Die casting production method of 12Cr2Mo1VR steel
Through the process flow of converter → LF furnace → slag → LF furnace → RH furnace → VD furnace → mold casting, the nitrogen content of 12Cr2Mo1VR steel is controlled, and the problem of excessive nitrogen content and high cost in mold casting production is solved, and low nitrogen is achieved Content and low cost production effect.
Patent Information
- Application Number
- CN202411180168.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-15
AI Technical Summary
In the process of mold casting production of 12Cr2Mo1VR steel, the prior art is difficult to effectively control the nitrogen content of the molten steel, resulting in the nitrogen content of the finished product often exceeding the standard requirements, and the production cost is higher when metal chromium is used.
The process flow of converter → LF furnace → slag → LF furnace → RH furnace → VD furnace → mold casting is adopted. By controlling the blowing of argon gas, vacuum treatment and alloy addition in each process step, the nitrogen content of the molten steel is reduced. Specific measures It includes adding low-carbon ferrochromium in the LF furnace without deoxygenation, adding ferrovanavana alloy and VD furnace vacuum treatment in the later stage of the vacuum process of the RH furnace, ensuring that the nitrogen content is below 50ppm.
It realizes low-cost control of the nitrogen content of molten steel, ensures that the nitrogen content of the finished product is below 65ppm, reduces production costs, and reduces the nitrogen increase of molten steel, and meets the requirements of the new implementation standard GB/T 713-2023.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a die casting production method of 12Cr2Mo1VR steel, which realizes the control of low nitrogen content and low cost. Background Art
[0002] 12Cr2Mo1VR steel has high strength and good plasticity, which can meet the use requirements of various parts of high-temperature and high-pressure containers and boilers. In addition, it has good processing performance and welding performance, which is convenient for processing and maintenance. It belongs to the national standard special steel plate for medium and high-temperature boilers and pressure vessels. It is widely used in the petroleum, chemical, electric power and other industries to make various equipment and components, such as reactors, heat exchangers, separators, spherical tanks, oil and gas tanks, etc. With the issuance of the new implementation standard GB / T 713-2023, it requires the nitrogen content of the finished product to be ≤0.0070%. For steel plates with a rolling thickness of ≥120mm, die casting is required. In the case of using low-carbon ferrochrome, the nitrogen content of molten steel before casting is high, and the die casting protection casting effect is relatively poor. The nitrogen increase during the casting process is generally above 10ppm, and some even exceed 20ppm. 12Cr2Mo1VR steel contains a high V content, which will cause nitrogen increase in molten steel and aggravate the nitrogen fixation effect. Therefore, the nitrogen content of the finished product is likely to exceed the standard requirements. In the case of using metallic chromium, the production cost will increase.
[0003] Therefore, how to achieve low nitrogen content and low cost control of die-cast 12Cr2Mo1VR steel has become a technical problem that troubles many steel mills. Summary of the invention
[0004] The invention aims to provide a die casting production method for 12Cr2Mo1VR steel, which can realize low nitrogen content and low cost control of molten steel.
