Preparation method of rare earth heat-resistant alloy steel 15CrMo hot rolled steel strip with thickness of 3.0-20.0 mm

By adding Mn, Cr, Mo, Ce elements and control processes to 15CrMo, a rare earth heat-resistant alloy steel hot-rolled steel strip was prepared, which solved the problem of undetailed production process of medium and thick plates and uneven tissue performance, and achieved high strength , Preparation of rare earth heat-resistant alloy steel with good oxidation resistance and welding properties.

CN118957402AActive Publication Date: 2024-11-15BEIJING BAOGANG STEEL TECHNOLOGY CO LTD

Patent Information

Application Number
CN202410872910.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-15
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

The prior art has failed to effectively solve the detailed production process problems of 3-20mm thickness 15CrMo medium-thickness plate heat-resistant alloy steel on the 2250mm production line and the unevenness of product tissue performance, and no rare earth elements were added to improve performance.

Method used

Using reasonable Mn, Cr, Mo and Ce element ratios, control gas element content and control rolling and cooling technology, combined with insulation and cooling measures, wet molten pretreatment, converter composite blowing, LF refining, RH vacuum treatment, and continuous Casting, slab heating, hot rolling and laminar flow cooling processes were prepared to produce a 3.0-20.0mm thickness rare earth heat-resistant alloy steel hot-rolled steel strip with uniform structure and stable performance.

Benefits of technology

The product has achieved good strength, welding and oxidation resistance, and its mechanical properties meet the tensile strength ≥450MPa, yield strength ≥295MPa, and elongation ≥19%. It is suitable for steel for high-temperature pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957402A_ABST
    Figure CN118957402A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a rare earth heat-resistant alloy steel 15CrMo hot rolled steel strip with the thickness of 3.0-20.0 mm. The preparation method comprises the following steps of molten iron pretreatment, converter combined blowing, LF refining, RH, continuous casting, slab heating, hot continuous rolling, laminar cooling and coiling and heat preservation and slow cooling. The heat-resistant alloy steel comprises the following chemical components in percentage by weight: 0.12%-0.18% of C, 0.15%-0.40% of Si, 0.40%-0.70% of Mn, less than or equal to 0.030% of P, less than or equal to 0.030% of S, 0.80%-1.10% of Cr, 0.40%-0.55% of Mo and less than or equal to 0.0030% of Ce. According to the invention, reasonable Mn, Cr, Mo and Ce are added, the content of gas elements is controlled, a reasonable controlled rolling and controlled cooling process is matched, and a heat preservation and slow cooling measure is adopted after rolling, so that a product is uniform and fine in structure, stable in performance and good in plate shape.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention is mainly used in industrial fields such as boiler heat-resistant structural parts, high-temperature pipelines, high-temperature flanges and ship desulfurization towers, and in particular relates to a preparation method of a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip. Background Art

[0002] With the fierce competition in the steel market and the rapid development of the domestic and foreign steel industry, customers' demand for 15CrMo coils is increasing. Combined with the application requirements of products in petroleum, aerospace, and energy, the toughness, oxidation resistance, and weldability of products are required. Products that serve in atmospheric corrosion environments, such as in power and chemical enterprise construction projects, 15CrMo steel is a pearlite heat-resistant steel. It has significant thermal strength and oxidation resistance in high temperature environments, and exhibits a certain resistance to hydrogen corrosion. These outstanding properties are mainly attributed to the higher content of Cr, C, and other alloying elements in the steel.

[0003] In order to meet production and market needs, we have developed 15CrMo hot-rolled coils that meet market requirements. Using 2250mm advanced rolling equipment and rolling technology that meets special product requirements, the product has good performance indicators and has been well received by customers.

[0004] Deng Jianjun et al. (Deng Jianjun et al., A rolling method for low-alloy 15CrMo steel plates, patent accepted, December 21, 2018) studied a rolling method for low-alloy 15CrMo steel plates, the rolling method comprising two-stage controlled rolling of continuous casting billets and controlled cooling after rolling. The thickness of the produced steel plates is 20-50 mm, and the performance meets the following requirements: yield strength ≥300 MPa, tensile strength Rm: 470-590 MPa; elongation ≥20%, and the transverse impact energy at 0°C is greater than 80 J. The products produced meet customer requirements. The shortcomings are that the products are designed as medium and thick plates, and the CVC technology is not used to adjust the straightness of the steel strip, and the composition of the steel strip and the rolling production situation are not introduced.

