9%-4.3%; Fe: 0.10%-0.20%; C: ≤0.05%; N: ≤0.03%; O:0.13%~0.17%; H: ≤0.008%; the balance is titanium.
2. According to claim 1, the large single-weight round wire for TC4 surface-coated fasteners is characterized in that: The grain size of the coiled wire is not greater than 3 μm, the tolerance is controlled within the range of 0 to -0.03 μm, and the surface coating thickness is 0.07 to 0.015 μm.
3. A method for producing a large single-weight round wire for TC4 surface-coated fasteners according to any one of claims 1 or 2, characterized in that: The following steps are involved: (1) Raw material selection and ingredients; (2) Ingot smelting: the raw materials prepared in step (1) are mixed and pressed into electrode blocks, and the electrode blocks are smelted three times in a vacuum consumable arc furnace to obtain an ingot; (3) Billet forging: heating the ingot to 1150° C. in the β phase region, performing a single-fire forging, and deforming the ingot to obtain a square billet; (4) First hot rolling: After the billet is sawn and surface defects are repaired, it is heated to 930-960°C and hot rolled in a horizontal rolling mill to obtain a billet; (5) Skin peeling and wound repair; (6) Second hot rolling: The stripped and repaired billet is hot rolled at 900-940°C, and then hot rolled into coils by three-roll rolling, with a total deformation of 99%; (7) Hot drawing: The coil is subjected to roller die hot drawing at a heating temperature of 750-850°C and a single-pass deformation rate controlled at 17%-25% to obtain a coiled wire; (8) Annealing; (9) Polishing: Polish the annealed wire coil, and control the surface roughness Ra to 1.0 μm to 1.6 μm; (10) Surface coating: The polished coiled wire is sprayed to obtain a large single weight coiled wire material for TC4 surface coated fasteners.
4. The method for producing a large single-weight round wire for TC4 surface-coated fasteners according to claim 3, characterized in that: The raw materials in step (1) include sponge titanium, aluminum vanadium alloy, aluminum beans and ferrotitanium.
5. The method for producing a large single-weight round wire for TC4 surface-coated fasteners according to claim 4, characterized in that: The titanium sponge is selected from grade 0 or above.
6. The method for producing the large single-weight round wire for TC4 surface-coated fasteners according to claim 3, characterized in that: The pressing density of the electrode block in step (2) is ≥3.7 g / cm 3 .
7. The method for producing a large single-weight round wire for TC4 surface-coated fasteners according to claim 3, characterized in that: The peeling and repairing in step (5) includes surface polishing and pickling.
8. The method for producing a large single-weight round wire for TC4 surface-coated fasteners according to claim 3, characterized in that: The annealing temperature in step (8) is 700-800° C. and the annealing time is 60-120 min.
9. The method for producing a large single-weight round wire for TC4 surface-coated fasteners according to claim 3, characterized in that: The components of the spraying material in step (10) mainly include 30-40% of modified potassium silicate resin, 20-35% of deionized water, 5-10% of graphite, and 20-25% of molybdenum disulfide.
Citation Information
Cited By
Preparation method and application of titanium alloy disc round wire resistant to high temperature of 650 DEG C
CN119702682A
Preparation method and application of a titanium alloy coil wire resistant to 650 °C high temperature
CN119702682B
Preparation method of high-precision and high-performance titanium alloy welding wire and welding wire
CN120095411A