[0005] The present invention is achieved through the following technical solutions: A die casting production method for 12Cr2Mo1VR steel comprises the following process steps: converter→LF furnace→slag removal→LF furnace→RH furnace→LF furnace→VD furnace→die casting. The chemical composition of steel is C=0.11~0.15, Si≤0.10, Mn=0.30~0.60, P≤0.006, S≤0.003, Mo=0.90~1.10, V=0.30~0.35, Cr=2.30~2.45%, Nb=0.025~0.035, Ni≤0.25, Al≤0.040, Ti≤0.030, B=0.010~0.020, [H]≤0.0002, [O]≤0.0025, [N]≤0.0070, As≤0.008, Sn≤0.005, Ca≤0.0015, and the rest are Fe and essential impurities. The process steps are as follows: A) Converter: Select molten iron, whose chemical composition weight percentage is P≤0.012, S≤0.040, As≤0.006, Sn≤0.005; molten iron ratio is 0.85~0.90, argon is blown at the bottom throughout the process, the end point is set at O≥0.05%, P≤0.008%, and the temperature is 1590~1620℃; add lime 4.0~5.0 kg / t when about 1 / 5 of the steel is tapped, and no deoxidation or alloying alloy is added during the tapping process; B) Dephosphorization in LF furnace: Add lime and blow argon from the bottom of the ladle to stir until the molten steel P is ≤ 0.003, then add 15.0~20.0 kg / t of low-carbon ferrochrome, and the temperature out of the station is 1550~1570 ℃; C) Slag removal: Use a slag removal machine to remove slag until the exposed surface of molten steel is ≥80%; D) LF furnace: add low silicon and low titanium refined slag to cover the molten steel surface, keep the LF furnace mouth at a slight positive pressure throughout the whole process, use lime and low silicon and low titanium pre-melted slag to make slag, use Al wire and aluminum shot to deoxidize, the total slag volume is 12.0~15.0 kg / t, add low nitrogen graphite recarburizer and low carbon and low nitrogen ferrochrome, ferroniobium and ferromolybdenum to adjust the composition, except V, B and Al elements, all other elements must meet the requirements, no calcium treatment is performed before leaving the station, and the leaving station temperature is 1650~1670℃; E) RH furnace: evacuate to a vacuum degree of 67Pa, add vanadium-iron alloy 2-4 minutes before breaking the vacuum, and maintain the vacuum for 12-15 minutes; F) LF furnace: Bottom blowing argon with weak stirring throughout the process, adjust boron and aluminum to the required range before leaving the station, feed pure calcium line 0.25~0.35kg / t, and the exit temperature is 1630~1650℃; G) VD furnace: VD furnace is evacuated to a vacuum degree of <67 Pa, the vacuum maintenance time is ≥18 min, the soft blowing time is ≥15 min, and pure calcium line is fed before leaving the station at 0.15~0.25 g / t; H) Mold casting: The whole process is protected, and 0.2~0.3Mpa argon gas is used for sealing. The casting superheat is 45~47 ℃.
[0006] The invention has the following beneficial effects: 1) all low-carbon ferrochrome is used, and the alloy cost is low; 2) part of the low-carbon ferrochrome is added to the LF furnace without deoxidation, so that Si and P therein can be oxidized and enter into the slag, and the Si content of the finished product can be effectively reduced by 0.02%-0.03% and the P content by 0.0005%-0.0006%; 3) ferrovanadium is not added to the LF furnace, so the nitrogen increase amount of molten steel is reduced; ferrovanadium is added to the RH furnace in the later stage of the vacuum process, so the nitrogen increase and nitrogen fixation of ferrovanadium are reduced; weak stirring is adopted in the whole process of entering the LF furnace again, and the nitrogen increase is less; VD vacuum treatment can control the nitrogen content of the outlet to be below 50ppm, and the nitrogen content of the molded finished product to be below 65ppm. DETAILED DESCRIPTION
[0007] The following is a description in conjunction with embodiments.