[0005] Yang Hua et al. (Yang Hua et al., A heat-treatment-free 15CrMo heat-resistant alloy steel hot-rolled coil and its CSP process production method, patent accepted, February 27, 2024) introduced a heat-treatment-free 15CrMo heat-resistant alloy steel hot-rolled coil and its CSP process production method. The disadvantage is that the thickness of the continuous casting slab is 60-70mm, compared with the 230mm slab of this patent, the compression ratio during rolling is small, the metallographic structure size and grain size are larger and more uneven than those of the 2250mm rolling mill steel strip, and the cost is relatively high, and no rare earth elements are added.

[0006] Nie Xinlei et al. (Nie Xinlei et al., A welding process for heat-resistant steel 15CrMo, patent accepted, September 29, 2023) introduced a welding process for heat-resistant steel 15CrMo, which belongs to the field of welding technology. Based on the use of GTAW+SMAW mixed welding process test, as well as the use of preheating, control of interlayer temperature, post-heating and insulation slow cooling, reasonable matching of welding materials, low heat input welding parameters and other welding processes, excellent performance of the welded joint is obtained. The disadvantage is that it does not provide a detailed description of the production process control of 15CrMo products, and no rare earth elements are added.

[0007] In summary, the above patents involve research and description of the production and welding process of heat-resistant alloy steel produced by 15CrMo medium and thick plate production lines, but fail to provide detailed descriptions of the production of 3-20mm thick heat-resistant alloy steel products on a 2250mm production line and the product's organizational properties. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip. By adding reasonable Mn, Cr, Mo, Ce and controlling the content of gas elements (H, O, N), matching a reasonable controlled rolling and controlled cooling process, and adopting heat preservation and slow cooling measures after rolling, the product has uniform and fine structure, stable performance, good plate shape, and good application effect, and customer feedback shows that the application effect is good.

[0009] The product thickness range is 3.0-20.0mm. After slow cooling under the heat preservation cover, the product has good plate quality, uniform structure, stable performance, especially strong toughness, weldability and oxidation resistance.

[0010] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0011] The present invention discloses a method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip, comprising the following steps: molten iron pretreatment, converter composite blowing, LF refining, RH, continuous casting, slab heating, hot rolling, laminar cooling and coiling, and heat preservation and slow cooling; the hot rolling comprises a heating furnace, rough rolling, and finishing rolling; wherein:

[0012] The continuous casting slab heating temperature is controlled at 1190-1250℃, the soaking temperature is 1190-1240℃, the furnace discharge temperature is controlled at 1220±20℃ when the thickness is ≤6mm, the furnace discharge temperature is controlled at 1210±20℃ when the thickness is 6.01-12.00mm, the furnace temperature is controlled at 1200±20℃ when the thickness is 12.01-20.00mm, and the slab time in the furnace is controlled within 180-240min;

[0013] The rough rolling adopts the 3+5 mode, and the rough rolling starting temperature is 980-1120℃;

[0014] The thickness of the finishing rolling is 3.0-12.00mm, the thickness of the intermediate billet is 40-55mm, and the final rolling temperature is 870-1010℃; the thickness of the intermediate billet is 12.0-20.00mm, the thickness is 55-65mm, and the final rolling temperature is 850-870℃;

[0015] In the cooling and coiling steps:

[0016] Thickness 3.0-12.0mm, cooling adopts "29" mode laminar cooling method, post-dispersion, cooling method is one-on-one, cooling speed is controlled at 30-50℃ / s, coiling temperature is 650-690℃;

[0017] Thickness 12.0-16.0mm, cooling adopts "12" mode laminar cooling method, front dispersion, cooling method is two-in-one, cooling speed is controlled at 25-45℃ / s, coiling temperature is 630-670℃;

[0018] The thickness is 16.0-20.0mm, and the cooling adopts the laminar cooling method of "11" mode, which is front dispersion, and the cooling method is one-on-one. The cooling speed is controlled at 20-40℃ / s, and the coiling temperature is 610-650℃.

[0019] Furthermore, the finishing rolling is carried out by a 7-stand continuous variable crown rolling mill, and the starting rolling temperature of the finishing rolling is 980-1120°C.

[0020] Furthermore, the chemical composition of the heat-resistant alloy steel is, by weight percentage, C: 0.12-0.18%, Si: 0.15-0.40%, Mn: 0.40-0.70%, P: ≤0.030%, S: ≤0.030%, Cr: 0.80-1.10%, Mo: 0.40-0.55%, Ce≤0.0030%, and the balance is Fe and unavoidable impurities.

[0021] Furthermore, the chemical composition of the heat-resistant alloy steel is, by weight percentage, C: 0.13-0.15%, Si: 0.20-0.30%, Mn: 0.40-0.55%, P: ≤0.015%, S: ≤0.01%, Cr: 0.90-1.10%, Mo: 0.40-0.50%, Ce: 0.0010-0.0025%, and the balance is Fe and unavoidable impurities.

[0022] Furthermore, the metallographic structure of the heat-resistant alloy steel is ferrite+pearlite, wherein the grain size is ≥11 levels.

[0023] Furthermore, the heat-resistant alloy steel meets the following requirements: tensile strength ≥ 450 MPa, yield strength ≥ 295 MPa, elongation ≥ 19%, and 180° cold bending test.

[0024] Compared with the prior art, the beneficial technical effects of the present invention are:

[0025] The present invention is based on C, Mn, Cr, Mo, supplemented by Ce microalloying alloy design system, by controlling various corrosion resistant elements and strengthening elements, the produced product has good corrosion resistance, weldability, strength and toughness. The inventors found that the raw material composition and mass ratio provided by the present invention, combined with the controlled rolling and controlled cooling process, and the rare earth heat-resistant alloy steel 15CrMo developed by using a 2250mm hot rolling production line has good corrosion resistance, toughness and weldability, and has been successfully applied to pipeline steel systems in metallurgy, electric power, chemical industry and other industrial fields;

[0026] The present invention adopts a reasonable component system design, the hot-rolled steel strip contains Cr: 0.90-1.00%, Mo: 0.40-0.50%, Ce: 0.0010-0.0030% corrosion-resistant elements, the microstructure is ferrite + pearlite, the grain size is about 12 levels, it has the characteristics of high strength, oxidation resistance and corrosion resistance, and is suitable for high-temperature pipeline steel. The mechanical properties and process properties meet the following requirements: tensile strength ≥ 450MPa, yield strength ≥ 295MPa, and elongation ≥ 19%. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The present invention will be further described below in conjunction with the accompanying drawings.

[0028] Figure 1 This is the metallographic structure diagram of the steel strip at 1 / 4 of the longitudinal direction implemented in the present invention;

[0029] Figure 2 Application diagram for customers. DETAILED DESCRIPTION

[0030] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0031] Example 1

[0032] A method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip:

[0033] The molten iron is pre-treated for desulfurization. The converter adopts the top and bottom combined blowing smelting technology. Ferromanganese, copper plate and ferrochrome are added to the converter for deoxidation and alloying. The composition is adjusted to meet the steel-making requirements. The tapping temperature of the converter is ≥1620℃. The molten steel after converter smelting is hoisted to the LF refining process for treatment. According to the composition of the molten steel, ferromanganese, ferrosilicon, ferrochrome, ferroaluminum, ferromolybdenum and other alloys are added to adjust the target composition. The molten steel is transported to the RH vacuum treatment, during which the composition and temperature are fine-tuned. The vacuum degree is required to be ≤2.6mbar, and the vacuum time is maintained for ≥10min, ensuring that the circulating pure degassing time is more than 7min. After the vacuum treatment, calcium treatment is carried out. After feeding the wire, the soft blowing time is guaranteed to be more than 8min. Before putting the steel, the argon flow rate is adjusted to make the molten steel in a soft blowing state to prevent the molten steel from being exposed. According to the chemical composition shown in Table 1, the slab continuous casting superheat is 33℃. After that, the slab is cleaned, slowly cooled, and the quality of the continuous casting billet is checked. The slab heating temperature is 1230°C, the soaking temperature is 1220°C, the furnace temperature is 1210°C, the heating time is 210 minutes, and the heated slab is subjected to high-pressure water dephosphorization. The width is determined by a fixed-width press, and 2 rough rolling mills and 7 CVC finishing mills are used. The intermediate billet thickness is 45.0mm, and the finishing temperature is 890°C. Laminar cooling adopts the post-dispersed cooling mode "29" (the upper and lower nozzles are separated by one open), the cooling rate is 38°C / s, the coiling temperature is 690°C, and the finished product thickness is 5.7mm. The mechanical properties test results of the steel strip prepared in the embodiment are shown in Table 2.