[0008] Example 1 A die casting production method of 12Cr2Mo1VR steel, the chemical composition weight percentage of the steel is shown in Table 1. The process steps are as follows: A) Converter: Iron-metal ratio 0.86, iron-metal composition: P = 0.112%, S = 0.031%, As = 0.004%, Sn = 0.002%, tapping oxygen 0.0612%, tapping P = 0.0071%, tapping temperature 1615°C, final slag basicity CaO / SiO2 = 4.1, N = 0.0018%, lime 4.6kg / t steel was added during tapping; B) LF furnace (dephosphorization): heat the molten steel to 1565℃, add 6.5 kg / t steel of active lime and 17.2 kg / t steel of low carbon ferrochrome in batches, add 3.0 kg / t steel thick slag of lime before leaving the station, the leaving station temperature is 15558℃, and the leaving station molten steel P=0.0025%; C) Slag removal: remove the slag cleanly; D) LF furnace: 3.0 kg / t steel of low silicon and low titanium refined slag was added into the molten steel station to cover the molten steel surface. After the temperature reached 1562℃, deoxidation and alloying were carried out. Lime and low silicon and low titanium refined slag were added during the process. The total slag amount was 14.2 kg / t steel. The LF station time was 85min. The exiting V=0.003%, B=0.0003%, Al=0.0025%, P=0.0047%, N=0.0095%, and the remaining elements were within the required range. The exiting temperature was 1662℃. E) RH furnace: evacuate to vacuum degree 67Pa, ultimate vacuum degree 29Pa, maintain vacuum degree for 15min, add vanadium iron alloy 6.5 kg / t steel when maintaining vacuum degree for 12min, exit V=0.324%, N=0.0065%; F) LF furnace: the whole process of bottom blowing argon flow rate is 150L / min for weak stirring, the outlet B=0.0015%, Al=0.041%, N=0.0071%, the other elements are within the required range, the pure calcium line is fed 0.29 kg / t steel, and the outlet temperature is 1638℃; G) VD furnace: evacuate to vacuum degree <67 Pa, ultimate vacuum degree 40Pa, vacuum maintenance time 20min, feed pure calcium wire 0.18 kg / t steel; soft blowing time 20min; exit H=0.00011%, N=0.0046%, Al=0..022%; H) Die casting: full protection casting, steel cover is used to protect the ladle water inlet to the center injection nozzle, 0.25Mpa argon gas is used for sealing, casting superheat is 45℃, ingot casting adopts uniform speed casting, and the liquid level rises steadily. Samples are taken from the head and tail of the rolled steel plate, head: N=0.0058%, tail: N=0.0057%. Example 2
[0009] A die casting production method of 12Cr2Mo1VR steel, the chemical composition weight percentage of the steel is shown in Table 1. The process steps are as follows: A) Converter: Iron-metal ratio 0.87, iron-metal composition: P = 0.115%, S = 0.029%, As = 0.003%, Sn = 0.003%, tapping oxygen 0.0586%, tapping P = 0.0074%, tapping temperature 1599 ° C, final slag basicity CaO / SiO2 = 4.2, N = 0.0020%, lime 4.5 kg / t steel during tapping; B) LF furnace (dephosphorization): heat the molten steel to 1567℃, add 6.2 kg / t steel of active lime and 17.1 kg / t steel of low carbon ferrochrome in batches, add 2.8 kg / t steel thick slag of lime before leaving the station, the leaving station temperature is 1560℃, and the leaving station molten steel P=0.0028%; C) Slag removal: remove the slag cleanly; D) LF furnace: 3.2 kg / t steel of low silicon and low titanium refined slag was added to the molten steel into the station to cover the molten steel surface. After the temperature reached 1568℃, deoxidation and alloying were carried out. Lime and low silicon and low titanium refined slag were added during the process. The total slag amount was 14.2 kg / t steel. The LF station time was 80min. The outgoing V=0.004%, B=0.0003%, Al=0.0028%, P=0.0052%, N=0.0089%, and the remaining elements were within the required range. The outgoing temperature was 1655℃. E) RH furnace: evacuate to vacuum degree 67Pa, ultimate vacuum degree 30Pa, maintain vacuum degree for 15min, add vanadium iron alloy 6.5 kg / t steel when maintaining vacuum degree for 12min, exit V=0.327%, N=0.0062%; F) LF furnace: the whole process of bottom blowing argon flow rate is 150L / min for weak stirring, the outlet B=0.0015%, Al=0.047%, N=0.0070%, the other elements are within the required range, the pure calcium line is fed 0.29 kg / t steel, and the outlet temperature is 1641℃; G) VD furnace: evacuate to vacuum degree <67 Pa, ultimate vacuum degree 39Pa, vacuum maintenance time 20min, feed pure calcium wire 0.18 kg / t steel; soft blowing time 25min; exit H=0.00012%, N=0.0043%, Al=0..024%; H) Die casting: full protection casting, steel cover is used to protect the ladle water inlet to the center injection nozzle, 0.25Mpa argon gas is used for sealing, casting superheat is 46 ℃, ingot casting adopts uniform speed steel pouring, and the liquid level rises steadily. Samples are taken from the head and tail of the rolled steel plate, head: N=0.0056%, tail: N=0.0055%.