[0034] Example 2

[0035] A method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip:

[0036] The molten iron is pre-treated for desulfurization. The converter adopts the top and bottom combined blowing smelting technology. Ferromanganese, copper plate and ferrochrome are added to the converter for deoxidation and alloying. The composition is adjusted to meet the steel-making requirements. The converter steel-making temperature is ≥1620℃. The molten steel after converter smelting is hoisted to the LF refining process for treatment. According to the composition of the molten steel, ferromanganese, ferrosilicon, ferrochrome, ferroaluminum, ferromolybdenum and other alloys are added to adjust the target composition. The molten steel is transported to RH vacuum treatment, during which the composition and temperature are fine-tuned. The vacuum degree is required to be ≤2.6mbar, and the vacuum time is maintained for ≥10min, ensuring that the circulating pure degassing time is more than 7min. After the vacuum treatment, calcium treatment is carried out. After feeding the wire, the soft blowing time is guaranteed to be more than 8min. Before putting the steel, the argon flow rate is adjusted to make the molten steel in a soft blowing state to prevent the molten steel from being exposed. According to the chemical composition shown in Table 1, the slab continuous casting superheat is 31℃. After that, the slab is cleaned, slowly cooled, and the quality of the continuous casting billet is checked. The slab heating temperature is 1220°C, the soaking temperature is 1210°C, the furnace temperature is 1200°C, the heating time is 216 minutes, and the heated slab is subjected to high-pressure water dephosphorization. The width is determined by a fixed-width press, and 2 rough rolling mills and 7 CVC finishing mills are used. The intermediate billet thickness is 45.0mm, and the finishing temperature is 890°C. Laminar cooling adopts the post-dispersed cooling mode "29" (upper and lower nozzles are separated by one open), the cooling rate is 44°C / s, the coiling temperature is 673°C, and the finished product thickness is 9.8mm. The mechanical properties test results of the steel strip prepared in the embodiment are shown in Table 2.

[0037] Example 3

[0038] A method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip:

[0039] The molten iron is pre-treated for desulfurization. The converter adopts the top and bottom combined blowing smelting technology. Ferromanganese, copper plate and ferrochrome are added to the converter for deoxidation and alloying. The composition is adjusted to meet the steel-making requirements. The converter steel-making temperature is ≥1620℃. The molten steel after converter smelting is hoisted to the LF refining process for treatment. According to the composition of the molten steel, ferromanganese, ferrosilicon, ferrochrome, ferroaluminum, ferromolybdenum and other alloys are added to adjust the target composition. The molten steel is transported to the RH vacuum treatment, during which the composition and temperature are fine-tuned. The vacuum degree is required to be ≤2.6mbar, and the vacuum time is maintained for ≥10min, ensuring that the circulating pure degassing time is more than 7min. After the vacuum treatment, calcium treatment is carried out. After feeding the wire, the soft blowing time is guaranteed to be more than 8min. Before putting the steel, the argon flow rate is adjusted to make the molten steel in a soft blowing state to prevent the molten steel from being exposed. According to the chemical composition shown in Table 1, the slab continuous casting superheat is 30℃. After that, the slab is cleaned, slowly cooled, and the quality of the continuous casting billet is checked. The slab heating temperature is 1210°C, the soaking temperature is 1200°C, the furnace temperature is 1190°C, the heating time is 220min, and the heated slab is subjected to high-pressure water dephosphorization. The width is determined by a fixed-width press, and 2 rough rolling mills and 7 CVC finishing mills are used. The intermediate billet thickness is 57.0mm, and the finishing rolling temperature is 864°C. Laminar cooling adopts the back-front scattered cooling mode "12" (the upper and lower nozzles are separated by two and one), the cooling rate is 46°C / s, the coiling temperature is 655°C, and the finished product thickness is 15.75mm. The mechanical properties test results of the steel strip prepared in the embodiment are shown in Table 2.

[0040] Example 4

[0041] A method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip:

[0042] The molten iron is pre-treated for desulfurization. The converter adopts the top and bottom combined blowing smelting technology. Ferromanganese, copper plate and ferrochrome are added to the converter for deoxidation and alloying. The composition is adjusted to meet the steel-making requirements. The converter steel-making temperature is ≥1620℃. The molten steel after converter smelting is hoisted to the LF refining process for treatment. According to the composition of the molten steel, ferromanganese, ferrosilicon, ferrochrome, ferroaluminum, ferromolybdenum and other alloys are added to adjust the target composition. The molten steel is transported to the RH vacuum treatment, during which the composition and temperature are fine-tuned. The vacuum degree is required to be ≤2.6mbar, and the vacuum time is maintained for ≥10min, ensuring that the circulating pure degassing time is more than 7min. After the vacuum treatment, calcium treatment is carried out. After feeding the wire, the soft blowing time is guaranteed to be more than 8min. Before putting the steel, the argon flow rate is adjusted to make the molten steel in a soft blowing state to prevent the molten steel from being exposed. According to the chemical composition shown in Table 1, the slab continuous casting superheat is 32℃. After that, the slab is cleaned, slowly cooled, and the quality of the continuous casting billet is checked. The slab heating temperature is 1211°C, the soaking temperature is 1208°C, the furnace temperature is 1193°C, the heating time is 220min, and the heated slab is subjected to high-pressure water dephosphorization. The width is determined by a fixed-width press, and 2 rough rolling mills and 7 CVC finishing mills are used. The intermediate billet thickness is 60.0mm, and the finishing rolling temperature is 850°C. Laminar cooling adopts the back-to-front scattered cooling mode "11" (upper and lower nozzles are separated by one open), the cooling rate is 53°C / s, the coiling temperature is 631°C, the finished product thickness is 19.8mm, and the mechanical properties test results of the steel strip prepared in the embodiment are shown in Table 2.

[0043] In order to improve the uniformity of the steel coil structure and reduce the stress of the steel strip, all specifications of steel coils are slowly cooled after rolling. The slow cooling time of the steel coils is not less than 48 hours, and they are not stacked near the ventilation holes.

[0044] Figure 1 This is a typical microstructure diagram of the steel strip prepared in this embodiment. It can be seen from the diagram that the microstructure is ferrite and a small amount of pearlite, and the grain size is about level 12. The mechanical property test results of the steel strip prepared in this embodiment are shown in Table 2.

[0045] Table 1 Chemical composition of Examples 1-3 of the present invention (wt%)

[0046] Example C Si Mn P S Mo Cr Ce 1 0.13 0.25 0.45 0.011 0.005 0.44 0.93 0.0020 2 0.14 0.26 0.44 0.012 0.003 0.43 0.95 0.0017 3 0.13 0.22 0.46 0.010 0.001 0.43 0.96 0.0015

[0047] Table 2 Mechanical properties and corrosion resistance test results of the steel strips prepared in Examples 1-3 of the present invention

[0048]

[0049] From the data in Table 2, we can see that:

[0050] The mechanical properties and process properties meet the following requirements: yield strength ≥ 295MPa, tensile strength ≥ 450MPa, elongation A ≥ 19%, cold bending d = 3a.

[0051] It can be seen from the results of the above embodiments that the heat-resistant alloy steel strip for boilers and pipelines of the present invention has excellent mechanical properties, welding properties, corrosion resistance and other characteristics.