[0010] Table 1 Chemical composition of example steel (wt, %) .
[0011] .
[0012] Comparative Example 1: A die casting production method for 12Cr2Mo1VR steel, which adopts the process of converter → LF furnace → slag removal → LF furnace → RH furnace → die casting; A) Converter: Iron-metal ratio 0.86, iron-metal composition: P = 0.114%, S = 0.032%, As = 0.003%, Sn = 0.003%, tapping oxygen 0.0649%, tapping P = 0.0065%, tapping temperature 1602 ° C, final slag basicity CaO / SiO2 = 4.5, N = 0.0022%, lime 4.4 kg / t steel was added during tapping; B) LF furnace (dephosphorization): heat the molten steel to 1564℃, add 6.2 kg / t steel of active lime and 17.6 kg / t steel of low carbon ferrochrome in batches, add 2.8 kg / t steel thick slag of lime before leaving the station, the leaving station temperature is 1561℃, and the leaving station molten steel P=0.0024%; C) Slag removal: remove the slag cleanly; D) LF furnace: 3.5 kg / t of low silicon and low titanium refined slag was added into the molten steel station to cover the molten steel surface. After the temperature of the molten steel reached 1570℃, lime and low silicon and low titanium refined slag were added in the process. The total slag amount was 14.3 kg / t of steel. The LF station time was 90 minutes. The steel output V=0.320%, B=0.0016%, P=0.0044%, Al=0.0038%, N=0.0118%, and the remaining elements were within the required range. The outlet temperature was 1652℃. E) RH furnace: evacuate to vacuum degree 67Pa, ultimate vacuum degree 30Pa, maintain vacuum twice, the first vacuum time is 15min, the second vacuum time is 21min according to the temperature measurement result, feed pure calcium wire 0.18 kg / t steel; soft blowing time is 17min. Outgoing N=0.0073%, other elements are within the required range; F) Die casting: full protection casting, steel cover is used to protect the ladle water inlet to the center injection nozzle, 0.25Mpa argon gas is used for sealing, casting superheat is 46 ℃, ingot casting adopts uniform speed steel pouring, and the liquid level rises steadily. Samples are taken from the head and tail of the rolled steel plate, head: N=0.0085%, tail: N=0.0083%;
[0013] Comparative Example 2: A die casting production method of 12Cr2Mo1VR steel, comprising the following production steps: converter → LF furnace → slag removal → LF furnace → RH furnace → die casting; A) Converter: Iron-metal ratio 0.87, iron-metal composition: P = 0.109%, S = 0.027%, As = 0.004%, Sn = 0.003%, tapping oxygen 0.0652%, tapping P = 0.0075%, tapping temperature 1610 ° C, final slag basicity CaO / SiO2 = 4.6, N = 0.0021%, lime 4.6 kg / t steel was added during tapping; B) LF furnace (dephosphorization): heat the molten steel to 1569℃, add 6.0 kg / t steel of active lime and 17.4 kg / t steel of low carbon ferrochrome in batches, add 2.8 kg / t steel thick slag of lime before leaving the station, the leaving station temperature is 1559℃, and the leaving station molten steel P=0.0025%; C) Slag removal: remove the slag cleanly; D) LF furnace: 3.4 kg / t steel of low silicon and low titanium refined slag was added into the molten steel station to cover the surface of the molten steel. After the temperature of the molten steel reached 1570℃, lime and low silicon and low titanium refined slag were added in the process. The total slag amount was 14.3 kg / t steel. The LF station time was 85 min. The steel tapping V=0.309%, B=0.0014%, P=0.0045%, Al=0.0072%, N=0.00125%, and the remaining elements were within the required range. The outlet temperature was 1675℃. E) VD furnace: evacuate to vacuum degree 67Pa, ultimate vacuum degree 30Pa, maintain vacuum twice, the first vacuum time is 15min, the second vacuum time is 20min according to the temperature measurement result, break the vacuum and feed pure calcium wire 0.18 kg / t steel; soft blowing time is 22min. Outgoing N=0.0061%, other elements are within the required range; F) Die casting: full protection casting, steel cover is used to protect the ladle water inlet to the center injection nozzle, 0.25Mpa argon gas is used for sealing, casting superheat is 46 ℃, ingot casting adopts uniform speed steel pouring, and the liquid level rises steadily. Samples are taken from the head and tail of the rolled steel plate, head: N=0.0075%, tail: N=0.0073%;
[0014] By comparing the comparative example with the embodiment, it can be seen that when LF is removed and ferrovanadium is added, the nitrogen content of LF at the secondary exit is less than 75ppm, while after adding ferrovanadium, the nitrogen content of LF at the secondary exit is greater than 115ppm. The nitrogen content of LF at the exit is significantly reduced. After two vacuum treatments, the nitrogen content of molten steel before mold casting is less than 50ppm by adopting the production method of the present invention, while the nitrogen content of molten steel before mold casting is greater than 60ppm by adopting the comparative example production method under the condition that the vacuum holding time of VD or RH is basically the same. The nitrogen content of molten steel in a single furnace is reduced by more than 10ppm.