[0052] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a 3.0-20.0 mm thick rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip, characterized in that: The process comprises the following steps: molten iron pretreatment, converter composite blowing, LF refining, RH, continuous casting, slab heating, hot rolling, laminar cooling and coiling, and heat preservation and slow cooling; the hot rolling comprises a heating furnace, rough rolling, and finishing rolling; wherein: The continuous casting slab heating temperature is controlled at 1190-1250℃, the soaking temperature is 1190-1240℃, the furnace discharge temperature is controlled at 1220±20℃ when the thickness is ≤6mm, the furnace discharge temperature is controlled at 1210±20℃ when the thickness is 6.01-12.00mm, the furnace temperature is controlled at 1200±20℃ when the thickness is 12.01-20.00mm, and the slab time in the furnace is controlled within 180-240min; The rough rolling adopts the 3+5 mode, and the rough rolling starting temperature is 980-1120℃; The thickness of the finishing rolling is 3.0-12.00mm, the thickness of the intermediate billet is 40-55mm, and the final rolling temperature is 870-1010℃; the thickness of the intermediate billet is 12.0-20.00mm, the thickness is 55-65mm, and the final rolling temperature is 850-870℃; In the cooling and coiling steps: Thickness 3.0-12.0mm, cooling adopts "29" mode laminar cooling method, post-dispersion, cooling method is one-on-one, cooling speed is controlled at 30-50℃ / s, coiling temperature is 650-690℃; Thickness 12.0-16.0mm, cooling adopts "12" mode laminar cooling method, front dispersion, cooling method is two-in-one, cooling speed is controlled at 25-45℃ / s, coiling temperature is 630-670℃; The thickness is 16.0-20.0mm, and the cooling adopts the laminar cooling method of "11" mode, which is front dispersion, and the cooling method is one-on-one. The cooling speed is controlled at 20-40℃ / s, and the coiling temperature is 610-650℃.

2. The method for preparing the rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip with a thickness of 3.0-20.0 mm according to claim 1, characterized in that: The finishing rolling adopts a 7-stand continuous variable crown rolling mill, and the starting rolling temperature of the finishing rolling is 980-1120℃.

3. The method for preparing the rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip with a thickness of 3.0-20.0 mm according to claim 1, characterized in that: The chemical composition of the heat-resistant alloy steel is C: 0.12-0.18%, Si: 0.15-0.40%, Mn: 0.40-0.70%, P: ≤0.030%, S: ≤0.030%, Cr: 0.80-1.10%, Mo: 0.40-0.55%, Ce≤0.0030%, and the balance is Fe and unavoidable impurities.

4. The method for preparing the rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip with a thickness of 3.0-20.0 mm according to claim 3, characterized in that: The chemical composition of the heat-resistant alloy steel is calculated by weight percentage as follows: C: 0.13-0.15%, Si: 0.20-0.30%, Mn: 0.40-0.55%, P: ≤0.015%, S: ≤0.01%, Cr: 0.90-1.10%, Mo: 0.40-0.50%, Ce: 0.0010-0.0025%, and the balance is Fe and unavoidable impurities.

5. The method for preparing the rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip with a thickness of 3.0-20.0 mm according to claim 3, characterized in that: The metallographic structure of the heat-resistant alloy steel is ferrite+pearlite, wherein the grain size is ≥11 levels.

6. The method for preparing the rare earth heat-resistant alloy steel 15CrMo hot-rolled steel strip with a thickness of 3.0-20.0 mm according to claim 3, characterized in that: The heat-resistant alloy steel meets the following requirements: tensile strength ≥450MPa, yield strength ≥295MPa, elongation ≥19%, and 180° cold bending test.

Citation Information

Patent Citations

  • Steel plate with great heat and abrasion resistance and manufacturing method thereof

    CN103205650A

  • Low-alloy 15CrMo steel plate and production method thereof

    CN105861924A

  • High-performance alloy steel flanges and forgings and manufacturing method thereof

    CN108359902A

  • 3 to 8 mm hot rolled steel strip with yield strength being 700 MPa and used for car transmission shaft tube and production method thereof

    CN109504898A

  • High-temperature-resistant 400 HB wearproof steel plate and production method thereof

    CN110499474A

Cited By

  • Heat-treatment-free 15CrMo heat-resistant steel and production method thereof

    CN121592962A

  • Production method of rare earth 15CrMo heat-resistant alloy structural steel plate

    CN121826529A