Claims
1. A die casting production method for 12Cr2Mo1VR steel, characterized in that: The chemical composition of steel is C=0.11~0.15, Si≤0.10, Mn=0.30~0.60, P≤0.006, S≤0.003, Mo=0.90~1.10, V=0.30~0.35, Cr=2.30~2.45%, Nb=0.025~0.035, Ni≤0.25, Al≤0.040, Ti≤0.030, B=0.0010~0.0020, [H]≤0.0002, [O]≤0.0025, [N]≤0.0070, As≤0.008, Sn≤0.005, Ca≤0.0015, and the rest is Fe and essential impurities; The process steps include: A) Converter: Select molten iron, whose chemical composition weight percentage is P≤0.012, S≤0.040, As≤0.006, Sn≤0.005; molten iron ratio is 0.85~0.90, argon is blown at the bottom throughout the process, the end point is set at O≥0.05%, P≤0.008%, and the temperature is 1590~1620℃; add lime 4.0~5.0 kg / t when about 1 / 5 of the steel is tapped, and no deoxidation or alloying alloy is added during the tapping process; B) Dephosphorization in LF furnace: Add lime and blow argon from the bottom of the ladle to stir until the molten steel P is ≤ 0.003, then add 15.0~20.0 kg / t of low-carbon ferrochrome, and the temperature out of the station is 1550~1570 ℃; C) Slag removal: Use a slag removal machine to remove slag until the exposed surface of molten steel is ≥80%; D) LF furnace: add low silicon and low titanium refined slag to cover the molten steel surface, keep the LF furnace mouth at a slight positive pressure throughout the whole process, use lime and low silicon and low titanium pre-melted slag to make slag, use Al wire and aluminum shot to deoxidize, the total slag volume is 12.0~15.0 kg / t, add low nitrogen graphite recarburizer and low carbon and low nitrogen ferrochrome, ferroniobium and ferromolybdenum to adjust the composition, except V, B and Al elements, all other elements must meet the requirements, no calcium treatment is performed before leaving the station, and the leaving station temperature is 1650~1670℃; E) RH furnace: evacuate to a vacuum degree of 67Pa, add vanadium-iron alloy 2-4 minutes before breaking the vacuum, and maintain the vacuum for 12-15 minutes; F) LF furnace: Bottom blowing argon with weak stirring throughout the process, adjust boron and aluminum to the required range before leaving the station, feed pure calcium line 0.25~0.35 kg / t, and the exit temperature is 1630~1650℃; G) VD furnace: VD furnace is evacuated to a vacuum degree of <67 Pa, the vacuum maintenance time is ≥18 min, the soft blowing time is ≥15 min, and pure calcium line is fed before leaving the station at 0.15~0.25 g / t; H) Mold casting: The whole process is protected, and 0.2~0.3Mpa argon gas is used for sealing. The casting superheat is 45~47 ℃.